High-binding-force copper bump structure and preparation method thereof
By etching grooves on bare silicon in semiconductor packaging, forming TSV through holes, depositing insulating layers and electroplating bumps, and etching protective structures around bumps, the insufficient bump binding force in the prior art is solved. The problem of this achieves higher binding force and process simplification, reducing costs.
Patent Information
- Application Number
- CN202410993692.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-24
AI Technical Summary
In the prior art, when preparing small-size copper column bumps, the photoresist material has insufficient resolution and poor uniformity of the bumps after electroplating, resulting in a small bonding force between the bumps and the substrate, affecting its reliability.
The etching and grooves on the front of the bare silicon, TSV through-hole plating, RDL rewiring layer production, glass bonding, photoresist pattern thinning, silicon etching to form pits, deposit insulating layer and electroplating to form convex points in the groove, and By etching to expose the back of the chip and attaching a heat sink, the lithography and CMP grinding steps are reduced, and the bonding force between the bumps and the substrate is improved.
Improve the uniformity and bonding of bumps, simplify the process flow, reduce packaging costs, and enhance the reliability of bumps.
Smart Images

Figure CN118919428A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of semiconductor packaging, and in particular relates to a high-binding force copper bump structure and a preparation method thereof. Background Art
[0002] Due to the increasing requirements of electronic devices for high performance, small size and multi-function, three-dimensional chip stacking technology has received increasing attention in recent years. In order to achieve the multi-function requirements of the next generation of electronic products, interconnections with high I / O and fine pitch are required. Therefore, through silicon via fine pitch interconnections for three-dimensional integration of semiconductor chips have been widely developed. High-density bump preparation is a key technology to achieve good interconnection in 3D integration, which requires physically stacking a chip or wafer onto another chip or wafer while forming a permanent electrical and mechanical connection between the I / O pins of the device. Copper pillar bumps with a Cu / Ni / SnAg structure are currently the most widely used small pitch interconnect bump solution.
[0003] The common bump preparation process usually uses photoresist exposure to form bump openings, and then forms the bump structure through electroplating. For small-size bump technology, the selection of photoresist materials is extremely important. On the one hand, the resolution of the photoresist needs to meet the bump exposure requirements; on the other hand, the bump morphology uniformity after electroplating etching is poor, and the large undercut of the bottom seed layer will result in a small bonding force between the bump and the substrate. Therefore, exploring new processes to prepare high-bonding bumps to improve bump reliability has become a focus of attention in the industry. Summary of the invention
[0004] In order to achieve the above purpose and the above technical effect, the technical solution adopted by the present invention is:
[0005] A method for preparing a high-bonding copper bump structure comprises the following steps:
[0006] Step 1: Etch and dig grooves on the front side of the bare silicon, and then bury the corresponding chip in the grooves;
[0007] Step 2: Etching and electroplating TSV through holes on the front side of bare silicon;
[0008] Step 3: Fabricate the RDL redistribution layer on the TSV through hole;
[0009] Step 4: Bonding the semi-finished product obtained in step 3 to glass;
[0010] Step 5: thinning the back side of the bare silicon and preparing a photoresist pattern to expose a photoresist opening;
[0011] Step 6: Perform silicon etching at the photoresist opening to form a pit to expose the bottom of the front TSV through hole;
[0012] Step 7: deposit an insulating layer at the etched pits, then electroplate or fill a conductive polymer to form a convex point in the groove, and then remove the photoresist pattern on the surface;
[0013] Step 8: Remove the glass and etch the silicon on both sides of the bumps in the groove to expose the bumps in the groove and the back of the chip, and attach a heat sink to the back of the chip.
[0014] Furthermore, in step 1, the shape of the groove is rectangular, circular or trapezoidal, and the type of chip 2 is a logic chip, a memory chip or a system-on-chip (SoC).
[0015] Furthermore, in step five, the thickness of the photoresist pattern is 10-20 microns.
[0016] Furthermore, in step six, the pit is a deep straight hole with a diameter of 10-40 microns, and the etching depth is 20-40 microns.
[0017] Furthermore, in step seven, the insulating layer is made of oxide or nitride and has a thickness of 0.5-2 microns.
[0018] Furthermore, in step seven, the height of the protrusions in the grooves is 20-60 microns.
[0019] Furthermore, in step eight, 15-55 microns of the bumps are exposed in the grooves, and 3-5 microns of silicon are left at the bottom as a bump protection structure to increase the bonding strength and reliability of the bumps and the substrate.
[0020] Furthermore, in step eight, the thickness of the heat sink is 20-50 microns.
[0021] The invention also discloses a method for preparing a high-binding-force copper bump structure and a high-binding-force copper bump structure prepared therefrom.
[0022] Furthermore, the high-bonding strength copper bump structure includes bare silicon and a chip, wherein a TSV through-hole is etched and electroplated on the front side of the bare silicon, an RDL redistribution layer is formed on the TSV through-hole, a pit corresponding to the position of the TSV through-hole is etched on the back side of the bare silicon, an insulating layer is deposited in the pit and a bump in the groove is formed by electroplating or filling with a conductive polymer, the silicon around the bump in the groove is etched away, the height of the bump in the groove is greater than the height of the bare silicon, the chip is mounted in the groove of the bare silicon, and a heat sink is arranged on the back side of the chip.
[0023] Compared with the prior art, the present invention has the following beneficial effects:
[0024] The invention discloses a high-bonding force copper bump structure and a preparation method thereof, which can improve the uniformity of the bump and enhance the bonding force between the bump and a substrate, reduce one step of photolithography and CMP grinding steps compared with traditional bump preparation, simplify the process flow and reduce packaging costs. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 It is a structural schematic diagram of step 1 of the present invention;
[0026] Figure 2 It is a structural schematic diagram of step 2 of the present invention;
[0027] Figure 3 It is a structural schematic diagram of step three of the present invention;
[0028] Figure 4 It is a structural schematic diagram of step 4 of the present invention;
[0029] Figure 5 It is a structural schematic diagram of step five of the present invention;
[0030] Figure 6 It is a structural schematic diagram of step six of the present invention;
[0031] Figure 7 It is a structural schematic diagram of step seven of the present invention;
[0032] Figure 8 It is a structural schematic diagram of step eight of the present invention. DETAILED DESCRIPTION
[0033] The present invention is described in detail below so that the advantages and features of the present invention can be more easily understood by those skilled in the art, thereby making a clearer and more definite definition of the protection scope of the present invention.
[0034] A brief summary of one or more aspects is given below to provide a basic understanding of these aspects. This summary is not an exhaustive overview of all conceived aspects, and is neither intended to identify the key or critical elements of all aspects nor to define the scope of any or all aspects. Its only purpose is to give some concepts of one or more aspects in a simplified form as a prelude to a more detailed description that will be given later.
[0035] like Figure 1-8 As shown, the present invention discloses a method for preparing a high-bonding force copper bump structure, comprising the following steps:
[0036] Step 1: If Figure 1 As shown, silicon etching is performed on the front side of the bare silicon 1 to dig a groove, the shape of which can be rectangular, circular, trapezoidal, etc., and then a matching chip 2 is buried in the groove, and the type of the chip 2 is a logic chip, a memory chip, or a system chip SoC, etc.;
[0037] Step 2: If Figure 2 As shown, etching and electroplating of TSV through hole 3 are performed on the front side of bare silicon 1, and the electroplating material is copper or other metal;
[0038] Step 3: If Figure 3 As shown, the RDL redistribution layer 4 is fabricated on the TSV through hole 3;
[0039] Step 4: If Figure 4 As shown, the semi-finished product obtained in step 3 is temporarily bonded to the glass 5;
[0040] Step 5: If Figure 5 As shown, wafer thinning and stress relief thinning are performed on the back of the bare silicon 1, and a layer of photoresist pattern 6 is prepared with a thickness of 10-20 microns to expose the photoresist opening;
[0041] Step 6: If Figure 6 As shown, silicon etching is performed at the photoresist opening to form a well-uniform pit, and the bottom of the front TSV through hole 3 is exposed; the pit is preferably a deep straight hole with a diameter of 10-40 microns, and the etching depth is 20-40 microns;
[0042] Step 7: If Figure 7 As shown, an insulating layer is deposited at the pit after etching. The insulating layer can be made of oxide, nitride, etc., with a thickness of 0.5-2 microns, and then electroplated or filled with a conductive polymer to form a convex point 7 in the groove with a height of 20-60 microns, and then the surface photoresist pattern 6 is removed;
[0043] Step 8: If Figure 8 As shown, the glass 5 is removed, and the silicon on both sides of the bump 7 in the groove is etched, and the bump 7 in the groove is exposed by 15-55 microns, but a certain height (3-5 microns) of silicon is left at the bottom as a bump protection structure to increase the bonding force and reliability between the bump and the substrate. At the same time, the back of the embedded chip 2 is exposed, and a heat sink 8 with a thickness of 20-50 microns is attached. The heat sink 8 can be metal, ceramic or other heat dissipation materials.
[0044] The structure of the bump 7 in the groove obtained by the above-mentioned preparation method disclosed in the present invention can maintain good side wall uniformity, omit the etching seed layer after electroplating, reduce undercut, and form a protective layer through the bare silicon 1 to protect the bump 7 in the groove, thereby increasing the bonding force at the bottom of the bump 7 in the groove. Compared with the traditional bump preparation, the present invention reduces one step of photolithography and CMP grinding steps, simplifies the process flow, reduces the packaging cost, and has a relatively simpler process.
[0045] The present invention also discloses a high-bonding force copper bump structure, comprising bare silicon 1 and a chip 2, wherein a TSV through hole 3 is etched and electroplated on the front side of the bare silicon 1, an RDL redistribution layer 4 is formed on the TSV through hole 3, a pit corresponding to the position of the TSV through hole 3 is etched on the back side of the bare silicon 1, an insulating layer is deposited in the pit and a groove bump 7 is formed by electroplating or filling a conductive polymer, the silicon around the groove bump 7 is etched away, the height of the groove bump 7 is greater than the height of the bare silicon 1, the chip 2 is mounted in the groove of the bare silicon 1, and a heat sink 8 is arranged on the back side of the chip 2.
[0046] Example 1
[0047] like Figure 1-8 As shown, a method for preparing a high-bonding copper bump structure comprises the following steps:
[0048] Step 1: If Figure 1 As shown, silicon etching is performed on the front side of the bare silicon 1 to dig a groove, the shape of the groove is rectangular, and then a matching chip 2 is buried in the groove, and the type of chip 2 is a logic chip;
[0049] Step 2: If Figure 2 As shown, etching and electroplating of TSV through hole 3 are performed on the front side of bare silicon 1, and copper is used as the electroplating material;
[0050] Step 3: If Figure 3 As shown, the RDL redistribution layer 4 is fabricated on the TSV through hole 3;
[0051] Step 4: If Figure 4 As shown, the semi-finished product obtained in step 3 is temporarily bonded to the glass 5;
[0052] Step 5: If Figure 5 As shown, wafer thinning and stress relief thinning are performed on the back of the bare silicon 1, and a layer of photoresist pattern 6 is prepared with a thickness of 10 microns to expose the photoresist opening;
[0053] Step 6: If Figure 6 As shown, silicon etching is performed at the photoresist opening to form a well-uniform pit, and the bottom of the front TSV through hole 3 is exposed; the pit is a deep straight hole with a diameter of 10 microns, and the etching depth is 30 microns;
[0054] Step 7: If Figure 7 As shown, an insulating layer is deposited at the pit after etching, the insulating layer is made of nitride with a thickness of 1 micron, and then electroplated or filled with a conductive polymer to form a convex point 7 in the groove with a height of 20 microns, and then the photoresist pattern 6 on the surface is removed;
[0055] Step 8: If Figure 8 As shown, the glass 5 is removed, and the silicon on both sides of the bump 7 in the groove is etched, and the bump 7 in the groove is exposed by 15 microns, but 3 microns of silicon are left at the bottom as a bump protection structure to increase the bonding strength and reliability between the bump and the substrate. At the same time, the back of the embedded chip 2 is exposed, and a heat sink 8 with a thickness of 20 microns is attached. The heat sink 8 is made of ceramic.
[0056] The structure of the bump 7 in the groove obtained by the above preparation method disclosed in this embodiment can maintain good side wall uniformity, omit the etching seed layer after electroplating, reduce undercut, and form a protective layer through the bare silicon 1 to protect the bump 7 in the groove, thereby increasing the bonding force at the bottom of the bump 7 in the groove. Compared with the traditional bump preparation, the present invention reduces one step of photolithography and CMP grinding steps, simplifies the process flow, reduces the packaging cost, and has a relatively simpler process.
[0057] A high-bonding copper bump structure comprises a bare silicon 1 and a chip 2, wherein a TSV through hole 3 is etched and electroplated on the front side of the bare silicon 1, an RDL redistribution layer 4 is formed on the TSV through hole 3, a pit corresponding to the position of the TSV through hole 3 is etched on the back side of the bare silicon 1, an insulating layer is deposited in the pit and a groove bump 7 is formed by electroplating or filling with a conductive polymer, the silicon around the groove bump 7 is etched away, the height of the groove bump 7 is greater than the height of the bare silicon 1, the chip 2 is mounted in the groove of the bare silicon 1, and a heat sink 8 is arranged on the back side of the chip 2.
[0058] Parts or structures not specifically described in the present invention may adopt existing technologies or existing products and will not be described in detail here.
[0059] The above descriptions are merely embodiments of the present invention and are not intended to limit the patent scope of the present invention. Any equivalent structure or equivalent process transformation made using the contents of the present invention specification, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present invention.
Claims
1. A method for preparing a high-bonding copper bump structure, It is characterized in that The following steps are involved: Step 1: Etch and dig grooves on the front side of the bare silicon, and then bury the corresponding chip in the grooves; Step 2: Etching and electroplating TSV through holes on the front side of bare silicon; Step 3: Fabricate the RDL redistribution layer on the TSV through hole; Step 4: Bonding the semi-finished product obtained in step 3 to glass; Step 5: thinning the back side of the bare silicon and preparing a photoresist pattern to expose a photoresist opening; Step 6: Perform silicon etching at the photoresist opening to form a pit to expose the bottom of the front TSV through hole; Step 7: deposit an insulating layer at the etched pits, then electroplate or fill a conductive polymer to form a convex point in the groove, and then remove the photoresist pattern on the surface; Step 8: Remove the glass and etch the silicon on both sides of the bumps in the groove to expose the bumps in the groove and the back of the chip, and attach a heat sink to the back of the chip.
2. A method for preparing a high-bonding copper bump structure according to claim 1, It is characterized in that In step 1, the shape of the groove is rectangular, circular or trapezoidal, and the type of chip 2 is a logic chip, a memory chip or a system-on-chip (SoC).
3. A method for preparing a high-bonding copper bump structure according to claim 1, It is characterized in that In step five, the thickness of the photoresist pattern is 10-20 microns.
4. A method for preparing a high-bonding copper bump structure according to claim 1, It is characterized in that In step six, the pit is a deep straight hole with a diameter of 10-40 microns, and the etching depth is 20-40 microns.
5. A method for preparing a high-bonding copper bump structure according to claim 1, It is characterized in that In step seven, the insulating layer is made of oxide or nitride and has a thickness of 0.5-2 microns.
6. A method for preparing a high-bonding copper bump structure according to claim 1, It is characterized in that In step seven, the height of the protrusion in the groove is 20-60 microns.
7. A method for preparing a high-bonding copper bump structure according to claim 1, It is characterized in that In step eight, 15-55 microns of the bumps are exposed in the grooves, and 3-5 microns of silicon are left at the bottom as a bump protection structure to increase the bonding strength and reliability of the bumps and the substrate.
8. A method for preparing a high-bonding copper bump structure according to claim 1, It is characterized in that In step eight, the thickness of the heat sink is 20-50 microns.
9. A high-bonding force copper bump structure prepared according to the method for preparing a high-bonding force copper bump structure according to any one of claims 1 to 8.
10. A high bonding strength copper bump structure according to claim 9, It is characterized in that It includes bare silicon and a chip. A TSV through-hole is etched and electroplated on the front side of the bare silicon, an RDL redistribution layer is formed on the TSV through-hole, a pit corresponding to the position of the TSV through-hole is etched on the back side of the bare silicon, an insulating layer is deposited in the pit and a convex point in the groove is formed by electroplating or filling with a conductive polymer, the silicon around the convex point in the groove is etched away, the height of the convex point in the groove is greater than the height of the bare silicon, the chip is mounted in the groove of the bare silicon, and a heat sink is arranged on the back side of the chip.
Citation Information
Patent Citations
A method for fabricating a through-silicon via interconnect structure
CN102270603A
Low-cost and high-reliability chip size CIS packaging structure
CN104465581A
Chip embedded silicon substrate type fan-out type packaging structure and manufacturing method therefor
CN106876356A
Silicon-based three-dimensional fan-out integrated packaging method and silicon-based three-dimensional fan-out integrated packaging structure
CN111463137A
Metal wiring layer structure capable of improving binding force and preparation method
CN114464597A