Copper-chromium contact material with honeycomb bionic structure chromium skeleton and preparation method and application thereof
By using 3D printing in copper-chromium contact materials to prepare a directionally distributed honeycomb structure chromium skeleton and landfill the copper matrix, the problem of low performance of copper-chromium contact materials is solved, and better thermal conductivity, electrical conductivity and anti-welding are achieved. Performance, suitable for higher-level vacuum circuit breakers.
Patent Information
- Application Number
- CN202411247949.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-06
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-09-06
AI Technical Summary
The random non-directional distribution of chromium skeletons in existing copper-chromium contact materials affects its conductivity and heat dissipation, making it difficult to meet the performance requirements of higher-grade vacuum circuit breakers.
A chromium skeleton with a honeycomb bionic structure is prepared by 3D printing process, and the copper matrix is buried in its pores through a vacuum seepage process to form a copper-chromium contact material with a honeycomb structure to avoid arc aggregation and improve thermal and electrical conductivity.
Through the directionally distributed honeycomb structure chrome skeleton, arc aggregation is avoided, thermal conductivity, electrical conductivity and anti-welding performance of copper-chrome contact materials are improved, and performance requirements of higher-grade vacuum circuit breakers are met.
Smart Images

Figure CN118919351A_ABST
Abstract
Description
Technical Field
[0001] The present application belongs to the technical field of contact materials, and in particular relates to a copper-chromium contact material having a honeycomb bionic structure chromium skeleton, a preparation method and an application thereof. Background Art
[0002] Vacuum circuit breakers have the advantages of small size, light weight, suitable for frequent operation, and arc extinguishing without maintenance. They have been widely used in electrical systems. The contact material is the contact part of the vacuum circuit breaker. Its quality and performance directly affect the performance and stability of the vacuum circuit breaker, which may affect the normal operation of the entire electrical system.
[0003] As vacuum circuit breakers are upgraded from 12kV to 126kV and then to 252kV, the first technical difficulty to be tackled is to enhance the insulation withstand voltage capability of vacuum contacts. Contact material is one of the key factors that determine the insulation withstand voltage capability of vacuum circuit breakers. Ideal vacuum circuit breaker contact materials should have large breaking current capability, high withstand voltage strength, reliable anti-welding performance, high electrical and thermal conductivity, low arc burn rate and low cutoff value. Copper-chromium alloy combines the advantages of high electrical and thermal conductivity of copper and high melting point, high hardness and oxygen affinity of chromium, and is currently the main contact material for vacuum circuit breakers.
[0004] However, the current copper-chromium contact materials are mainly obtained by melting copper and chromium through vacuum casting, vacuum infiltration, arc melting and mixed powder metallurgy. The copper and chromium in the copper-chromium contact materials do not have a specific preferential directional distribution in space, which affects the electrical conductivity and heat dissipation properties of the copper-chromium contact materials. The performance of the copper-chromium contact materials is not high enough to meet the requirements of higher-level vacuum circuit breakers.
[0005] Natural biomaterials in nature exhibit unique functional properties due to their ingenious microstructural laws, providing important inspiration for the development of high-performance bionic materials. Summary of the invention
[0006] In view of this, the present application provides a copper-chromium contact material with a honeycomb bionic structure chromium skeleton, a preparation method and an application thereof, which are used to solve the technical problem of low performance of copper-chromium contact materials in the prior art.
[0007] The first aspect of the present application provides a copper-chromium contact material having a honeycomb bionic structure chromium skeleton, comprising: a honeycomb structure chromium skeleton, a copper matrix;
[0008] The chromium skeleton of the honeycomb structure is embedded in the copper matrix.
[0009] Preferably, the mass ratio of the chromium skeleton of the honeycomb structure to the copper matrix is 20-30:70-80.
[0010] Preferably, the chromium skeleton of the honeycomb structure comprises: 3 to 7 single-room structures;
[0011] One of the single-room structures comprises: 2 to 5 layers of chrome sheets in the shape of hollow regular prisms, and the cross-sectional diagonal lines of adjacent chrome sheets in the shape of hollow regular prisms partially overlap and have the same center.
[0012] Preferably, in the single-chamber structure, the spacing between adjacent hollow regular prism-shaped chromium sheet layers is 0.5-2 μm.
[0013] Preferably, the thickness of the hollow regular prism-shaped chromium sheet layer is 0.5-2 μm, and the side length is 5-10 μm.
[0014] Preferably, the shape of the hollow regular prism is selected from a hollow regular triangular prism, a hollow regular quadrangular prism or a hollow regular hexagonal prism.
[0015] The second aspect of the present application provides a method for preparing a copper-chromium contact material having a honeycomb bionic structure chromium skeleton, the preparation method comprising the steps of:
[0016] Step S1, loading chromium powder into a 3D printing device and establishing a 3D model of a chromium skeleton, and performing 3D printing to obtain a chromium skeleton with a honeycomb structure;
[0017] Step S2, placing the chromium skeleton of the honeycomb structure in a copper-chromium contact material mold, infiltrating the pores of the chromium skeleton of the honeycomb structure with the heated and melted copper powder, and obtaining the copper-chromium contact material with the chromium skeleton of the honeycomb structure after cooling.
[0018] Preferably, in step S1, the 3D printing equipment is selected from direct metal laser sintering equipment, electron beam melting equipment or selective laser sintering equipment.
[0019] A third aspect of the present application provides an application of a copper-chromium contact material having a honeycomb bionic structure chromium skeleton in a vacuum circuit breaker.
[0020] A fourth aspect of the present application provides a vacuum circuit breaker, including a vacuum interrupter and an operating mechanism;
[0021] The operating mechanism is used to control the contact assembly in the vacuum interrupter to open or close the switch;
[0022] The contact assembly includes the copper-chromium contact material having a honeycomb bionic structure chromium skeleton as described in the first aspect.
[0023] In summary, the present application provides a copper-chromium contact material with a honeycomb bionic structure chromium skeleton, a preparation method and an application thereof. The copper-chromium contact material with a honeycomb bionic structure chromium skeleton provided by the present application first obtains a honeycomb structure chromium skeleton by 3D printing, and then the copper matrix is buried in the honeycomb structure chromium skeleton by a solution infiltration process. Compared with the randomly non-directionally distributed chromium skeleton, the honeycomb bionic structure chromium skeleton set in the copper-chromium contact material provided by the present application can avoid arc aggregation when electrical breakdown occurs, and can also improve its thermal conductivity and electrical conductivity, thereby improving the performance of the copper-chromium contact material and solving the technical problem of low performance of the copper-chromium contact material in the prior art. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] In order to more clearly illustrate the specific implementation methods of the present application or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0025] Figure 1 A schematic cross-sectional view of a honeycomb bionic structural chromium skeleton including seven single-room structures;
[0026] Figure 2 A schematic cross-sectional view of a single-room structure in a honeycomb bionic chromium skeleton including seven single-room structures;
[0027] Figure 3 A schematic cross-sectional view of a copper-chromium contact material having a honeycomb biomimetic chromium skeleton provided in Example 1 of the present application;
[0028] Figure 4 A schematic cross-sectional view of a single-chamber structure in the copper-chromium contact material having a honeycomb biomimetic chromium skeleton provided in Example 1 of the present application;
[0029] Figure 5 This is a schematic diagram of a model of different chromium skeleton distributions in the copper-chromium contact material described in the embodiment constructed using the simulation software comsol in Experimental Example 1;
[0030] Figure 6 This is the thermal stress simulation result diagram of the random non-directional distribution of the chromium skeleton in the copper-chromium contact material built by the simulation software comsol in Experimental Example 1;
[0031] Figure 7 This is the thermal stress simulation result diagram of the directional distribution of the hollow regular quadrangular prisms of the chromium skeleton in the copper-chromium contact material built by the simulation software comsol in Experimental Example 1;
[0032] Figure 8This is the thermal stress simulation result diagram of the directional distribution of hollow hexagonal prisms in the chromium skeleton of the copper-chromium contact material built using the simulation software Comsol for Experimental Example 1. DETAILED DESCRIPTION
[0033] The present application provides a copper-chromium contact material with a honeycomb bionic structure chromium skeleton, a preparation method and an application thereof, which are used to solve the technical problem of low performance of the copper-chromium contact material in the prior art.
[0034] The technical solution of the present application will be described clearly and completely below in conjunction with the accompanying drawings. Obviously, the described embodiments are part of the embodiments of the present application, rather than all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present application.
[0035] In view of the fact that the chromium skeleton in the current copper-chromium contact material is randomly and non-directionally distributed, and there is no preferential directional distribution, which affects the performance of the chromium contact material; the present application provides a copper-chromium contact material with a honeycomb bionic structure chromium skeleton, a preparation method and an application; the composition of the copper-chromium contact material with a honeycomb bionic structure chromium skeleton provided by the present application includes: a honeycomb structure chromium skeleton, a copper matrix, and the honeycomb structure chromium skeleton is embedded in the copper matrix; after the copper-chromium contact material provided by the present application is used in a vacuum circuit breaker, when an electrical breakdown occurs, the first breakdown phase will occur at the chromium skeleton, and the arc root will extend along the chromium skeleton of the honeycomb structure in the copper-chromium contact material. The frame moves quickly, which effectively avoids the arc gathering and the arc gathering phenomenon caused by the random non-directional distribution of the chromium skeleton in the traditional copper-chromium contact material. At the same time, the bionic structure of the honeycomb structure has the advantages of large structural heat dissipation specific surface area and high average convection heat transfer coefficient, which makes the chromium skeleton of the honeycomb structure in the copper-chromium contact material have excellent thermal diffusion performance and thermal stability, avoiding the defect of poor thermal conductivity of the chromium skeleton in the traditional copper-chromium contact material due to random non-directional distribution. The chromium skeleton of the honeycomb structure is also beneficial to improving the electrical conductivity and anti-welding performance of the copper-chromium contact material, thereby improving the performance of the copper-chromium contact material.
[0036] At the same time, the specific composition of the chromium skeleton of the honeycomb structure in the copper-chromium contact material provided in the present application is composed of 3 to 7 single-room structures; the single-room structure includes chromium sheets in the shape of hollow regular prisms, the number of chromium sheets is 2 to 5 layers, and the cross-sectional diagonal lines of the hollow regular prism-shaped chromium sheets partially overlap and have the same center; wherein a schematic diagram of the chromium skeleton of the honeycomb bionic structure including seven single-room structures is as shown in Figure 1 As shown, the single room structure is as follows Figure 2 As shown, the structural schematic diagram of the copper-chromium contact material having a honeycomb bionic structure chromium skeleton with three single-room structures is shown in Figure 3 As shown, it includes a honeycomb bionic structure chromium skeleton and a copper matrix with three single-room structures. Figure 4shown.
[0037] As for the distance between adjacent hollow regular prism-shaped chromium sheets, the present application sets the spacing to be 0.5-2 μm, and the thickness of the chromium sheet is 0.5-2 μm, and the side length is 5-10 μm.
[0038] For the hollow regular prism shape of the sheet in the single-room structure, the present application can select a chromium sheet in the shape of a hollow regular triangular prism, a hollow regular quadrangular prism or a hollow hexagonal regular prism; preferably, the chromium sheet in the shape of a hollow hexagonal regular prism is beneficial to reducing the resistance of the fluid network system and reducing the local flow dead zone formed by the corners / right angles of the hollow regular triangular prism / hollow regular quadrangular prism compared with the sheets of the hollow regular triangular prism and the hollow regular quadrangular prism, thereby improving the electrical conductivity / heat exchange efficiency and further improving the electrical conductivity / thermal conductivity and other properties of the copper-chromium contact material.
[0039] For the preparation method of the copper-chromium contact material with a honeycomb bionic structure chromium skeleton provided in the present application, the chromium skeleton of the honeycomb structure is first prepared by a 3D printing process, and then the copper matrix is filled into the pores of the chromium skeleton of the honeycomb structure by a vacuum infiltration process; wherein, the 3D printing process selects direct metal laser sintering equipment, electron beam melting molding equipment or selective laser sintering equipment, etc., which can be used for metal material 3D printing equipment, and the vacuum infiltration process is to melt the copper powder and then infiltrate the chromium skeleton, fill the skeleton pores with copper melt, and after cooling to room temperature, the copper-chromium contact material with a honeycomb bionic structure chromium skeleton can be obtained.
[0040] Example 1
[0041] Example 1 of the present application provides a method for preparing a copper-chromium contact material having a honeycomb bionic structure chromium skeleton, the preparation method comprising: a step of 3D printing the chromium skeleton of the honeycomb structure, and a step of vacuum infiltration to fill the pores of the chromium skeleton of the honeycomb structure with a copper matrix.
[0042] The steps of 3D printing a chromium skeleton of a honeycomb structure include: loading chromium powder into a direct metal laser sintering device and modeling a chromium skeleton of a designed honeycomb structure in the device, evacuating the vacuum to below 500 Pa, and performing 3D printing to obtain a chromium skeleton of a honeycomb structure; wherein the designed chromium skeleton of the honeycomb structure is a 3-cell structure, each of which includes 2 layers of chromium sheets in the shape of hollow regular hexagonal prisms, and its structure is as follows Figure 3-4 As shown in the figure, the thickness of the chromium sheet layer is 1μm, the side length of the outer layer is 10μm, and the spacing between adjacent chromium sheets is 0.5μm; the 3D printing parameters are: laser power is 150W, scanning speed is 100mm / s, and laser beam diameter is 100nm.
[0043] The step of vacuum infiltration to fill the pores of the chromium skeleton of the honeycomb structure with a copper matrix includes: placing the chromium skeleton of the honeycomb structure in a hollow cylindrical copper-chromium contact material graphite mold, and placing an excess infiltration pure copper block on the chromium skeleton, and then placing the graphite mold in a sintering furnace, heating to 1400°C at a rate of 10°C / min under a vacuum condition of -0.05MPa, and keeping the temperature for 30min, infiltrating the chromium skeleton with molten metal copper, filling the skeleton pores with copper melt in the graphite mold, so that the chromium skeleton of the honeycomb structure is embedded in the copper matrix, and then cooling to room temperature at a rate of 5°C / min to obtain a copper-chromium contact material with a honeycomb bionic structure chromium skeleton, wherein the mass ratio of Cu to Cr in the copper-chromium contact material is 75:25.
[0044] Experimental Example 1
[0045] The experimental example of this application uses the simulation software Comsol to build a model schematic diagram of different chromium skeleton distribution in copper-chromium contact materials, and evaluates its thermal performance through simulation experiments. The three established models are as follows: Figure 3 As shown, Figure 5 (a) shows the model of random non-directional distribution of chromium skeleton, (b) shows the model of directional distribution of chromium skeleton with regular tetrahedron, and (c) shows the model of directional distribution of chromium skeleton with regular hexagonal prism.
[0046] The simulation experiment process is the thermal stress distribution when the room temperature rises to the arc temperature of 3000K. The results of the simulation experiment are as follows: Figure 6-8 As shown, from Figure 6-8 It can be seen that the minimum thermal stress of the model with random non-directional distribution of the chromium skeleton is 0.00583μm, and the maximum thermal stress is 0.39414μm, while the minimum thermal stress of the model with directional distribution of the chromium skeleton regular tetrahedron is 0.04107μm, and the maximum thermal stress is 0.23833μm, and the minimum thermal stress of the model with directional distribution of the chromium skeleton regular hexagonal prism is 0.02686μm, and the maximum thermal stress is 0.24130μm; From the results of this simulation experiment, it can be seen that the model with directional distribution of the chromium skeleton regular tetrahedron and the model with directional distribution of the chromium skeleton regular hexagonal prism are The thermal performance is better than that of the model with random non-directional distribution of the chromium skeleton, and it has superior thermal stability and thermal diffusion capacity, which indirectly verifies that compared with the random non-directional chromium skeleton, the copper-chromium contact material provided by the present application has better thermal diffusion performance and thermal stability due to the directionally distributed honeycomb bionic structure chromium skeleton; at the same time, the thermal performance of the model with regular hexagonal prism directional distribution of the chromium skeleton is better, which indirectly shows that compared with the chromium skeleton with regular quadrangular prism directional distribution, the chromium skeleton with regular hexagonal prism directional distribution can reduce the local flow dead zone formed by right angles and reduce resistance, thereby having better thermal stability and thermal diffusion capacity.
[0047] The above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit them. Although the present application has been described in detail with reference to the aforementioned embodiments, a person skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some or all of the technical features thereof may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the scope of the technical solutions of the embodiments of the present application.
Claims
1. A copper-chromium contact material with a honeycomb bionic structure chromium skeleton, characterized in that: include: The chromium skeleton and copper matrix of the honeycomb structure; The chromium skeleton of the honeycomb structure is embedded in the copper matrix.
2. The copper-chromium contact material with a honeycomb bionic structure chromium skeleton according to claim 1, characterized in that: The chromium skeleton of the honeycomb structure includes: 3 to 7 single-room structures; One of the single-room structures comprises: 2 to 5 layers of chrome sheets in the shape of hollow regular prisms, and the cross-sectional diagonal lines of adjacent chrome sheets in the shape of hollow regular prisms partially overlap and have the same center.
3. The copper-chromium contact material with a honeycomb bionic structure chromium skeleton according to claim 1, characterized in that: The hollow regular prism is selected from a hollow regular triangular prism, a hollow regular quadrangular prism or a hollow regular hexagonal prism.
4. The copper-chromium contact material with a honeycomb bionic structure chromium skeleton according to claim 1, characterized in that: The spacing between adjacent hollow regular prism-shaped chromium flake layers is 0.5~2μm.
5. The copper-chromium contact material with a honeycomb bionic structure chromium skeleton according to claim 1, characterized in that: The thickness of the hollow regular prism-shaped chromium sheet layer is 0.5-2 μm, and the side length is 5-10 μm.
6. The copper-chromium contact material with a honeycomb bionic structure chromium skeleton according to claim 1, characterized in that: The mass ratio of the chromium skeleton of the honeycomb structure to the copper matrix is 20-30:70-80.
7. A method for preparing a copper-chromium contact material having a honeycomb bionic structure chromium skeleton according to any one of claims 1 to 6, characterized in that: Includes steps: Step S1, loading chromium powder into a 3D printing device and establishing a 3D model of a chromium skeleton, and performing 3D printing to obtain a chromium skeleton with a honeycomb structure; Step S2, placing the chromium skeleton of the honeycomb structure in a copper-chromium contact material mold, infiltrating the pores of the chromium skeleton of the honeycomb structure with the heated and melted copper powder, and obtaining the copper-chromium contact material with the chromium skeleton of the honeycomb structure after cooling.
8. The method for preparing a copper-chromium contact material having a honeycomb bionic structure chromium skeleton according to claim 7, characterized in that: The 3D printing device is selected from direct metal laser sintering equipment, electron beam melting molding equipment or selective laser sintering equipment.
9. Application of the copper-chromium contact material having a honeycomb bionic structure chromium skeleton as claimed in any one of claims 1 to 6 in a vacuum circuit breaker.
10. A vacuum circuit breaker, characterized in that: Including vacuum interrupter and operating mechanism; The operating mechanism is used to control the static contact material and the moving contact material in the vacuum interrupter to open or close the circuit breaker; The static contact material and the dynamic contact material are selected from the copper-chromium contact material with a honeycomb bionic structure chromium skeleton described in the first aspect.
Citation Information
Patent Citations
Contact with function of controlling directional extension movement of vacuum arc
CN102881511A
Method for preparing arc ablation resistant CuCr contact material through 3D printing
CN116586633A
Metal-graphene composite conductor and preparation method and application thereof
CN116682597A
Ordered heterostructure multi-metal composite material and preparation method thereof
CN117340274A
Copper-based conductor structure and preparation method thereof
CN117423556A