Anode foil for aluminum electrolytic capacitor, wound body, and aluminum electrolytic capacitor
By using arc-shaped anode foil with dielectric layer on the surface in an aluminum electrolytic capacitor, the flash breakdown and mechanical performance problems are solved, the reliability of the capacitor and the parallel flash voltage are improved, and the oxide film is too thick is avoided. Winding difficulties and volume increase.
Patent Information
- Application Number
- CN202411310151.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-19
- Publication Date
- 2024-11-08
AI Technical Summary
Aluminum electrolytic capacitors are prone to flash breakdown at high voltage and high frequency, discharge breakdown at conductor material nail connections and cold press connections, resulting in short-circuit failure, and the thickening of the oxide film of the anode foil will reduce mechanical properties and winding difficulty. , affects the miniaturization of capacitors.
Arc-angle anode foil with dielectric layer on the surface, and the radius of the arc angle is set according to the width of the foil. It is used for the anode foil, winding body and capacitor of aluminum electrolytic capacitor to avoid the risk of flash fire in rectangular corners and corners. , improve the parallel voltage and mechanical properties of the oxide film.
It effectively increases the flash fire voltage, reduces the cracking phenomenon of oxide film, improves the reliability of the product and the parallel flash fire voltage, and avoids the problems of increasing winding volume and degradation of mechanical properties caused by excessive oxide film.
Smart Images

Figure CN118919302A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of aluminum electrolytic capacitors, and in particular to an anode foil for an aluminum electrolytic capacitor, a winding body, and an aluminum electrolytic capacitor. Background Art
[0002] The main types of capacitors are aluminum electrolytic capacitors, film capacitors, ceramic capacitors, tantalum capacitors, etc. Aluminum electrolytic capacitors are an important part of the electronic information industry. Aluminum electrolytic capacitors are polar electrolytic capacitors, known as the vitamins of modern industry. They are one of the most commonly used passive components in electronic circuits, mainly used for energy storage, filtering, compensation and protection circuits. Aluminum electrolytic capacitors are widely used in electronics, electricity, communications, home appliances and other fields due to their small size, large capacity, long life and low cost.
[0003] In aluminum electrolytic capacitors, the anode foil is usually in an oxidized state. Its main function is to transmit current and form a dense anodic oxide film. This oxide film can have good electrical conductivity and insulation properties, pass AC and isolate DC, so that the capacitor has high electrical performance. The anode foil can also provide the contact resistance between the electrolyte and the electrolyte and the anode of the aluminum electrolytic capacitor, as well as transmit current during the electrolysis process. In specific applications, the voltage of aluminum electrolytic capacitors is sometimes unstable, especially when an overvoltage exceeding the rated voltage is applied to the aluminum electrolytic capacitor. Due to the applied overvoltage, the capacitor may fail due to electrolyte flashover, capacitor rapid heating and breakdown, conductor material nailing, cold pressing connection, and discharge breakdown at the tip of the rolled rectangular corner burr. As a result, the operating voltage and operating frequency of aluminum capacitors required by more and more high-end large-scale instruments and equipment are gradually increasing.
[0004] It is well known that the voltage of the anode foil is generally higher than that of the cathode foil. Therefore, the oxide film is thicker after the potential voltage is increased, and it can withstand higher voltage and current. Although the oxide film can be thickened, further increasing the withstand voltage of the aluminum electrolytic capacitor will reduce the effective specific capacity. However, the oxide film on the surface of the anode foil cannot be thickened too much. The thickened oxide film will block the groove holes on the anode foil and reduce the specific capacity. At the same time, the mechanical properties of the anode foil material will be reduced when it is wound, and the bending strength of the oxide film will be reduced, which will make it easier to crack. Moreover, the oxide foil will continue to thicken, which is not conducive to winding. There will be cracking problems during the winding process. The thickening of the oxide film means the thickening of the anode foil. It is difficult to reduce the volume of the capacitor after winding multiple layers, which is not conducive to the miniaturization of the capacitor. Summary of the invention
[0005] Based on this, it is necessary to provide an anode foil, a winding body and an aluminum electrolytic capacitor for an aluminum electrolytic capacitor in order to solve the above-mentioned technical problems.
[0006] The present invention is achieved through the following technical solutions: In a first aspect, an anode foil for an aluminum electrolytic capacitor includes a foil having a dielectric layer on its surface; the foil has an arc-shaped corner.
[0007] As a preferred embodiment of the anode foil for aluminum electrolytic capacitor provided by the present invention, the two closest corners of the foil are set as arc angles.
[0008] As a preferred embodiment of the anode foil for aluminum electrolytic capacitor provided by the present invention, three corners of the foil are configured as arc angles.
[0009] As a preferred embodiment of the anode foil for aluminum electrolytic capacitor provided by the present invention, the four corners of the foil are all set as arc corners.
[0010] As a preferred embodiment of the anode foil for aluminum electrolytic capacitors provided by the present invention, when the width w of the foil is within 8 mm, the radius R of the arc angle is set to: w / 5≤R≤w / 2; when the width w of the foil is greater than 8 mm, the radius R of the arc angle is set to greater than 2 mm.
[0011] As a preferred implementation of the anode foil for aluminum electrolytic capacitor provided by the present invention, the arc angle is a circular arc angle or an elliptical arc angle.
[0012] In a second aspect, a wound body of an aluminum electrolytic capacitor includes the anode foil according to the first aspect.
[0013] As a preferred embodiment of the aluminum electrolytic capacitor winding body provided by the present invention, the winding body further includes a cathode foil and a separator paper, and the winding body is formed by winding the anode foil, the cathode foil, and the separator paper arranged between the anode foil and the cathode foil.
[0014] In a third aspect, an aluminum electrolytic capacitor includes the wound body according to the second aspect.
[0015] As a preferred implementation manner of the aluminum electrolytic capacitor provided by the present invention, the aluminum electrolytic capacitor is a medium- and high-voltage aluminum electrolytic capacitor.
[0016] As a preferred implementation manner of the aluminum electrolytic capacitor provided by the present invention, the aluminum electrolytic capacitor is a lead-type aluminum electrolytic capacitor, a horn-type aluminum electrolytic capacitor, a bolt-type aluminum electrolytic capacitor and a supercapacitor.
[0017] Compared with the prior art, the present invention has the following beneficial effects: In aluminum electrolytic capacitors, the anode foil provides electrons in the electrolyte, thereby reducing the electrolyte and completing the closure of the electron flow, that is, the current and voltage of the anode foil are transmitted as balanced as possible during the electrolysis process to avoid the appearance of voltage and current collecting flash points. The inventors unintentionally processed the anode foil into an arc angle, that is, the corners of the anode foil were set to arc angles, and the flash voltage can be effectively increased when applied to aluminum electrolytic capacitors. Compared with the long rectangular foil without arc angles, after experimental verification, the flash voltage has been increased by more than 1.15 times; it effectively solves the technical defects in the application of traditional preparation processes for aluminum electrolytic capacitors, effectively solves the mechanical properties of the progressive bending of the anode foil when the winding process is unwinding, reduces the cracking of the oxide film, and increases the effective parallel voltage of the oxide film. After the arc angle, the possibility of tip discharge after the sharp current collecting voltage of the rectangular corners when the capacitor is under load or overpressure is effectively avoided, that is, the risk of discharge flash at the sharp current collecting corners of the rectangular corners is effectively avoided, thereby increasing the parallel flash voltage of the product and ensuring the real high reliability of the product. Compared with the products of traditional processes, the present invention has the ability to increase the parallel voltage of capacitor load, which greatly improves the reliability of the product. There is no need to further thicken the oxide film on the anode foil in order to increase the VF voltage, thereby reducing the effective specific capacity of the material, and at the same time avoid the problem of cracking of the oxide film during winding and the problem of increasing the volume of the winding body.
[0018] It is to be understood that the foregoing general description and the following detailed description are exemplary and explanatory only and are not restrictive of the invention.
[0019] For better understanding and implementation, the present invention is described in detail below with reference to the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] In order to more clearly illustrate the scheme of the present invention, a brief introduction is given below to the drawings required for use in the description of the embodiments. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0021] Figure 1 A three-dimensional schematic diagram of an embodiment of an anode foil for an aluminum electrolytic capacitor provided by the present invention; Figure 2 A three-dimensional schematic diagram of another embodiment of the anode foil for aluminum electrolytic capacitor provided by the present invention; Figure 3 A three-dimensional schematic diagram of another embodiment of the anode foil for aluminum electrolytic capacitor provided by the present invention; Figure 4 A three-dimensional exploded schematic diagram of the winding process of the winding body provided by the present invention; Figure 5A three-dimensional schematic diagram of a lead-type aluminum electrolytic capacitor in a wound state provided by the present invention, wherein a housing and a sealing member are not shown in the figure; Figure 6 A three-dimensional schematic diagram of a horn-type aluminum electrolytic capacitor in a wound state provided by the present invention, wherein a housing and a sealing member are not shown in the figure; In the figure, 100-anode foil; 110-arc angle; 200-Isolation paper; 300- anode foil; 400-lead piece. DETAILED DESCRIPTION
[0022] Hereinafter, examples will be given to illustrate the embodiments of the present disclosure, but the present disclosure is not limited to the examples described below. In the following description, specific numerical values and materials are sometimes exemplified, but other numerical values and materials may also be used as long as the effects of the present disclosure can be obtained. In this specification, a description such as "numerical value A to numerical value B" includes numerical value A and numerical value B, and can be replaced by "numerical value A or more and numerical value B or less". In the following description, when a lower limit and an upper limit are exemplified with respect to numerical values such as specific physical properties and conditions, any one of the exemplified lower limits and any one of the exemplified upper limits can be arbitrarily combined as long as the lower limit does not become above the upper limit. When multiple materials are exemplified, one of them can be selected and used alone, or two or more can be used in combination.
[0023] In order to enable those skilled in the art to better understand the scheme of the present invention, the technical scheme in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.
[0024] It should be noted that, in the absence of conflict, the embodiments of the present invention and the features and technical solutions in the embodiments may be combined with each other.
[0025] It should be noted that similar reference numerals and letters denote similar items in the following drawings, and therefore, once an item is defined in one drawing, further definition and explanation thereof is not required in subsequent drawings.
[0026] Anode foil for aluminum electrolytic capacitors An anode foil for an aluminum electrolytic capacitor according to one embodiment of the present invention includes a foil having a dielectric layer on its surface. The foil substrate is a valve metal, such as aluminum (Al), tantalum (Ta), niobium (Nb), etc., and may also be an alloy or compound containing a valve metal. The dielectric layer is, for example, a layer containing an oxide of a valve metal. The foil of the anode foil for an aluminum electrolytic capacitor is in a strip or strip shape before winding, and the surface of the foil is roughened by etching or the like before the dielectric layer is formed, so that the anode foil has a large surface area.
[0027] like Figure 1-3 As shown, the foil has arc angles. In one embodiment, the two closest corners of the foil are set as arc angles, such as Figure 2 For example, the two corners of the foil in the width direction are set as arc angles. When the foil is used for winding, the side with the arc angle is used as the unwinding side. In another embodiment, the four corners of the foil are set as arc angles, such as Figure 1 , 3 shown.
[0028] When the width w of the foil is within 8 mm, the radius R of the arc angle is set to: w / 5≤R≤w / 2; when the width w of the foil is greater than 8 mm, the radius R of the arc angle is set to be greater than 2 mm. The arc angle can be a circular arc angle or an elliptical arc angle.
[0029] Flash fire occurs when the oxygen ion concentration at the interface between the metal oxide film and the electrolyte increases to a potential that can release electrons. The free electrons are accelerated in the electric field and emitted into the film, hitting the oxide film structure and developing into local electrical breakdown. In the prior art, the corners of the rectangular foil after cutting are all corners. After the voltage is input, the electron current is more likely to gather at the corners. The current concentration at the corners causes local heating, and the winding body is a tight winding structure. The winding body is in a high-heat state under working conditions. In particular, the heat generated by the winding body of medium and high-voltage capacitor products is greater, making it impossible for the local heating heat at the corners to be dissipated in time. The concentration of local current and the local temperature rise promote each other, and finally reach a local high-temperature state, and flash fire occurs.
[0030] According to experimental verification, after the anode foil is processed with arc angles, that is, the corners of the anode foil are set to arc angles, the flash voltage can be effectively improved when applied to aluminum electrolytic capacitors. Compared with the long rectangular foil without arc angles, the flash voltage is increased by more than 1.15 times after experimental verification; it effectively solves the technical defects in the application of the traditional preparation process of aluminum electrolytic capacitors, effectively solves the mechanical properties of the progressive bending of the anode foil during the winding process, reduces the cracking of the oxide film, and improves the effective parallel voltage of the oxide film. After the anode foil is processed with arc angles, the possibility of tip discharge after the rectangular corners are collected when the capacitor is loaded or overpressured is effectively avoided, that is, the risk of flash discharge at the rectangular corners is effectively avoided, thereby improving the product parallel flash voltage and ensuring the real high reliability of the product. Compared with the products of traditional processes, the present invention has the ability to increase the parallel voltage of higher capacitor loads, which greatly improves the reliability of the product. There is no need to further thicken the oxide film on the anode foil in order to improve the withstand voltage, so as to avoid the problem of cracking of the oxide film when winding and the problem of increasing the volume of the winding body.
[0031] Aluminum electrolytic capacitor windings The anode foil for an aluminum electrolytic capacitor according to the embodiment of the present invention is suitable for use in a wound body of an aluminum electrolytic capacitor.
[0032] like Figure 4-6 As shown, the wound body is formed by winding the above-mentioned anode foil, cathode foil, and separator paper arranged between the anode foil and the cathode foil.
[0033] The coiled body made of the above-mentioned anode foil is processed into an arc angle by the anode foil, which effectively avoids the risk of current discharge and flashover at the sharp corners of the anode foil when the capacitor is under load or overpressured, thereby improving the parallel flashover voltage of the product and ensuring the real high reliability of the product. At the same time, after the corners of the unwinding side of the anode foil are arc-shaped, the technical defects in the application of the traditional preparation process of aluminum electrolytic capacitors are effectively solved, and the mechanical properties of the anode foil gradually bending when the winding process is unwinding are effectively solved, reducing the cracking phenomenon of the oxide film and improving the effective parallel voltage of the oxide film.
[0034] The cathode foil is not particularly limited, and may be, for example, a metal foil made of a valve metal such as aluminum, tantalum, or niobium. It should be noted that the valve metals constituting the anode foil and the anode foil may be the same or different.
[0035] The release paper is not particularly limited, and may be, for example, a nonwoven fabric having synthetic cellulose, polyethylene terephthalate, vinylon, aramid fiber, or the like as a main component.
[0036] like Figure 5 , 6 As shown, the winding body further includes lead-out pieces connected to the anode foil and the anode foil respectively, and the materials thereof are not particularly limited and any known materials may be used.
[0037] There is also an electrolyte between the anode foil and the cathode foil, which functions as a capacitor. The electrolyte includes at least one of a solid electrolyte having a conductive polymer and a liquid electrolyte.
[0038] Aluminum electrolytic capacitors The aluminum electrolytic capacitor wound body according to the embodiment of the present invention is suitable for use in an aluminum electrolytic capacitor.
[0039] The aluminum electrolytic capacitor of this embodiment adopts the above-mentioned winding body, which is accommodated in a case with an opening, and the lead member extends out of the opening. As the material of the case body, metals such as aluminum, stainless steel, copper, iron, brass, etc. or their alloys can be used.
[0040] A sealing member is also arranged on the open side, and the sealing member is riveted to the open side of the housing and crimped, thereby sealing the winding body in the housing. The lead member passes through the sealing member. The sealing member is preferably an insulating material with high heat resistance, such as silicone rubber, fluororubber, ethylene-propylene rubber, hepalon rubber, butyl rubber, isoprene rubber, etc.
[0041] The rated voltage of the aluminum electrolytic capacitor involved in this embodiment can be low voltage, such as 2.5V~63V; it can also be medium voltage, such as 63V~200V; it can also be high voltage, such as 200V~800V, or even higher.
[0042] It is worth noting that the materials of aluminum electrolytic capacitors with different rated voltages can be selected from known materials. The present invention sets the arc angle of the selected anode foil before winding the winding body, and then winds it into a winding body. There is no special limitation on the materials of the anode foil and other aluminum electrolytic capacitors.
[0043] In the present invention, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral one; it can be a mechanical connection, an electrical connection, or communication with each other; it can be a direct connection, or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements, unless otherwise clearly defined. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0044] Obviously, the embodiments described above are only some embodiments of the present invention, rather than all embodiments. The preferred embodiments of the present invention are given in the accompanying drawings, but they do not limit the patent scope of the present invention. The present invention can be implemented in many different forms. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present invention more thorough and comprehensive. Although the present invention has been described in detail with reference to the aforementioned embodiments, for those skilled in the art, it is still possible to modify the technical solutions recorded in the aforementioned specific embodiments, or to perform equivalent replacements for some of the technical features therein. Any equivalent structure made using the contents of the specification and drawings of the present invention, directly or indirectly used in other related technical fields, is also within the scope of patent protection of the present invention.
Claims
1. An anode foil for an aluminum electrolytic capacitor, characterized in that: The invention comprises a foil with a dielectric layer on its surface; the foil has an arc-shaped corner.
2. The anode foil for aluminum electrolytic capacitor according to claim 1, wherein: The two closest corners of the foil are set as arc angles.
3. The anode foil for aluminum electrolytic capacitor according to claim 1, wherein: The four corners of the foil are all set as arc corners.
4. The anode foil for aluminum electrolytic capacitor according to claim 1, wherein: When the width w of the foil is within 8 mm, the radius R of the arc angle is set to: w / 5≤R≤w / 2; when the width w of the foil is greater than 8 mm, the radius R of the arc angle is set to greater than 2 mm.
5. The anode foil for aluminum electrolytic capacitor according to claim 1, wherein: The arc angle is a circular arc angle or an elliptical arc angle.
6. An aluminum electrolytic capacitor winding body, characterized in that: It comprises the anode foil as claimed in any one of claims 1 to 5.
7. The aluminum electrolytic capacitor wound body according to claim 6, characterized in that: It also includes a cathode foil and a separator paper, and the winding body is formed by winding the anode foil, the cathode foil, and the separator paper arranged between the anode foil and the cathode foil.
8. An aluminum electrolytic capacitor, characterized in that: It comprises the wound body according to claim 6 or 7.
9. The aluminum electrolytic capacitor according to claim 8, characterized in that: The aluminum electrolytic capacitor is a medium- and high-voltage aluminum electrolytic capacitor.
10. The aluminum electrolytic capacitor according to claim 8 or 9, characterized in that: The aluminum electrolytic capacitor is a lead-type aluminum electrolytic capacitor, a horn-type aluminum electrolytic capacitor, a bolt-type aluminum electrolytic capacitor and a lithium-ion supercapacitor.
Citation Information
Cited By
High-performance shrinkage type aluminum electrolytic capacitor
CN223770971U