Silicon wafer surface metal collection method and detection method
By using a low-concentration etching solution on the surface of the silicon wafer to remove the oxide film and adjust the scanning solution to dissolve precious metals, the problem of the inability to detect precious metals in the existing technology is solved, and efficient and accurate detection of precious metals on the surface of the silicon wafer is achieved.
Patent Information
- Application Number
- CN202411012982.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-08
AI Technical Summary
The existing metal detection methods for surface metals of silicon wafers cannot effectively detect precious metals (such as Ag and Au), because the scanning solution of HF+H2O2 cannot dissolve precious metals, resulting in the inability to perform accurate detection.
The silicon wafer is covered with an etching solution with a mass percentage concentration below the preset threshold, and the oxide film is removed, and the scanning solution is adjusted to a mixed acid solution of HF acid solution, HNO3 acid solution and HCl acid solution, so as to enhance the etching ability to dissolve precious metals, thus realizing the detection of precious metals on the surface of silicon wafers.
By diluting the concentration of the scanning solution, the damage to the inductively coupled plasma mass spectrometer is avoided, and the detection accuracy and accuracy of precious metals are improved. It can effectively detect precious metals on the surface of silicon wafers, meeting the lower detection limit of method.
Smart Images

Figure CN118919443A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of semiconductor manufacturing technology, and in particular to a method for collecting and detecting metal on a silicon wafer surface. Background Art
[0002] During the processing of silicon wafers (wafers), various metal impurities will be contaminated, which will lead to the failure of subsequent devices. For example, light metals (Na, Mg, Al, K, Ca, etc.) will reduce the breakdown voltage of the device, and heavy metals (Cr, Mn, Fe, Ni, Cu, Zn, etc.) will reduce the life of the device. Therefore, as the raw material of the device, the metal content on the surface of the silicon wafer will directly affect the qualified rate of the device. Therefore, it is very important to analyze the metal elements on the surface of the silicon wafer.
[0003] The current method for detecting metal on the surface of silicon wafers is to use HF spray to etch the oxide film on the surface of the silicon wafer, and then use a scanning solution of HF+H2O2 to collect the metal on the surface of the silicon wafer. However, for the detection of precious metals (Ag, Au) on the surface of silicon wafers, the scanning solution of HF+H2O2 cannot dissolve precious metals, so it is impossible to detect precious metals on the surface of silicon wafers. Summary of the invention
[0004] In order to solve the above technical problems, the present invention provides a method for collecting and detecting metal on the surface of a silicon wafer, which can realize the detection of metal on the surface of a silicon wafer.
[0005] In order to achieve the above object, the technical solution adopted by the embodiment of the present invention is:
[0006] A method for collecting metal on a silicon wafer surface, comprising:
[0007] Covering the silicon wafer to be processed with an etching solution having a mass percentage concentration lower than a preset threshold value to remove an oxide film on the surface of the silicon wafer;
[0008] Controlling the scanning solution to run along a target path on the surface of the silicon wafer to complete the collection of metal on the surface of the silicon wafer;
[0009] Wherein, the scanning solution is a mixed acid solution of HF acid solution and other acid solution, and the other acid solution is at least one of HNO3 acid solution, HCl acid solution and H2O2 acid solution.
[0010] In some embodiments, the etching solution is a HF solution.
[0011] In some embodiments, the mass percentage concentration of the etching solution is 0.5%-1%, and the volume is 1.3-1.5 ml.
[0012] In some embodiments, the scanning speed of the scanning solution is 5 ml / min-6 ml / min, and the volume of the scanning solution is 1.3-1.5 ml.
[0013] In some embodiments, the scanning solution is a mixed acid solution of HF acid solution, HNO3 acid solution and HCl acid solution.
[0014] In some embodiments, in the scanning solution, the mass percentage concentration of the HF acid solution is 0.5%-1%.
[0015] In some embodiments, in the scanning solution, the mass percentage concentration of the HNO3 acid solution is 33%-35%.
[0016] In some embodiments, in the scanning solution, the mass percentage concentration of the HCl acid solution is 2%-3%.
[0017] In some embodiments, the size of the silicon wafer is 8 inches or 12 inches, the thickness of the silicon wafer is 700-800 microns, and the surface of the silicon wafer is hydrophobic.
[0018] The embodiment of the present invention further provides a method for detecting metal on the surface of a silicon wafer, comprising:
[0019] Obtaining a liquid to be analyzed, wherein the liquid to be analyzed is obtained by the above-mentioned collection method;
[0020] The liquid to be analyzed is introduced into an inductively coupled plasma mass spectrometer for elemental analysis.
[0021] The beneficial effects of the present invention are:
[0022] In this embodiment, the silicon wafer to be processed is covered with an etching solution having a mass percentage concentration lower than a preset threshold value to remove the oxide film on the surface of the silicon wafer. Compared with etching the oxide film on the surface of the silicon wafer by using a high concentration HF spray, the etching solution having a mass percentage concentration lower than the preset threshold value helps to reduce the concentration of the scanning solution in the subsequent process, and can dilute the scanning solution to avoid damage to the inductively coupled plasma mass spectrometer when the scanning solution is passed into the inductively coupled plasma mass spectrometer. In addition, in this embodiment, by adjusting the formula of the scanning solution, the scanning solution can be adjusted to a mixed acid solution of HF acid solution, HNO3 acid solution and HCl acid solution, so that the scanning solution can dissolve the precious metal, thereby detecting the precious metal on the surface of the silicon wafer; when the mixed acid solution of HF acid solution, HNO3 acid solution and HCl acid solution is used to detect the precious metal on the surface of the silicon wafer, the scanning solution has a strong etching ability, and the etching solution having a mass percentage concentration lower than the preset threshold value can be used to dilute the scanning solution to avoid damage to the inductively coupled plasma mass spectrometer when the scanning solution is passed into the inductively coupled plasma mass spectrometer. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 A schematic diagram showing a method for collecting metal on a silicon wafer surface according to an embodiment of the present invention;
[0024] Figure 2 A schematic diagram showing the verification of spike recovery rate using standard solutions of different concentrations in an embodiment of the present invention;
[0025] Figure 3 A schematic diagram showing the detection limit of the method according to an embodiment of the present invention.
[0026] Reference numerals
[0027] 1 Oxide film
[0028] 2 Silicon wafer
[0029] 3 Etching solution
[0030] 4 Scanning Solution DETAILED DESCRIPTION
[0031] In order to make the purpose, technical solution and advantages of the embodiment of the present invention clearer, the technical solution of the embodiment of the present invention will be clearly and completely described below in conjunction with the drawings of the embodiment of the present invention. Obviously, the described embodiment is a part of the embodiment of the present invention, not all of the embodiments. Based on the described embodiment of the present invention, all other embodiments obtained by ordinary technicians in this field belong to the scope of protection of the present invention.
[0032] Currently, metal collection on the surface of silicon wafers is performed by using a nozzle in a metal collection device to absorb a scanning solution to collect metal on the surface of the silicon wafer, and the metal content in the scanning solution is detected by an inductively coupled plasma mass spectrometer (ICP-MS).
[0033] The present invention provides a method for collecting and detecting metal on the surface of a silicon wafer, which can realize the detection of metal on the surface of a silicon wafer.
[0034] The embodiment of the present invention provides a method for collecting metal on the surface of a silicon wafer, comprising:
[0035] Covering the silicon wafer to be processed with an etching solution having a mass percentage concentration lower than a preset threshold value to remove an oxide film on the surface of the silicon wafer;
[0036] Controlling the scanning solution to run along a target path on the surface of the silicon wafer to complete the collection of metal on the surface of the silicon wafer;
[0037] Wherein, the scanning solution is a mixed acid solution of HF acid solution and other acid solution, and the other acid solution is at least one of HNO3 acid solution, HCl acid solution and H2O2 acid solution.
[0038] In this embodiment, the silicon wafer to be processed is covered with an etching solution having a mass percentage concentration lower than a preset threshold value to remove the oxide film on the surface of the silicon wafer. Compared with etching the oxide film on the surface of the silicon wafer by using a high concentration HF spray, the etching solution having a mass percentage concentration lower than the preset threshold value helps to reduce the concentration of the scanning solution in the subsequent process, and can dilute the scanning solution to avoid damage to the inductively coupled plasma mass spectrometer when the scanning solution is passed into the inductively coupled plasma mass spectrometer. In addition, in this embodiment, by adjusting the formula of the scanning solution, the scanning solution can be adjusted to a mixed acid solution of HF acid solution, HNO3 acid solution and HCl acid solution, so that the scanning solution can dissolve the precious metal, thereby detecting the precious metal on the surface of the silicon wafer; when the mixed acid solution of HF acid solution, HNO3 acid solution and HCl acid solution is used to detect the precious metal on the surface of the silicon wafer, the scanning solution has a strong etching ability, and the etching solution having a mass percentage concentration lower than the preset threshold value can be used to dilute the scanning solution to avoid damage to the inductively coupled plasma mass spectrometer when the scanning solution is passed into the inductively coupled plasma mass spectrometer.
[0039] The value of the above-mentioned preset threshold can be adjusted according to actual needs. In some embodiments, the value of the preset threshold can be 1%. When the mass percentage concentration of the etching solution is lower than 1%, the etching solution can effectively dilute the scanning solution to prevent the scanning solution from damaging the inductively coupled plasma mass spectrometer.
[0040] In some embodiments, the etching solution may be an HF solution, which can effectively remove the oxide film on the surface of the silicon wafer.
[0041] In some embodiments, the mass percentage concentration of the etching solution can be 0.5%-1%, and the volume is 1.3-1.5 ml. For example, the mass percentage concentration of the etching solution can be 0.5%, 0.6%, 0.7%, 0.8%, 0.9% or 1%, and the volume can be 1.3 ml, 1.35 ml, 1.4 ml, 1.45 ml or 1.5 ml. When the etching solution adopts the above mass percentage concentration and volume, on the one hand, it can ensure that the etching solution completely covers the surface of the silicon wafer and effectively removes the oxide film on the surface of the silicon wafer; on the other hand, the etching solution can effectively dilute the scanning solution to avoid the scanning solution from damaging the inductively coupled plasma mass spectrometer.
[0042] In this embodiment, the formula of the scanning solution can be determined according to the metals to be collected. When it is necessary to collect common light metals (Na, Mg, Al, K, Ca, etc.) and heavy metals (Cr, Mn, Fe, Ni, Cu, Zn, etc.), the scanning solution can be a mixed acid solution of HF acid and H2O2 acid; when it is necessary to collect precious metals (Ag, Au), the scanning solution can be a mixed acid solution of HF acid, HNO3 acid and HCl acid.
[0043] In some embodiments, the scanning speed of the scanning solution may be 5ml / min-6ml / min, and the volume of the scanning solution may be 1.3-1.5ml. For example, the scanning speed of the scanning solution may be 5ml / min, 5.1ml / min, 5.2ml / min, 5.3ml / min, 5.4ml / min, 5.5ml / min, 5.6ml / min, 5.7ml / min, 5.8ml / min, 5.9ml / min or 6ml / min; the volume of the scanning solution may be 1.3ml, 1.35ml, 1.4ml, 1.45ml or 1.5ml. When the scanning solution adopts the above scanning speed and volume, it can be ensured that the scanning solution can fully collect the metal on the surface of the silicon wafer.
[0044] When it is necessary to collect the precious metals (Ag, Au) on the surface of the silicon wafer, the scanning solution can be a mixed acid solution of HF acid solution, HNO3 acid solution and HCl acid solution. In the scanning solution, the mass percentage concentration of the HF acid solution can be 0.5%-1%, such as 0.5%, 0.6%, 0.7%, 0.8%, 0.9% or 1%. The mass percentage concentration of the HNO3 acid solution is 33%-35%, such as 33%, 33.5%, 34%, 34.5% or 35%. The mass percentage concentration of the HCl acid solution is 2%-3%, such as 2%, 2.5%, or 3%. When the scanning solution adopts the above formula, the precious metals on the surface of the silicon wafer can be fully dissolved, thereby improving the detection accuracy of the precious metals on the surface of the silicon wafer.
[0045] The size of the silicon wafer with unknown metal content is 8 inches or 12 inches, the thickness of the silicon wafer is 700-800 microns, and the surface of the silicon wafer is hydrophobic. The collection method of the present invention is applicable to silicon wafers of these specifications. Only when the silicon wafer surface is in a hydrophobic state will the scanning solution not spread on the silicon wafer surface.
[0046] The embodiment of the present invention further provides a method for detecting metal on the surface of a silicon wafer, comprising:
[0047] Obtaining a liquid to be analyzed, wherein the liquid to be analyzed is obtained by the above-mentioned collection method;
[0048] The liquid to be analyzed is introduced into an inductively coupled plasma mass spectrometer for elemental analysis.
[0049] In this embodiment, the liquid to be analyzed is a scanning solution diluted with an etching solution, which can avoid damage to the inductively coupled plasma mass spectrometer when the scanning solution is passed into the inductively coupled plasma mass spectrometer. When it is necessary to collect precious metals on the surface of the silicon wafer, the scanning solution can be adjusted to a mixed acid solution of HF acid solution, HNO3 acid solution and HCl acid solution, so that the scanning solution can dissolve the precious metals, thereby enabling the detection of precious metals on the surface of the silicon wafer; when the mixed acid solution of HF acid solution, HNO3 acid solution and HCl acid solution is used to detect the precious metals on the surface of the silicon wafer, the scanning solution has a strong etching ability, and the etching solution with a mass percentage concentration lower than the preset threshold can be used to dilute the scanning solution, thereby avoiding damage to the inductively coupled plasma mass spectrometer when the scanning solution is passed into the inductively coupled plasma mass spectrometer.
[0050] Figure 1 The schematic diagram of the method for collecting precious metals on the surface of a silicon wafer according to an embodiment of the present invention mainly comprises the following steps:
[0051] Step 1, removing the oxide film 1 on the surface of the silicon wafer 2;
[0052] Specifically, the oxide film 1 is a SiO2 film. Since SiO2 film is generated on the surface of silicon wafers in the natural environment, the SiO2 film on the surface of the silicon wafer needs to be removed before metal collection. The traditional method of etching the SiO2 film on the surface of the silicon wafer is to atomize HF with a high mass percentage concentration (greater than 38%) into gas and spray it onto the surface of the silicon wafer for etching (HF+SiO2→H2SiF6+H2O). The present invention uses an etching solution 3 (HF solution with a mass percentage concentration of 0.5%, a volume of 1.3 ml) to evenly cover the surface of the silicon wafer with the SiO2 film to etch the SiO2 film on the surface of the silicon wafer.
[0053] Step 2, using a scanning solution 4 with a formula of 0.5% HF + 3% HCl + 35% HNO3 to scan the surface of the silicon wafer, with a scanning speed of 5 ml / min and a scanning liquid volume of 1.3 ml, to collect the precious metals on the surface of the silicon wafer;
[0054] Step 3: Detect the metal content of the scanning solution by inductively coupled plasma mass spectrometry. In order to avoid interference and ensure the accuracy of the detection results, ICP-MS can use a quartz injection system.
[0055] In order to collect the precious metals on the surface of the silicon wafer and reduce the corrosion of the concentrated acid to the ICP-MS, the present embodiment firstly uses 0.5% HF to treat the surface of the silicon wafer to remove the oxide film on the surface of the silicon wafer, then uses a scanning solution of 0.5% HF+3% HCl+35% HNO3 to collect the precious metals on the surface of the silicon wafer, and finally combines the two solutions to enter the ICP-MS detection, that is, the concentration of the solution detected by ICP-MS is 0.5% HF+1.62% HCl+18.67% HNO3 (volume is 2.6ml), that is, in the solution detected by ICP-MS, the mass percentage concentration of HF is 0.5%, the mass percentage concentration of HCl is 1.62%, and the mass percentage concentration of HNO3 is 18.67%. Among them, the role of the 0.5% HF etching solution includes diluting the scanning solution and etching the SiO2 film on the surface of the silicon wafer.
[0056] The technical solution of this embodiment can be verified by adding 50ppt, 100ppt and 200ppt of standard solution (containing Au and Ag) to the surface of a clean silicon wafer. Figure 1 The test was carried out according to the process shown in the figure. After testing, the spiked recovery rate was between 75% and 125%.
[0057] Among them, the spiked recovery rate includes two types: absolute recovery rate and relative recovery rate, absolute recovery rate = a / spike concentration, relative recovery rate = a / (a+b+c), wherein a is the result obtained by detecting the solution recovered for the first time using an inductively coupled plasma mass spectrometer, b is the result obtained by detecting the solution recovered for the second time using an inductively coupled plasma mass spectrometer, and c is the result obtained by detecting the solution recovered for the third time using an inductively coupled plasma mass spectrometer.
[0058] Figure 2 A schematic diagram showing the verification of the spiked recovery rate using standard solutions of different concentrations in an embodiment of the present invention. After testing, the relative recovery rate of Ag collected using the technical solution of this embodiment is greater than 80%, and the absolute recovery rate is greater than 80%; the relative recovery rate of Au collected using the technical solution of this embodiment is greater than 60%, and the absolute recovery rate is greater than 75%, which can meet the requirements for collecting precious metals on the surface of silicon wafers.
[0059] The method detection limit of the technical solution of this embodiment is verified by using a clean silicon wafer according to Figure 1 The process shown is to perform the test for 5 days, test 10 sets of data every day, and calculate 3*SD (3 times the standard deviation). Figure 3 The detection limit of the method is Ag = 2.57E+06atom / cm 2 (0.110ppt), Au=5.51E+06atom / cm 2(0.435ppt). The method detection limit refers to the lowest concentration of the substance being measured that can be distinguished from the blank sample with 99% confidence after the entire processing and measurement process of a certain analytical method (including sample preparation and sample measurement).
[0060] In the related art, the oxide film on the surface of the silicon wafer is etched by HF spray, and then the metal on the surface of the silicon wafer is collected by a scanning solution. The collected solution is diluted by adding an alkaline solution and the pH value is controlled to obtain a solution to be analyzed, and then the solution to be analyzed is passed into an inductively coupled plasma mass spectrometer for elemental analysis. Among them, the purpose of adding an alkaline solution to the collected solution is to reduce the corrosion caused by the collected solution to the inductively coupled plasma mass spectrometer. The detection process is cumbersome and the detection time is long. The alkaline solution itself contains a small amount of metal, and the operation process of adding the alkaline solution will also bring metal contamination, affecting the accuracy of the detection results of the collected solution. In addition, the above method cannot achieve a lower method detection limit when detecting precious metals on the surface of the silicon wafer.
[0061] In this embodiment, the surface of the silicon wafer is treated by covering the surface of the silicon wafer with a 0.5% HF solution by mass percentage, and the precious metals on the surface of the silicon wafer are collected by scanning the solution, and the collected solution is passed into an inductively coupled plasma mass spectrometer for elemental analysis. The detection process is simple, the detection time is short, and there is no need to add other solutions to introduce pollution. The 0.5% HF solution is used to treat the surface of the silicon wafer on the one hand, and the collected solution is diluted on the other hand, which can reduce ICP-MS corrosion. The recovery rate verification results meet the requirements, and the lower method detection limit (Ag = 2.57E+06atom / cm 2 , Au=5.51E+06atom / cm 2 ) can detect silicon wafers with low precious metal concentrations with high detection accuracy.
[0062] When the mass percentage concentration range of the etching solution is 0.5%-1%, and the mass percentage concentration range of the scanning solution is (0.5%-1%) HF+3%HCl+35%HNO3, according to Figure 1 The detection steps are shown in the figure. The detection limit of the method is 1.00E+07atom / cm for Ag and Au. 2 The following can detect silicon wafers with lower precious metal concentrations with higher detection accuracy.
[0063] An embodiment of the present invention also provides a device for collecting metal from the surface of a silicon wafer, the device comprising a processor, a memory, and a computer program stored in the memory and running on the processor, and the processor implements the steps of the method for collecting metal from the surface of a silicon wafer as described above when executing the computer program.
[0064] Specifically, the processor is used to cover the silicon wafer to be processed with an etching solution whose mass percentage concentration is lower than a preset threshold value to remove the oxide film on the surface of the silicon wafer; control the scanning solution to run on the surface of the silicon wafer according to the target path to complete the metal collection on the surface of the silicon wafer; wherein the scanning solution is a mixed acid solution of HF acid solution and other acid solution, and the other acid solution is at least one of HNO3 acid solution, HCl acid solution and H2O2 acid solution.
[0065] It should be noted that the silicon wafer surface metal collection device provided in the embodiment of the present invention is a device capable of executing the above-mentioned silicon wafer surface metal collection method. All embodiments of the above-mentioned silicon wafer surface metal collection method are applicable to the silicon wafer surface metal collection device and can achieve the same or similar technical effects.
[0066] It should be noted that each embodiment in this specification is described in a progressive manner, and the same or similar parts between the embodiments can be referred to each other, and each embodiment focuses on the differences from other embodiments. In particular, for the embodiments, since they are basically similar to the product embodiments, the description is relatively simple, and the relevant parts can be referred to the partial description of the product embodiments.
[0067] Unless otherwise defined, the technical terms or scientific terms used in the present disclosure should be understood by people with ordinary skills in the field to which the present disclosure belongs. The "first", "second" and similar words used in the present disclosure do not indicate any order, quantity or importance, but are only used to distinguish different components. "Include" or "comprise" and similar words mean that the elements or objects appearing before the word cover the elements or objects listed after the word and their equivalents, without excluding other elements or objects. "Connect" or "connected" and similar words are not limited to physical or mechanical connections, but can include electrical connections, whether direct or indirect. "Up", "down", "left", "right" and the like are only used to indicate relative positional relationships. When the absolute position of the described object changes, the relative positional relationship may also change accordingly.
[0068] It will be understood that when an element such as a layer, film, region, or substrate is referred to as being “on” or “under” another element, it can be “directly on” or “under” the other element or intervening elements may be present.
[0069] In the description of the above embodiments, specific features, structures, materials or characteristics may be combined in a suitable manner in any one or more embodiments or examples.
[0070] The above is only a specific embodiment of the present disclosure, but the protection scope of the present disclosure is not limited thereto. Any person skilled in the art who is familiar with the technical field can easily think of changes or substitutions within the technical scope disclosed in the present disclosure, which should be included in the protection scope of the present disclosure. Therefore, the protection scope of the present disclosure should be based on the protection scope of the claims.
Claims
1. A method for collecting metal on the surface of a silicon wafer, characterized in that: include: Covering the silicon wafer to be processed with an etching solution having a mass percentage concentration lower than a preset threshold value to remove an oxide film on the surface of the silicon wafer; Controlling the scanning solution to run along a target path on the surface of the silicon wafer to complete the collection of metal on the surface of the silicon wafer; Wherein, the scanning solution is a mixed acid solution of HF acid solution and other acid solution, and the other acid solution is at least one of HNO3 acid solution, HCl acid solution and H2O2 acid solution.
2. The method for collecting metal on the surface of a silicon wafer according to claim 1, characterized in that: The etching solution is HF solution.
3. The method for collecting metal on the surface of a silicon wafer according to claim 2, characterized in that: The mass percentage concentration of the etching solution is 0.5%-1%, and the volume is 1.3-1.5 ml.
4. The method for collecting metal on the surface of a silicon wafer according to claim 1, characterized in that: The scanning speed of the scanning solution is 5 ml / min-6 ml / min, and the volume of the scanning solution is 1.3-1.5 ml.
5. The method for collecting metal on the surface of a silicon wafer according to claim 1, characterized in that: The scanning solution is a mixed acid solution of HF acid solution, HNO3 acid solution and HCl acid solution.
6. The method for collecting metal on the surface of a silicon wafer according to claim 5, characterized in that: In the scanning solution, the mass percentage concentration of the HF acid solution is 0.5%-1%.
7. The method for collecting metal on the surface of a silicon wafer according to claim 5, characterized in that: In the scanning solution, the mass percentage concentration of the HNO3 acid solution is 33%-35%.
8. The method for collecting metal on the surface of a silicon wafer according to claim 5, characterized in that: In the scanning solution, the mass percentage concentration of the HCl acid solution is 2%-3%.
9. The method for collecting metal on the surface of a silicon wafer according to any one of claims 1 to 8, characterized in that: The size of the silicon wafer is 8 inches or 12 inches, the thickness of the silicon wafer is 700-800 microns, and the surface of the silicon wafer is hydrophobic.
10. A method for detecting metal on the surface of a silicon wafer, characterized in that: include: Obtaining a liquid to be analyzed, wherein the liquid to be analyzed is obtained by the collection method according to any one of claims 1 to 9; The liquid to be analyzed is introduced into an inductively coupled plasma mass spectrometer for elemental analysis.
Citation Information
Cited By
Method for testing content of precious metal on surface of wafer
CN119643681A
A method for testing the noble metal content on the surface of a wafer
CN119643681B