Wafer bonding method and preparation method of functional substrate thereof
By separating the wafer in a vacuum environment and applying step-by-step pressure, the bonding problems caused by air gaps and impurities in direct bonding technology are solved, and high-quality wafer bonding is achieved, avoiding displacement and holes. occur.
Patent Information
- Application Number
- CN202410867660.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-28
- Publication Date
- 2024-11-08
AI Technical Summary
In the existing semiconductor manufacturing processes, direct bonding technology can easily lead to wafer displacement and bonding holes, which mainly leads to air gaps and impurities entering the bonding interface due to different initial states and morphology, affecting the bonding quality.
By separating the wafer under vacuum, bonding is in line with the bonding and bonding step by step under pressure, gradually increasing the pressure to ensure bonding is in line with the avoidance of air gaps and impurities entering.
It effectively avoids the occurrence of bonding holes and wafer displacement, improves the yield of the wafer bonding process, and ensures the cleanliness and stability of the bonding interface.
Smart Images

Figure CN118919403A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of semiconductor manufacturing process technology, and in particular to a wafer bonding method and a method for preparing a functional substrate thereof. Background Art
[0002] As the development of Moore's Law encounters bottlenecks, a single material can no longer meet the rapid development of semiconductor technology. The technology development route beyond Moore has put forward an urgent need for heterogeneous integration technology, which integrates materials with different properties to achieve high-density integration of multiple functional devices. The bonding process is an important method to achieve heterogeneous integration technology. Among them, the direct bonding technology of the bonding process is to directly bond two wafers with sufficiently clean and smooth surfaces, and use the intermolecular force between the two wafers or the interaction force between the chemical bonds attached to the surface of the wafer. It has extremely high requirements for the flatness, surface smoothness and cleanliness of the wafer, but this direct bonding technology is prone to wafer displacement and bonding holes, mainly due to the following aspects: (1) Since the initial states and morphologies of the two bonded wafers may be different, during the bonding process, the two bonded wafers will begin to contact from multiple directions and begin to expand to the surrounding area, which can easily trap some air in the bonding interface to form air gaps and form bonding holes that cannot be eliminated; (2) Since there may be an air gap between the two bonded wafers, they need to gradually overcome the air resistance and the initial warping of the wafers before they can contact and bond with each other. In this case, it is easy to encounter obstacles such as particles or impurities during the bonding process, thus forming bonding holes that cannot be eliminated. (3) Since there may be an air gap between the two bonded wafers, the two bonded wafers may move relative to each other after contact, resulting in wafer displacement, and may also cause the alignment of the wafer bonding area to shift. Summary of the invention
[0003] In view of the above problems in the prior art, the present application provides a wafer bonding method and a functional substrate preparation method thereof, which can avoid the occurrence of wafer displacement and bonding holes caused by the wafer direct bonding technology in the prior art. The specific technical solution is as follows: In one aspect, the present application provides a wafer bonding method, the method comprising: Providing a first wafer and a second wafer, wherein the first wafer has a first bonding surface, and the second wafer has a second bonding surface; Separating the first wafer and the second wafer, and arranging the first bonding surface and the second bonding surface relative to each other and aligning them; In a vacuum environment, the first wafer and the second wafer are brought close to each other and subjected to a bonding process. During the bonding process of the first wafer and the second wafer, pressure is applied to at least one of the first wafer and the second wafer so that the first bonding surface and the second bonding surface are aligned and bonded under the action of pressure.
[0004] In a possible implementation manner, during the process of applying pressure to at least one of the first wafer and the second wafer, the pressure applying position is located in the middle of the first wafer and / or the second wafer being pressed.
[0005] In a possible implementation manner, applying pressure to at least one of the first wafer and the second wafer includes: applying pressure in steps, during which pressure is applied in steps to the first bonding surface and / or the second bonding surface, and the pressure application area is different each time, so that the first bonding surface and the second bonding surface are bonded in steps under pressure, and the pressure application area refers to an effective pressure area extending circumferentially from the pressure application position.
[0006] In a possible implementation manner, during the step-by-step pressure application process, the pressure application area range of the latter pressure application is larger than the pressure application area range of the previous pressure application.
[0007] In a possible implementation manner, during the step-by-step pressure application process, the pressure applied to the pressure application area each time is not greater than 10000N, and the pressure applied to the pressure application area each time is not less than 10N.
[0008] In a possible implementation manner, during the step-by-step pressing process, the number of times the step-by-step pressing is performed is determined by the total area of the first bonding surface and / or the second bonding surface, and the area of a pre-set pressing area for each time pressure is applied to the first bonding surface and / or the second bonding surface.
[0009] In a possible implementation manner, the step-by-step pressurization includes a first pressurization process and a second pressurization process, wherein the first pressurization process includes pressurization using a first pressure, and the second pressurization process includes pressurization using a second pressure, and the step-by-step pressurization process satisfies at least one of the following characteristics: The pressure range of the first pressure is 10-500N; The pressure range of the second pressure is 500-10000N; The area of the pressure region of the first pressure accounts for 0.001% to 25% of the total area of the first wafer; The area of the second pressure application region accounts for 25% to 100% of the total area of the first wafer; The pressure application area of the first pressure and the pressure application area of the second pressure both cover the center of the first wafer; The duration of applying the first pressure is ≤30s.
[0010] In a possible implementation manner, the step-by-step pressurization includes a first pressurization process, a second pressurization process, and a third pressurization process, wherein the first pressurization process includes pressurization using a first pressure, the second pressurization process includes pressurization using a second pressure, and the third pressurization process includes pressurization using a third pressure, and the step-by-step pressurization process satisfies at least one of the following characteristics: The pressure range of the first pressure is 10-500N; The pressure range of the second pressure is 200-2000N; The pressure range of the third pressure is 500-10000N; The area of the pressure region applied by the first pressure accounts for 0.001% to 25% of the total area of the first wafer; The area of the pressure region applied by the second pressure accounts for 25% to 50% of the total area of the first wafer; The area of the pressure region applied by the third pressure accounts for 50% to 100% of the total area of the first wafer; The pressure application area of the first pressure, the pressure application area of the second pressure, and the pressure application area of the third pressure all cover the center of the first wafer; The duration of applying the first pressure and the duration of applying the second pressure are both ≤30s.
[0011] In a possible implementation manner, the preparation method satisfies at least one of the following characteristics: Before bringing the first wafer and the second wafer closer to each other and performing a bonding process, the method further includes: Under a vacuum environment, applying pressure to at least one of the first wafer and the second wafer so that external pressure exists when the first wafer and the second wafer are in contact; Under the vacuum environment, bringing the first wafer and the second wafer close to each other and performing a bonding process comprises: In a vacuum environment, after the first wafer and the second wafer are brought close to and in contact with each other, during the process of applying pressure to at least one of the first wafer and the second wafer for bonding, the vacuum degree of the vacuum environment is reduced so that the first bonding surface and the second bonding surface are aligned and bonded under pressure.
[0012] In a possible implementation manner, the preparation method satisfies at least one of the following characteristics: When the first wafer and the second wafer are brought into contact, the vacuum degree under the vacuum environment is a first vacuum degree. After the first wafer and the second wafer are brought close to and into contact, the vacuum degree under the vacuum environment is a second vacuum degree. The difference between the first vacuum degree and the second vacuum degree ranges from 1E2mbar to 1E3mbar.
[0013] During the contact and bonding process, the vacuum degree of the vacuum environment is gradually reduced based on the step-by-step pressure application process. The vacuum degree in the previous pressure application process is higher than the vacuum degree in the next pressure application process. The difference in vacuum degree between two adjacent pressure application processes ranges from 1E2mbar to 1E4mbar.
[0014] On the other hand, the present application provides a method for preparing a functional substrate, which at least includes: the steps included in the wafer bonding method described in the above embodiment, removing the non-functional layer of the structure obtained by the wafer bonding method to obtain a functional substrate.
[0015] Based on the above technical solution, this application has the following beneficial effects: The technical solution of the present application provides a wafer bonding method, comprising the following steps: providing a first wafer and a second wafer, separating the first wafer and the second wafer, and making the first bonding surface of the first wafer and the second bonding surface of the second wafer relatively arranged and aligned, in a vacuum environment, bringing the first wafer and the second wafer close to each other and performing a bonding process, and during the bonding process of the first wafer and the second wafer, applying pressure to at least one of the first wafer and the second wafer so that the first bonding surface and the second bonding surface are aligned and bonded under the action of pressure. By separating the first wafer and the second wafer, it is possible to avoid the two wafers from contacting from multiple positions during the bonding process to generate air gaps, and to avoid the generation of bonding holes due to the presence of air gaps during the bonding process. By bonding the first wafer and the second wafer in a vacuum environment, it is possible to avoid particles or impurities in the air from entering the bonding interface, so that the bonding interface when the first wafer and the second wafer are bonded is clean, and the generation of bonding holes is avoided. By applying pressure to at least one of the first wafer and the second wafer, the air in the bonding process can be discharged in time, and the generation of air gaps and the occurrence of wafer displacement are avoided. The use of this method effectively improves the yield of the wafer bonding process. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] In order to more clearly illustrate the technical solution of the present application, the following is a brief introduction to the drawings required for use in the embodiments or prior art descriptions. Obviously, the drawings described below are only some embodiments of the present application, and for ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0017] Figure 1 The figure is a schematic diagram of the steps of a method for preparing a functional substrate in a specific embodiment of the present invention.
[0018] Figure 2 The figure is a schematic diagram of the steps of a method for preparing a functional substrate in a specific embodiment of the present invention.
[0019] Figure 3 Schematic diagram of the steps of the wafer bonding method in Embodiment 3-4 of the present invention.
[0020] Figure 4 Schematic diagram of the steps of the wafer bonding method in Examples 5-6 of the present invention.
[0021] Figure 5 Schematic diagram of the bonding interface after wafer bonding in Example 4 of the present invention.
[0022] Figure 6 It is a schematic diagram of the bonding interface after wafer bonding in Comparative Example 1 of the present invention.
[0023] Figure 7 Schematic diagram of the bonding interface after wafer bonding in Comparative Example 2 of the present invention.
[0024] In the figure: 1-first wafer, 11-first bonding surface, 2-second wafer, 12-second bonding surface, 3-structure with defective layer, 4-functional substrate with first damaged layer, 5-first functional substrate, 6-wafer structure, 7-structure with second damaged layer, 8-second functional substrate, 21-pressure application area of first pressure, 22-pressure application area of second pressure, 31-pressure application area of first pressure, 32-pressure application area of second pressure, 33-pressure application area of third pressure, 101-first substrate layer, 102-defective layer, 103-first functional thin film layer, 104-second substrate layer, 105-first damaged layer, 106-third substrate layer, 107-fourth substrate layer, 108-second damaged layer, 109-second functional thin film layer. DETAILED DESCRIPTION
[0025] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.
[0026] For the following defined terms, these definitions shall apply unless a different definition is given in the claims or elsewhere in this specification. All numerical values, whether or not explicitly indicated, are defined herein as modified by the term "about". The term "about" generally refers to a numerical range that a person of ordinary skill in the art considers to be equivalent to the stated values to produce substantially the same properties, functions, results, etc. A numerical range indicated by a lower value and a higher value is defined to include all numerical values included in the numerical range and all subranges included in the numerical range.
[0027] It should be noted that the terms "first", "second", etc. in the specification and claims of the present application and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the data used in this way can be interchanged where appropriate, so that the embodiments of the present application described herein can be implemented in an order other than those illustrated or described herein. In addition, the terms "including" and "having" and any variations thereof are intended to cover non-exclusive inclusions.
[0028] On the one hand, a method for preparing wafer bonding provided by an embodiment of the present application is described below, the method comprising: S1: providing a first wafer and a second wafer, wherein the first wafer has a first bonding surface, and the second wafer has a second bonding surface; In some embodiments, the first bonding surface refers to a surface of the first wafer used for bonding, and similarly, the second bonding surface also refers to a surface of the second wafer used for bonding. Because the cleanliness of the surface between the two bonded wafers determines whether the bonding is successful and the bonding strength, if there are dust particles between the bonding sheets, the bonding is difficult to succeed. Even if the bonding is successful, the dust in the middle of the bonding body will form a bonding void (local warping, that is, the particles are bonded around but the part with particles is not bonded), which directly affects its application. High surface roughness (similar to the presence of particles, that is, the surface is uneven) will also reduce the bonding area of the bonding surface, thereby reducing the key bonding force-Van der Waals force, weakening the bonding strength, and affecting its application. If the surface roughness of the two wafers is less than 1nm, the wafers can be spontaneously bonded through hydrogen bonds, Van der Waals forces, etc., that is, pre-bonding. Therefore, in order to meet the requirements of subsequent bonding, the first bonding surface and the second bonding surface need to meet the predetermined conditions that: the roughness of the first bonding surface and the second bonding surface are both lower than 1 nm, and the cleanliness is such that there are 1-5 nanometer-level particles.
[0029] Specifically, the material of the first wafer and the second wafer includes at least one of silicon, silicon oxide, germanium, lithium niobate, lithium tantalate, aluminum nitride, gallium nitride, silicon carbide, sapphire, III-V compound semiconductors, quartz, gallium oxide or diamond.
[0030] S2: Separate the first wafer and the second wafer, and arrange the first bonding surface and the second bonding surface relatively and aligned; by separating the first wafer and the second wafer, it is possible to avoid the two wafers from contacting from multiple directions during the bonding process to generate air gaps, thereby avoiding the generation of bonding holes due to the existence of air gaps during the bonding process.
[0031] Specifically, the first wafer and the second wafer are separated, and the first bonding surface and the second bonding surface are arranged relative to each other and aligned, specifically including: In a vacuum environment, the first wafer and the second wafer are separated, and the first bonding surface and the second bonding surface are arranged opposite to each other and aligned.
[0032] Specifically, the vacuum degree of the vacuum environment during the separation process is in the range of 100mbar-1000mbar. The vacuum degree of the vacuum environment during the separation process can be any point value within the above range, which is not enumerated here. By using a vacuum environment during the separation process, the bonding interface during wafer bonding can be made cleaner and the influence of suspended particles and water vapor in the air can be reduced.
[0033] Specifically, the separation process of the first wafer and the second wafer includes: using a partition to separate the first wafer and the second wafer by a preset distance, and the partition is distributed on both sides of the first wafer and the second wafer, so that the first bonding surface and the second bonding surface are arranged opposite to each other and aligned. By separating the first wafer and the second wafer, it is possible to avoid the two wafers from contacting from multiple directions during the bonding process to generate air gaps, and avoid the generation of bonding holes due to the existence of air gaps during the bonding process.
[0034] Specifically, the number of partitions during the separation process is ≥ 2. The number of partitions during the separation process can be any point value within the above range, which is not enumerated here. By limiting the number range of partitions, the stability of the wafer during the pressure application process can be ensured.
[0035] Specifically, the preset distance is 0.1-1 mm. The preset distance can be any point value within the above range, which is not enumerated here. When the preset distance is small, the first wafer and the second wafer may contact each other due to their own morphology, thereby generating an air gap. When the preset distance is too large, one wafer will freely fall and contact the other wafer when the interval is removed, which may cause wafer bonding deviation, particle introduction, etc.
[0036] Specifically, during the separation process, the partition contacts the first bonding surface of the first wafer to form a first contact surface, and contacts the second bonding surface of the second wafer to form a second contact surface. The length of the first contact surface and the length of the second contact surface are both 1-10 mm. The length of the first contact surface and the second contact surface can be any point value within the above range, which is not enumerated here. By limiting the length of the first contact surface and the length of the second contact surface, on the one hand, if the contact surface between the wafer and the partition is too short, it may cause the two wafers to contact prematurely and cause multi-point bonding. On the other hand, if the contact surface between the wafer and the partition is too long, the wafer may be damaged when the partition is removed.
[0037] In some embodiments, after the first wafer and the second wafer are separated, the method further includes: preheating at least one of the first wafer and the second wafer. The two wafers are preheated before bonding, and the preheating process can reduce the temperature difference between the bonding temperature and the heat treatment temperature of the wafers, reduce the thermal strain caused by the temperature difference and the different thermal expansion coefficients of the materials during the heat treatment process, and help improve the strength of the wafer bonding.
[0038] Specifically, the temperature of the preheating treatment is 25°C ~ 450°C, and the time is 5s ~ 5h. The temperature and time of the preheating treatment can be any point value within the above range, which is not enumerated here. By limiting the temperature range of the preheating treatment, it is avoided that the temperature is too high or too low, which may cause damage to the wafer or performance degradation; if the preheating time is too short, the wafer cannot be fully preheated to the required temperature, and the bonding strength of the wafer will be reduced; if the preheating time is too long, the production efficiency will be reduced, and it may affect the performance of the final product.
[0039] In some embodiments, after the first wafer and the second wafer are separated, the method further comprises: performing a plasma activation process on at least one of the first wafer and the second wafer in a vacuum environment. Plasma activation process can improve wafer bonding quality and reduce stress and defects.
[0040] Specifically, the process of performing the plasma activation treatment on at least one of the first wafer and the second wafer may be performed before or after performing the preheating treatment on the first wafer or the second wafer.
[0041] Specifically, the vacuum degree of the vacuum environment used in the plasma activation process is 1E-4mbar-100mbar. If the vacuum degree is too high during the plasma activation process, the density of the plasma will be insufficient, thereby weakening the plasma treatment effect on the wafer surface, thereby affecting the wafer bonding quality. If the vacuum degree is too low, it may cause defects in the bonding interface, such as holes or cracks.
[0042] Specifically, the plasma activation process further includes performing plasma activation on at least one of the first wafer and the second wafer using at least one of nitrogen, oxygen, and a rare gas.
[0043] S3: In a vacuum environment, the first wafer and the second wafer are brought close to each other and bonded. During the bonding process of the first wafer and the second wafer, pressure is applied to at least one of the first wafer and the second wafer so that the first bonding surface and the second bonding surface are aligned and bonded under pressure. By bonding the first wafer and the second wafer in a vacuum environment, particles or impurities in the air can be prevented from entering the bonding interface, so that the bonding interface of the first wafer and the second wafer is clean when they are bonded, and the generation of bonding holes is avoided. By applying pressure to at least one of the first wafer and the second wafer, the air in the bonding process can be discharged in time, avoiding the generation of air gaps and the occurrence of wafer displacement. The use of this method effectively improves the yield of the wafer bonding process.
[0044] In some embodiments, before bringing the first wafer and the second wafer close to each other and performing a bonding process, the method further includes: In a vacuum environment, at least one of the first wafer and the second wafer is pressurized so that there is external pressure when the first wafer and the second wafer are in contact. This arrangement can ensure the stability of wafer bonding during the subsequent pressurization process, thereby improving the bonding quality of the wafers.
[0045] Specifically, in a vacuum environment, applying pressure to at least one of the first wafer and the second wafer so that there is an external pressure effect when the first wafer and the second wafer are in contact, including: In a vacuum environment, pressure is applied to at least one of the first wafer and the second wafer for a period of time, so that external pressure exists when the first wafer and the second wafer are in contact.
[0046] Specifically, the duration of applying pressure to at least one of the first wafer and the second wafer is 1-30 seconds, and the applied pressure is 10-500 N. By limiting the duration to 1-30 seconds, the stability of the wafer is improved during subsequent wafer bonding, and limiting the applied pressure to 10-500 N to avoid excessive pressure that may cause damage to the wafer.
[0047] In some embodiments, in a vacuum environment, bringing the first wafer and the second wafer close to each other and performing a bonding process includes: In a vacuum environment, after the first wafer and the second wafer are brought close to and in contact with each other, during the process of applying pressure to at least one of the first wafer and the second wafer for bonding, the vacuum degree of the vacuum environment is reduced so that the first bonding surface and the second bonding surface are aligned and bonded under the action of pressure. By reducing the vacuum degree, the influence of suspended particles and water vapor in the air can be reduced, and a relatively clean bonding interface can be achieved.
[0048] Specifically, in a vacuum environment, bringing the first wafer and the second wafer close to and in contact with each other includes: performing a spacer removal process on the first wafer and the second wafer to bring the first wafer close to and in contact with each other.
[0049] Specifically, the spacing removal process includes: removing a partition between the first wafer and the second wafer, so that the first wafer and the second wafer are close to and in contact with each other.
[0050] Specifically, when the first wafer is brought into contact with the second wafer, the vacuum degree in the vacuum environment is a first vacuum degree. After the first wafer and the second wafer are brought close to and into contact with each other, the vacuum degree in the vacuum environment is a second vacuum degree. The difference between the first vacuum degree and the second vacuum degree ranges from 1E2mbar to 1E3mbar.
[0051] Specifically, the ranges of the first vacuum degree and the second vacuum degree are both 1E-4 mbar-1000 mbar. By limiting the ranges of the first vacuum degree and the second vacuum degree, a good bonding effect can be achieved and the influence of inappropriate vacuum degree on bonding strength can be avoided.
[0052] Specifically, the first vacuum degree is 1E-3 mbar-100 mbar, and the second vacuum degree is 1E-4 mbar-10 mbar.
[0053] In some embodiments, during the process of applying pressure to at least one of the first wafer and the second wafer, the pressure application position is located in the middle of the first wafer and / or the second wafer being pressed. By applying pressure to the middle of at least one of the first wafer and the second wafer, air can be discharged in time during the bonding process of the two wafers, which greatly avoids the generation of air gaps and improves the bonding quality of the wafers.
[0054] In some embodiments, applying pressure to at least one of the first wafer and the second wafer includes: applying pressure once, and during the single pressure application, the pressure application position is located in the middle of the first wafer and / or the second wafer being pressed. By adopting a single pressure application, the work efficiency can be improved and the wafer bonding effect can be ensured to be better.
[0055] Specifically, the specific step of applying pressure once includes: applying pressure to the middle of at least one of the first wafer and / or the second wafer to achieve bonding of the first wafer and the second wafer.
[0056] Specifically, during a single pressurization process, the applied pressure ranges from 10 N to 1000 N. By limiting the pressure range of a single pressurization, on the one hand, it is possible to avoid excessive pressure causing damage to the wafer during the bonding process, and on the other hand, it is possible to avoid excessive pressure causing low bonding strength of the wafer.
[0057] In some embodiments, applying pressure to at least one of the first wafer and the second wafer includes: applying pressure in steps, during which the first bonding surface and / or the second bonding surface are pressed in steps, and the pressure application area of each pressure application is different, so that the first bonding surface and the second bonding surface are bonded in steps under pressure, and the pressure application area refers to an effective pressure area extending circumferentially from the pressure application position. By adopting the step-by-step pressure application method, the air when the first wafer and the second wafer are bonded can be gradually discharged, thereby improving the bonding quality of the wafers, and avoiding wafer displacement and the generation of bonding holes. At the same time, the force on the two wafers when bonding can be made more uniform, thereby avoiding the occurrence of wafer breakage.
[0058] Specifically, during the step-by-step pressure application process, the pressure application area of the subsequent pressure application is larger than that of the previous pressure application. When the pressure application area of the subsequent pressure application is smaller than that of the previous pressure application, the air in different pressure application areas may not be discharged in time, thereby causing the air gap phenomenon.
[0059] Specifically, in the step-by-step pressing process, the pressing area of the latter pressing covers the pressing area of the previous pressing. This arrangement can improve the bonding strength of the wafer.
[0060] In some embodiments, the shape of the pressure area can be a figure with a center, such as a circle, an equilateral triangle, etc., or a figure without a center, such as a trapezoid, etc.
[0061] In some embodiments, in the step-by-step pressure application process, the pressure applied to the pressure area each time is not greater than 10000N, and the pressure applied to the pressure area each time is not less than 10N. By adopting this setting, on the one hand, it is avoided that the pressure applied to the pressure area each time is too large, which may cause the wafer to break easily. On the other hand, it is avoided that the pressure applied to the pressure area each time is too small, which may cause low wafer bonding strength.
[0062] In some embodiments, during the step-by-step pressing process, the number of times the step-by-step pressing is applied is determined by the total area of the first bonding surface and / or the second bonding surface. By adopting this configuration, the number of times the step-by-step pressing is applied can be determined according to the area of the wafer, thereby improving work efficiency, and being applicable to wafers of different sizes, thereby expanding the scope of application of the method.
[0063] Specifically, when the area of the first bonding surface and / or the second bonding surface is not greater than 80 cm 2 The number of times of step-by-step pressing is 1-3 times, when the area of the first bonding surface and / or the second bonding surface is 80-400cm 2 When applying pressure in steps, the number of times of pressure application ranges from 2 to 5 times.
[0064] In some embodiments, the pressure area during the step-by-step pressure application process is circular, and the diameter of the pressure area gradually increases with the increase in the number of pressure applications. When the area of the first bonding surface and / or the second bonding surface is not greater than 80 cm 2 After each step of pressure application, the diameter of the pressure area increases by 0.1-5cm.
[0065] In some embodiments, the pressure area during the step-by-step pressure application process is circular, and the diameter of the pressure area gradually increases with the increase in the number of pressure applications. When the area range of the first bonding surface and / or the second bonding surface is 80-400 cm 2 After each step of pressure application, the diameter of the pressure area increases by 0.1-10cm.
[0066] In some embodiments, the step-by-step pressurization includes a first pressurization process and a second pressurization process, wherein the first pressurization process includes pressurization with a first pressure, and the second pressurization process includes pressurization with a second pressure. By performing the first pressurization process and the second pressurization process, the pressure can be gradually increased, so that the air in the bonding process can be slowly discharged to avoid the generation of air gaps. At the same time, the force on the wafer is more uniform, the bonding accuracy is improved, and defects caused by uneven pressure are avoided.
[0067] Specifically, the specific steps of applying pressure in steps include: applying a first pressure to a side of the first wafer away from the first bonding surface for a period of time so that the pressure area of the first pressure is bonded to the second wafer, and then applying a second pressure to a side of the first wafer away from the second bonding surface so that the pressure area of the second pressure is bonded to the second wafer.
[0068] Specifically, the duration of applying the first pressure is ≤30s. By limiting the duration of the first pressure, the bonding strength during the wafer bonding process can be guaranteed, and at the same time, there is enough time for the bonding wave to expand outward from the middle to avoid the occurrence of multi-point bonding.
[0069] Specifically, the duration of applying the first pressure is 5-30s. The duration of applying the first pressure and the duration of applying the second pressure can be any point value within the above range, which is not enumerated here. By further limiting the duration of the first pressure, while ensuring the bonding strength of the wafer, the work efficiency is also improved.
[0070] Specifically, the pressure range of the first pressure in the first pressure treatment process is 10-500N, and the pressure range of the second pressure in the second pressure treatment process is 500-10000N. The upper limit value of the first pressure can be but not limited to 500N, 490N, 480N, etc., and the lower limit value of the first pressure can be but not limited to 10N, 11N, 12N, etc.; it can be understood that the first pressure can also be any point value within the above range, which is not enumerated here. The upper limit value of the second pressure can be but not limited to 10000N, 9999N, 9998N, etc., and the lower limit value of the second pressure can be but not limited to 500N, 501N, 502N, etc.; it can be understood that the second pressure can also be any point value within the above range, which is not enumerated here. By limiting the pressure range of the first pressure to 10-500N and the pressure range of the second pressure to 500-1000N, the second pressure is greater than the first pressure. Gradually increasing the pressure helps to control the bonding and avoid damage to the wafer due to excessive pressure or unnecessary stress concentration. It can help form a tighter bond between wafers, reduce bubbles and gaps, and improve bonding strength and reliability.
[0071] Specifically, the area of the first pressure application region in the first pressure application process accounts for 0.001% to 25% of the total area of the first wafer, and the area of the second pressure application region accounts for 25% to 100% of the total area of the first wafer. Furthermore, the area of the first pressure application region is 0.02-5 cm 2 The second pressure area is 18-350cm 2 . The area of the pressure area of the first pressure and the area of the pressure area of the second pressure can be any point value within the above range, which will not be enumerated here. By limiting the area of the pressure area of the first pressure, it is avoided that the area of the pressure area is too large, which may cause uneven pressure distribution and increase stress concentration, thereby reducing bonding strength and reliability. In addition, too large a pressure range may cause deformation or damage to the material, further affecting the bonding quality. By limiting the area of the pressure area of the second pressure, it is avoided that the area of the pressure area of the second pressure is too small, which may result in low bonding strength of the wafer.
[0072] Specifically, the pressure area of the first pressure and the pressure area of the second pressure both cover the center of the first wafer. Furthermore, the distance between the center of the pressure area of the first pressure and the center of the first wafer is 0-5cm, and the distance between the center of the pressure area of the second pressure and the center of the first wafer is 0-5cm. The distance between the center of the pressure area of the first pressure and the center of the first wafer and the distance between the center of the pressure area of the second pressure and the center of the first wafer can be any point value within the above range, which are not enumerated here. By respectively limiting the distance between the pressure area of the first pressure and the pressure area of the second pressure and the center of the first wafer, the flatness of the wafer during bonding can be ensured, stress concentration can be reduced, and the bonding quality and bonding process yield can be effectively improved.
[0073] Specifically, the shapes of the pressure application areas of the first pressure and the second pressure can be figures with a center, such as a circle, a rectangle, a square, an equilateral triangle, a dot, etc., and the present application does not make any specific limitation here.
[0074] In some embodiments, the step-by-step pressurization includes a first pressurization process, a second pressurization process, and a third pressurization process, wherein the first pressurization process includes pressurization with a first pressure, the second pressurization process includes pressurization with a second pressure, and the third pressurization process includes pressurization with a third pressure. The three-step pressurization method has a better wafer bonding effect, but the bonding equipment and process requirements are more complicated, the use cost is higher, and the work efficiency is reduced.
[0075] Specifically, the specific steps of applying pressure in steps include: applying a first pressure to the side of the first wafer away from the first bonding surface for a period of time so that the pressure area of the first pressure is bonded to the second wafer, then applying a second pressure to the side of the first wafer away from the first bonding surface so that the pressure area of the second pressure is bonded to the second wafer, and finally applying a third pressure to the side of the first wafer away from the first bonding surface so that the pressure area of the third pressure is bonded to the second wafer.
[0076] Specifically, the duration of applying the first pressure and the duration of applying the second pressure are both ≤30s. By limiting the duration of the first pressure and the second pressure to 5-30s, it is avoided that the wafer is cracked or damaged due to too long a pressure time, and the wafer bonding strength is insufficient due to too short a pressure time.
[0077] Further, the duration of applying the first pressure is 5-25s, and the duration of applying the second pressure is 10-30s. The duration of applying the first pressure and the duration of applying the second pressure can be any point value within the above range, which is not enumerated here. By further limiting the duration of the first pressure to 5-25s, the work efficiency can be improved while ensuring the bonding strength of the wafer.
[0078] Specifically, the pressure range of the first pressure is 10-500N, the pressure range of the second pressure is 200-2000N, and the pressure range of the third pressure is 500-10000N. The upper limit value of the first pressure can be but not limited to 500N, 490N, 480N, etc., and the lower limit value of the first pressure can be but not limited to 10N, 11N, 12N, etc.; it can be understood that the first pressure can also be any point value within the above range, which is not enumerated here. The upper limit value of the second pressure can be but not limited to 2000N, 1999N, 1998N, etc., and the lower limit value of the second pressure can be but not limited to 200N, 201N, 202N, etc.; it can be understood that the second pressure can also be any point value within the above range, which is not enumerated here. The upper limit of the third pressure may be, but not limited to, 10000N, 9999N, 9998N, etc., and the lower limit of the third pressure may be, but not limited to, 500N, 501N, 502N, etc.; it is understandable that the third pressure may also be any point value within the above range, which is not enumerated here. By gradually limiting the range of the pressure applied by the first pressure, the second pressure, and the third pressure, the accuracy of the pressure application can be improved, and the force applied to the bonded wafers can be made more uniform, thereby improving the bonding accuracy and optimizing the performance of subsequent products.
[0079] Specifically, the area of the pressure region applied by the first pressure accounts for 0.001% to 25% of the total area of the first wafer, the area of the pressure region applied by the second pressure accounts for 25% to 50% of the total area of the first wafer, and the area of the pressure region applied by the third pressure accounts for 50% to 100% of the total area of the first wafer. Furthermore, the area of the pressure region of the first pressure is 0.02-5cm 2 The second pressure area is 3-180cm 2 The third pressure area is 18-350cm 2 . The pressure area of the first pressure, the pressure area of the second pressure, and the pressure area of the third pressure can be any point value within the above range, which is not enumerated here. By gradually increasing the pressure area, the increase in void volume caused by thermal expansion of gas during heat treatment can be reduced, bonding defects can be reduced, and the bonding effect can be improved. At the same time, the force on the wafer in the radial direction can be made more uniform, thereby optimizing the wafer bonding process, adjusting the diffusion speed of the bonding wave, and improving the accuracy of wafer bonding.
[0080] Specifically, the pressure area of the first pressure, the pressure area of the second pressure, and the pressure area of the third pressure all cover the center of the first wafer. Further, the distance between the center of the pressure area of the first pressure and the center of the first wafer is 0-5cm, the distance between the center of the pressure area of the second pressure and the center of the first wafer is 0-5cm, and the distance between the center of the pressure area of the third pressure and the center of the first wafer is 0-5cm. The distance between the center of the pressure area of the first pressure and the center of the first wafer, the distance between the center of the pressure area of the second pressure and the center of the first wafer, and the distance between the center of the pressure area of the third pressure and the center of the first wafer can be any point value within the above range, which is not enumerated here. By limiting the center distances of the pressure areas of the first pressure, the second pressure, and the third pressure, the pressure can be more evenly transmitted to the entire wafer surface, reducing damage or defects caused by uneven pressure, while ensuring that the contact area between the wafers is maximized, thereby enhancing the bonding strength.
[0081] Specifically, the shapes of the pressure application areas of the first pressure, the second pressure and the third pressure can be figures with a center, such as a circle, a rectangle, a square, an equilateral triangle, etc., and the present application does not make specific limitations here.
[0082] In some embodiments, during the contact and bonding process, the vacuum degree of the vacuum environment is gradually reduced based on the step-by-step pressure application process, the vacuum degree in the previous pressure application process is higher than the vacuum degree in the next pressure application process, and the difference in the vacuum degree in the pressure application process between two adjacent steps ranges from 1E2mbar to 1E4mbar. By limiting the difference in the vacuum degree in the step-by-step pressure application process, the bonding interface can be made cleaner and the bonding effect can be better.
[0083] In some embodiments, the first wafer and the second wafer after bonding are subjected to heat treatment, and the bonding strength of the bonded wafers can be improved by heat treatment.
[0084] Specifically, the first wafer and the second wafer after bonding are subjected to heat treatment, including: performing the treatment in a vacuum environment or in a protective atmosphere formed by at least one of nitrogen, oxidizing gas, rare gas, and air.
[0085] Specifically, the temperature of the heat treatment is 50-1000° C. If the temperature of the heat treatment is too high, it may cause oxidation, cracks or other forms of damage to the bonding interface, reduce the bonding strength, and also cause thermal stress inside the wafer to cause the wafer to crack. If the temperature of the heat treatment is too low, it is not enough to activate sufficient intermolecular forces, resulting in insufficient bonding strength.
[0086] On the other hand, the following describes a method for preparing a functional substrate provided by an embodiment of the present application, the method at least comprising: removing a non-functional layer from a structure obtained by the wafer bonding method as in the above-mentioned embodiment, to obtain a functional substrate. The quality of the functional substrate obtained by the wafer bonding method is better.
[0087] In some embodiments, Figure 1 As shown, the structure obtained by the wafer bonding method removes the non-functional layer to obtain a functional substrate, which specifically includes: before the first wafer 1 and the second wafer 2 are separated, ion implantation is performed on the first bonding surface 11 or the second bonding surface 12 to form a defect layer 102 at a preset depth of the first wafer 1 or the second wafer 2; The structure 3 with a defective layer obtained by the wafer bonding method is heat-treated to peel off part of the wafer along the defective layer to obtain a functional substrate 4 with a first damaged layer 105, and then the functional substrate 4 with the first damaged layer 105 is annealed and flattened to obtain a first functional substrate 5, and the temperature of the annealing treatment is not lower than the temperature of the heat treatment.
[0088] Specifically, the structure 3 with defective layers includes, from top to bottom, a first substrate layer 101, a defective layer 102, a first functional thin film layer 103, and a second substrate layer 104. The functional substrate 4 with defective layers includes, from top to bottom, a first damaged layer 105, a first functional thin film layer 103, and a second substrate layer 104; the first functional substrate 5 includes, from top to bottom, a first functional thin film layer 103 and a second substrate layer 104.
[0089] Specifically, the temperature of the heat treatment is 50°C-1000°C, and the temperature of the annealing treatment is 100°C-1000°C.
[0090] In some embodiments, Figure 2 As shown, the non-functional layer of the structure obtained by the wafer bonding method is removed to obtain a functional substrate, which specifically includes: heat treating and thinning the wafer structure 6 obtained by the wafer bonding method to obtain a structure 7 with a second damaged layer, and then flattening the structure 7 with the second damaged layer to obtain a second functional substrate 8.
[0091] Specifically, the wafer structure 6 includes, from top to bottom, a third substrate layer 106 and a fourth substrate layer 107. The structure 7 with a damaged layer includes, from top to bottom, a second damaged layer 108, a second functional film layer 109 and a fourth substrate layer 106. The second functional substrate 8 includes, from top to bottom, a second functional film layer 108 and a fourth substrate layer 106.
[0092] Specifically, the heat treatment temperature is 50°C-1000°C. The following reference Figure 1-4 The specific embodiments of the present application are introduced in conjunction with the above-mentioned wafer bonding method and the method for preparing a functional substrate thereof. The following embodiments describe the technical solution of the present application in more detail, and these embodiments are only used for illustrative purposes, because various modifications and changes within the scope of the disclosure of the present application are obvious to those skilled in the art. The reagents used in the embodiments can be obtained commercially or synthesized according to conventional methods, and can be used directly without further treatment, and the instruments and devices used in the embodiments can be obtained commercially.
[0093] Example 1 This embodiment provides a wafer bonding method, and the specific steps are as follows: S11 : providing a first wafer 1 and a second wafer 2 , wherein the first wafer 1 has a first bonding surface 11 , and the second wafer 2 has a second bonding surface 12 .
[0094] S12: In a vacuum environment with a vacuum degree of 100mbar-1000mbar, a partition is used to separate the first wafer 1 and the second wafer 2 by a preset distance, and the first bonding surface 11 and the second bonding surface 12 are arranged relatively and aligned, wherein the preset distance is 0.1-10mm, the partition and the first bonding surface 11 of the first wafer 1 form a first contact surface, the length of the first contact surface is 1-10mm, the partition and the second bonding surface 12 of the second wafer form a second contact surface, the contact length of the second contact surface is 1-10mm.
[0095] S13: In a vacuum environment with a vacuum degree of 1E-3mbar-100mbar, remove the partition between the first wafer 1 and the second wafer 2 so that the first bonding surface 11 and the second bonding surface 12 are in contact with each other, and apply pressure to the middle of the side of the first wafer 1 away from the first bonding surface 11, and the pressure range is 10N-10000N, thereby achieving bonding between the first wafer 1 and the second wafer 2.
[0096] In this embodiment, the bonding interface after wafer bonding is clean, and no air gap, wafer displacement, or bonding void is generated.
[0097] Example 2 This embodiment provides a wafer bonding method, and the same points as those in Embodiment 1 are not repeated here. The difference between this embodiment and Embodiment 1 is that: S13: Under a vacuum environment with a vacuum degree of 1E-3 mbar-100 mbar, the middle of the first wafer 1 away from the first bonding surface 11 is pressed with a pressure range of 10 N-10000 N. Then, the partition between the first wafer 1 and the second wafer 2 is removed, so that the first bonding surface 11 and the second bonding surface 12 are in contact with each other and bonded.
[0098] In this embodiment, the bonding interface after wafer bonding is clean, and no air gap, wafer displacement, or bonding void is generated.
[0099] Embodiment 3: This embodiment provides a wafer bonding method, and the specific steps are as follows: S111: Figure 1 As shown, a first wafer 1 and a second wafer 2 are provided, wherein the first wafer 1 and the second wafer 2 are single-throw wafers, respectively having a first bonding surface 10 and a second bonding surface 20 .
[0100] S112: In a vacuum environment with a vacuum degree of 100mbar-1000mbar, a partition is used to separate the first wafer 1 and the second wafer 2 by a preset distance, and the first bonding surface 11 and the second bonding surface 12 are arranged relatively to each other and aligned, wherein the preset distance is 0.1-1mm, the partition and the first bonding surface 11 of the first wafer 1 form a first contact surface, the length of the first contact surface is 1-10mm, the partition and the second bonding surface 12 of the second wafer 1 form a second contact surface, the contact length of the second contact surface is 1-10mm.
[0101] S113: Figure 1 As shown, a first pressure is applied to a side of the first wafer 1 away from the first bonding surface 11, and the first pressure is maintained for 1-30 seconds. Then, the partition between the first wafer 1 and the second wafer 2 is removed, so that the first bonding surface 11 and the second bonding surface 12 are in contact with each other. After 5-30 seconds, the pressure area 11 of the first pressure is bonded to the second wafer 2. Then, a second pressure is applied to a side of the first wafer 1 away from the first bonding surface 11. At this time, the pressure area 12 of the second pressure is bonded to the second wafer 2, thereby achieving the bonding of the first wafer 1 and the second wafer 2. The pressure range of the first pressure is 10-500N, the pressure range of the second pressure is 500-10000N, and the area of the pressure area 21 of the first pressure is 0.02-5cm 2 The area of the second pressure application area 22 is 18-350cm 2 ; The distance between the center of the pressure area of the first pressure and the center of the first wafer is 0-5cm, and the distance between the center of the pressure area of the second pressure and the center of the first wafer is 0-5cm.
[0102] In this embodiment, the bonding interface after wafer bonding is relatively clean, and no air gap, wafer displacement, or bonding void is generated.
[0103] Embodiment 4: This embodiment provides a wafer bonding method, and the same points as those in Embodiment 3 are not repeated here. The difference between this embodiment and Embodiment 3 is that: S113: Figure 1As shown, in a vacuum environment with a vacuum degree of 1E-3mbar-100mbar, a first pressure is applied to a side of the first wafer 1 away from the first bonding surface 11, and the first pressure is maintained for 1-30s. Then, the partition between the first wafer 1 and the second wafer 2 is removed, so that the first bonding surface 11 and the second bonding surface 12 are in contact with each other. After 5-30s, the pressure area 11 of the first pressure is bonded to the second wafer 2, and then a second pressure is applied to the side of the first wafer 1 away from the first bonding surface 11. At this time, the pressure area 12 of the second pressure is bonded to the second wafer 2, thereby achieving the bonding of the first wafer 1 and the second wafer 2, wherein the pressure range of the first pressure is 10-500N, the pressure range of the second pressure is 500-10000N, and the area of the pressure area 21 of the first pressure is 0.02-5cm 2 The area of the second pressure application area 22 is 18-350cm 2 ; The distance between the center of the pressure area of the first pressure and the center of the first wafer is 0-5cm, and the distance between the center of the pressure area of the second pressure and the center of the first wafer is 0-5cm.
[0104] In this embodiment, if Figure 5 As shown in the figure, the bonding interface after wafer bonding is clean, and no air gap, wafer displacement or bonding void is generated.
[0105] Embodiment 5: This embodiment provides a wafer bonding method, and the same points as those in Embodiment 3 are not repeated here. The difference between this embodiment and Embodiment 3 is that: S113: Figure 2 As shown, a first pressure is applied to a side of the first wafer 1 away from the first bonding surface 11, and the first pressure is maintained for 1-30s, then the partition between the first wafer 1 and the second wafer 2 is removed, so that the first bonding surface 11 and the second bonding surface 12 are in contact with each other, and after 5-25s, the pressure area 31 of the first pressure is bonded to the second wafer 2, and then a second pressure is applied to a side of the first wafer 1 away from the first bonding surface 11, and the second pressure is maintained for 10-30s, at this time, the pressure area 32 of the second pressure is bonded to the second wafer 2, and then a third pressure is applied to a side of the first wafer 1 away from the first bonding surface 11, thereby achieving the bonding of the first wafer 1 and the second wafer 2, wherein the pressure range of the first pressure is 10-500N, the pressure range of the second pressure is 200-2000N, the pressure range of the third pressure is 500-10000N, and the area of the pressure area 31 of the first pressure is 0.02-5cm 2 The area of the second pressure application area 32 is 3-180cm 2 The area of the third pressure application area 33 is 18-350cm 2The center of the pressure area of the first pressure is 0-5cm away from the center of the first wafer, the center of the pressure area of the second pressure is 0-5cm away from the center of the first wafer, and the center of the pressure area of the third pressure is 0-5cm away from the center of the first wafer.
[0106] In this embodiment, the bonding interface after wafer bonding is relatively clean, and no air gap, wafer displacement, or bonding void is generated.
[0107] Embodiment 6: This embodiment provides a wafer bonding method, and the same points as those in Embodiment 5 are not repeated here. The difference between this embodiment and Embodiment 5 is that: S113: Figure 2 As shown, in a vacuum environment with a vacuum degree of 1E-3mbar-100mbar, a first pressure is applied to a side of the first wafer 1 away from the first bonding surface 11, and the first pressure is maintained for 1-30s, and then the vacuum degree is reduced to 1E-4mbar-10mbar, and then the partition between the first wafer 1 and the second wafer 2 is removed, so that the first bonding surface 11 and the second bonding surface 12 are in contact with each other, and after 5-25s, the pressure area 31 of the first pressure is bonded to the second wafer 2, and then the first wafer 1 is away from the first bonding surface 11. A second pressure is applied to one side of the first bonding surface 11. After the second pressure lasts for 10-30s, the pressure area 32 of the second pressure is bonded to the second wafer 2. Then, a third pressure is applied to the side of the first wafer 1 away from the first bonding surface 11, thereby achieving the bonding of the first wafer 1 and the second wafer 2. The pressure range of the first pressure is 10-500N, the pressure range of the second pressure is 200-2000N, and the pressure range of the third pressure is 500-10000N. The area of the pressure area 31 of the first pressure is 0.02-5cm 2 The area of the second pressure application area 32 is 3-180cm 2 The area of the third pressure application area 33 is 18-350cm 2 The center of the pressure area of the first pressure is 0-5cm away from the center of the first wafer, the center of the pressure area of the second pressure is 0-5cm away from the center of the first wafer, and the center of the pressure area of the third pressure is 0-5cm away from the center of the first wafer.
[0108] In this embodiment, the bonding interface after wafer bonding is clean, and no air gap, wafer displacement, or bonding void is generated.
[0109] Comparative Example 1: This comparative example provides a wafer bonding method. The similarities with Example 1 are not repeated here. The difference from Example 1 is that there is no step S12. The specific process of step S13 is: in a vacuum environment with a vacuum degree of 1E-4mbar to 1000mbar, pressure is applied to the middle part of the side of the first wafer away from the first bonding surface, and the pressure range is 10N-10000N, thereby achieving bonding between the first wafer and the second wafer.
[0110] In this comparative example, Figure 6 As shown, an air gap is generated at the bonding interface after the two wafers are bonded, and the wafers are displaced.
[0111] Comparative Example 2: This comparative example provides a wafer bonding method. The similarities with Example 1 are not repeated here. The difference from Example 1 is that: S13: In a vacuum environment with a vacuum degree of 1E-4mbar to 1000mbar, the partition between the first wafer and the second wafer is removed so that the first bonding surface and the second bonding surface are in contact with each other and bonded.
[0112] In this comparative example, Figure 7 As shown, the wafers are displaced after the two wafers are bonded.
[0113] Through the above embodiments and comparative examples, we can see that in Embodiments 1-2, whether pressure is applied first and then the two wafers are brought into contact, or the two wafers are brought into contact first and then pressure is applied, the effects produced by the two are equivalent, the bonding interface after the wafers are bonded is clean, and no air gap, wafer displacement and bonding holes are generated. It can be obtained from Embodiments 3 and 4 that increasing the vacuum degree during the process of applying pressure to the two wafers can make the bonding interface after the wafers are bonded cleaner. The same is true for Embodiments 5 and 6. It can be obtained from Embodiment 1 and Comparative Example 1 that if no separation treatment is performed, an air gap will be generated at the bonding interface after the two wafers are bonded, and the wafers will be displaced. It can be obtained from Embodiment 1 and Comparative Example 2 that if no pressure treatment is performed, the wafers will be displaced after the two wafers are bonded.
[0114] The above description has fully disclosed the specific implementation methods of the present application. It should be pointed out that any changes made by technicians familiar with the field to the specific implementation methods of the present application do not deviate from the scope of the claims of the present application. Accordingly, the scope of the claims of the present application is not limited to the above specific implementation methods.
Claims
1. A wafer bonding method, It is characterized in that The method comprises: Providing a first wafer and a second wafer, wherein the first wafer has a first bonding surface, and the second wafer has a second bonding surface; Separating the first wafer and the second wafer, and arranging the first bonding surface and the second bonding surface relative to each other and aligning them; In a vacuum environment, the first wafer and the second wafer are brought close to each other and subjected to a bonding process. During the bonding process of the first wafer and the second wafer, pressure is applied to at least one of the first wafer and the second wafer so that the first bonding surface and the second bonding surface are aligned and bonded under the action of pressure.
2. The method according to claim 1, It is characterized in that In the process of applying pressure to at least one of the first wafer and the second wafer, the pressure application position is located in the middle of the first wafer and / or the second wafer being pressed.
3. The method according to claim 1, It is characterized in that The applying pressure to at least one of the first wafer and the second wafer includes: applying pressure in steps, during which the first bonding surface and / or the second bonding surface are pressurized in steps, and the pressure application area is different each time, so that the first bonding surface and the second bonding surface are bonded in steps under pressure, and the pressure application area refers to an effective pressure area extending circumferentially from the pressure application position.
4. The method according to claim 3, It is characterized in that In the step-by-step pressure application process, the pressure application area range of the latter pressure application is larger than the pressure application area range of the previous pressure application.
5. The method according to claim 3, It is characterized in that In the step-by-step pressure application process, the pressure applied to the pressure application area each time is not greater than 10000N, and the pressure applied to the pressure application area each time is not less than 10N.
6. The method according to claim 3, It is characterized in that In the step-by-step pressing process, the number of times of pressing in the step-by-step pressing is determined by the total area of the first bonding surface and / or the second bonding surface.
7. The method according to claim 3, It is characterized in that The step-by-step pressurization includes a first pressurization process and a second pressurization process, wherein the first pressurization process includes pressurization using a first pressure, and the second pressurization process includes pressurization using a second pressure, and the step-by-step pressurization process satisfies at least one of the following characteristics: The pressure range of the first pressure is 10-500N; The pressure range of the second pressure is 500-10000N; The area of the pressure region of the first pressure accounts for 0.001% to 25% of the total area of the first wafer; The area of the second pressure application region accounts for 25% to 100% of the total area of the first wafer; The pressure application area of the first pressure and the pressure application area of the second pressure both cover the center of the first wafer; The duration of applying the first pressure is ≤30s.
8. The method according to claim 3, It is characterized in that The step-by-step pressurization includes a first pressurization process, a second pressurization process and a third pressurization process. The first pressurization process includes pressurization using a first pressure, the second pressurization process includes pressurization using a second pressure, and the third pressurization process includes pressurization using a third pressure. The step-by-step pressurization process satisfies at least one of the following characteristics: The pressure range of the first pressure is 10-500N; The pressure range of the second pressure is 200-2000N; The pressure range of the third pressure is 500-10000N; The area of the pressure region applied by the first pressure accounts for 0.001% to 25% of the total area of the first wafer; The area of the pressure region applied by the second pressure accounts for 25% to 50% of the total area of the first wafer; The area of the pressure region applied by the third pressure accounts for 50% to 100% of the total area of the first wafer; The pressure application area of the first pressure, the pressure application area of the second pressure, and the pressure application area of the third pressure all cover the center of the first wafer; The duration of applying the first pressure and the duration of applying the second pressure are both ≤30s.
9. The method according to any one of claims 1 to 8, It is characterized in that The preparation method meets at least one of the following characteristics: Before bringing the first wafer and the second wafer closer to each other and performing a bonding process, the method further includes: Under a vacuum environment, applying pressure to at least one of the first wafer and the second wafer so that external pressure exists when the first wafer and the second wafer are in contact; Under the vacuum environment, bringing the first wafer and the second wafer close to each other and performing a bonding process comprises: In a vacuum environment, after the first wafer and the second wafer are brought close to and in contact with each other, during the process of applying pressure to at least one of the first wafer and the second wafer for bonding, the vacuum degree of the vacuum environment is reduced so that the first bonding surface and the second bonding surface are aligned and bonded under pressure.
10. The method according to claim 9, It is characterized in that The preparation method meets at least one of the following characteristics: When the first wafer and the second wafer are brought into contact, the vacuum degree in the vacuum environment is a first vacuum degree; after the first wafer and the second wafer are brought into close contact, the vacuum degree in the vacuum environment is a second vacuum degree; and the difference between the first vacuum degree and the second vacuum degree is in a range of 1E2 mbar to 1E3 mbar; During the contact and bonding process, the vacuum degree of the vacuum environment is gradually reduced based on the step-by-step pressure application process. The vacuum degree in the previous pressure application process is higher than the vacuum degree in the next pressure application process. The difference in vacuum degree between two adjacent pressure application processes ranges from 1E2mbar to 1E4mbar.
11. A method for preparing a functional substrate, It is characterized in that The preparation method at least comprises: the steps included in the wafer bonding method according to any one of claims 1 to 10, removing the non-functional layer from the structure obtained by the wafer bonding method to obtain a functional substrate.