High-residual-magnetism high-coercivity neodymium-iron-boron magnet and preparation method thereof
By using gallium and cobalt in neodymium iron boron magnets to optimize grain boundary performance, combined with inorganic fluoride and high-temperature resistant inorganic adhesives, the problem of improving magnetic performance under the limitation of rare earth elements is solved, and high residual magnetism and high coercivity are achieved NdFeB magnet improves the stability and corrosion resistance of the magnet.
Patent Information
- Application Number
- CN202411325034.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-23
- Publication Date
- 2024-11-12
AI Technical Summary
The existing neodymium iron boron magnets have not reached the theoretical value in terms of magnetic properties, especially the residual magnetism and intrinsic coercive forces. Due to the scarcity and high price of rare earth elements, it is difficult to further improve.
By adding two non-rare earth elements gallium and cobalt to the neodymium iron boron magnet, gallium strengthens the grain boundary mechanical properties, cobalt regulates the grain boundary electronic structure, combines inorganic fluoride and high-temperature resistant inorganic adhesives, optimizes the grain boundary phase and forms a protective film. Improve the stability and corrosion resistance of magnets.
It significantly improves the residual magnetism and coercivity of the neodymium iron boron magnet, improves the long-term stability and corrosion resistance of the magnet, ensures stable operation in harsh environments, reduces the impact of oxidation and corrosion, and enhances the thermal stability of the magnet and magnetization efficiency.
Smart Images

Figure BDA0005055175920000061 
Figure BDA0005055175920000071 
Figure BDA0005055175920000091
Abstract
Description
Technical Field
[0001] The present application relates to the field of preparation of NdFeB magnets, and in particular to a NdFeB magnet with high remanence and high coercivity and a preparation method thereof. Background Art
[0002] NdFeB magnets are the most cost-effective commercial magnetic materials so far due to their high coercivity and high remanence. They are widely used in many fields related to people's livelihood, such as home appliances, transportation, and medical treatment. However, the remanence and intrinsic coercivity of existing NdFeB magnets have not reached the theoretical value. Researchers have been studying to continuously improve the remanence and intrinsic coercivity of NdFeB magnets.
[0003] High remanence and high coercivity NdFeB magnets are a type of NdFeB magnets with strong magnetic properties. The improvement of the magnetic properties of this type of NdFeB magnet is mainly considered in terms of rare earth elements. For example, the use of heavy rare earth elements such as terbium and dysprosium can effectively bring about a significant improvement in magnetic properties. Or other rare earth elements, such as lanthanum and samarium, are added to form different crystal phases with iron and boron to improve magnetic properties. But rare earth elements are scarce after all, and the price of heavy rare earth elements is much higher than that of praseodymium and neodymium. The prices of other rare earth elements are relatively low compared to those of praseodymium and neodymium, but are still relatively high compared to other metals. The scarcity of rare earth elements has always restricted the improvement of the magnetic properties of NdFeB magnets. Summary of the invention
[0004] In order to solve the problem of how to use non-rare earth elements to improve the magnetic properties of high remanence and high coercivity NdFeB magnets, the present application provides a high remanence and high coercivity NdFeB magnet, which uses gallium to strengthen the mechanical properties of the grain boundaries, while cobalt adjusts the electronic structure of the grain boundaries. Through the synergistic effect of the two non-rare earth elements, the performance of the grain boundary phase is comprehensively improved, thereby improving the remanence and coercivity of the high remanence and high coercivity NdFeB magnet.
[0005] In a first aspect, the present application provides a high remanence and high coercivity neodymium iron boron magnet, which adopts the following technical solution: A high remanence and high coercivity neodymium iron boron magnet comprises the following components in parts by weight: 21.1-22.15 parts of praseodymium and neodymium, 8.5-9.1 parts of cerium, 0.91 parts of boron, 0.05-0.15 parts of cobalt, 0.04-0.08 parts of gallium, 0.15 parts of titanium, 0.05 parts of aluminum, 0.1 parts of gallium, 0.05 parts of zirconium and 68.5 parts of iron.
[0006] By adopting the above technical solution, gallium is mainly located in the grain boundary phase in the NdFeB magnet, and as a strengthening agent, it can significantly enhance the mechanical properties near the grain boundary. The grain boundary phase is the interface area between the magnet grains, and its structure, composition and performance have an important influence on the overall performance of the magnet. The addition of gallium can optimize the structure of the grain boundary phase, thereby improving the stability of the magnet. The strengthened grain boundary phase can resist the influence of the external environment (such as temperature, humidity, etc.) on the performance of the magnet, thereby improving the long-term stability of the magnet. Since the addition of gallium can improve the chemical stability of the grain boundary phase, the corrosion resistance of the magnet is also improved, and it can work stably for a long time in a more severe environment.
[0007] The main role of cobalt as a moderator in NdFeB magnets is to adjust the electronic structure near the grain boundaries. Due to element segregation and diffusion, the electronic structure of the grain boundary region is often different from that inside the grain, which will lead to a decrease in magnet performance. The addition of cobalt can neutralize this difference and make the electronic structure of the grain boundary region more uniform, thereby improving the performance of the magnet. The moderating effect of cobalt can reduce the performance degradation caused by element segregation and diffusion, such as the reduction of remanence (Br) and coercivity (Hcj). Remanence is the maximum magnetic induction intensity that a magnet can maintain after the external magnetic field is removed, while coercivity is the ability of a magnet to resist an external reverse magnetic field without demagnetization. The addition of cobalt helps to maintain these two key performance parameters at a high level.
[0008] The cooperation of gallium and cobalt in NdFeB magnets is mainly reflected in the optimization of grain boundary phase. Gallium strengthens the mechanical properties of grain boundaries, while cobalt adjusts the electronic structure of grain boundaries. The synergistic effect of the two makes the performance of grain boundary phase comprehensively improved. The optimized grain boundary phase can not only improve the stability and corrosion resistance of the magnet, but also improve the remanence and coercive force by improving the magnetic flux distribution inside the magnet.
[0009] Preferably, the mass ratio of cobalt to gallium is 1:0.5-0.7.
[0010] By adopting the above technical solution, the above ratio achieves the best balance between cobalt and gallium in improving the performance of magnets. Cobalt is used to adjust the electronic structure, while gallium is used to strengthen the grain boundaries. The appropriate ratio can ensure that the two work synergistically, so that the magnet has better magnetic properties, thermal stability and corrosion resistance. Too high a gallium content will introduce too much non-magnetic phase, thereby reducing the volume fraction of the main phase in the magnet, which may cause the coercive force of the magnet to decrease and the brittleness to increase. And when gallium is excessive, it may change the chemical composition and physical properties of the grain boundary phase, resulting in a weakening of the pinning effect of the grain boundary on the main phase grains, thereby reducing the coercive force.
[0011] Preferably, the high remanence and high coercivity NdFeB magnet further comprises inorganic fluoride and high temperature resistant inorganic glue.
[0012] By adopting the above technical solution, the metal elements in the inorganic fluoride have excellent diffusivity and can effectively diffuse at the grain boundaries, which helps to improve the microstructure of the magnet and thus improve the magnetic properties. The grain boundary is the interface area between the magnet grains, and its structure and properties have an important influence on the overall performance of the magnet. Through the grain boundary diffusion of inorganic fluorides, the structure and properties of the grain boundary phase can be optimized, thereby enhancing the magnetic properties of the magnet.
[0013] High temperature resistant inorganic glue forms multiple layers of strong and high temperature resistant protective film inside the magnet. The protective film can effectively prevent oxygen and corrosive media from contacting the magnet material in a high temperature environment, thereby significantly reducing the oxidation and corrosion of the magnet. Oxidation and corrosion are one of the main reasons for the degradation of magnet performance at high temperatures. Therefore, by reducing these processes, high temperature resistant inorganic glue can significantly improve the thermal stability of the magnet. Magnets with reduced oxidation and corrosion can better maintain their original magnetic properties. Long-term high temperature operation and storage will cause oxide layers and corrosion spots on the surface of the magnet, which will damage the magnetic properties and overall performance of the magnet. These adverse effects are greatly reduced through the protection of high temperature resistant inorganic glue.
[0014] Through the adhesion of inorganic glue, the magnetic powder particles in the magnet can be arranged more closely together to form a more ordered magnetic domain structure. This ordered magnetic domain structure helps to improve the key performance indicators of the magnet, such as the remanence and intrinsic coercive force. At the same time, the ordered magnetic domain structure can also reduce the energy loss of the magnet during the magnetization process and improve the magnetization efficiency of the magnet.
[0015] Although the metal elements in inorganic fluorides can diffuse at the grain boundaries, the fluorine elements are more likely to be concentrated on the high-temperature resistant inorganic glue than the metal elements. This selective distribution helps to reduce the concentration of fluorine elements at the grain boundaries and avoid the negative impact on magnetic properties.
[0016] The present application achieves effective improvement of the magnetic properties of high remanence and high coercivity NdFeB magnets by diffusion of metal elements in inorganic fluorides at grain boundaries, formation of a protective film by high temperature resistant inorganic glue to reduce oxidation and corrosion, adhesion of magnetic powder to improve structural stability, and adsorption of fluorine by high temperature resistant inorganic glue to reduce the concentration of fluorine at grain boundaries.
[0017] Preferably, the inorganic fluoride includes at least one of calcium fluoride, sodium fluoride and potassium fluoride.
[0018] By adopting the above technical scheme, calcium fluoride has a relatively high stability at high temperature, but its diffusion process may involve ion exchange or solid phase diffusion. This means that Ca 2 + and F- ions may migrate directly through grain boundaries in the solid state. The diffusion of calcium fluoride may have a direct impact on the structure and properties of the grain boundary phase of the magnet, thereby affecting the magnetic properties and stability of the magnet.
[0019] During high temperature treatment, sodium fluoride may undergo a phase change from solid to liquid or gas, depending on the treatment temperature. When in liquid or gaseous state, the ions in sodium fluoride are more likely to diffuse at the grain boundaries of the magnet. The diffusion of NaF may help optimize the grain boundary phase, which can affect the chemical composition and structure at the grain boundaries of the magnet, thereby changing the magnetic properties of the magnet. The diffusion principle of potassium fluoride is similar to that of sodium fluoride.
[0020] Preferably, the weight portion of the inorganic fluoride is 0.05-0.15 parts.
[0021] By adopting the above technical solution, when the amount of inorganic fluoride added is too small, the number of fluoride ions participating in grain boundary diffusion is limited, which may lead to the effect of grain boundary diffusion being not obvious. Grain boundary diffusion is crucial to improving the microstructure and magnetic properties of magnets, and too little fluoride addition may not fully play this role. Due to the limited effect of grain boundary diffusion, the improvement of the magnetic properties of the magnet will also be limited. For example, key properties such as the coercive force and remanence of the magnet may not be significantly improved.
[0022] Too much addition of inorganic fluoride may cause excessive changes in the grain boundary structure. Such changes may be detrimental to the improvement of magnet performance and may even lead to a decrease in magnetic properties. For this reason, the applicant has finally determined after a lot of research and experimental verification that the weight of the inorganic fluoride in this application is preferably the above.
[0023] Preferably, the high temperature resistant inorganic glue includes at least one of aluminum silicate inorganic glue, sodium silicate inorganic glue and aluminum oxide inorganic glue.
[0024] By adopting the above technical solutions, aluminum silicate inorganic glue has excellent high temperature stability, can maintain stable performance at extremely high temperatures, and reduce oxidation and corrosion of magnets at high temperatures. Aluminum silicate has a low thermal conductivity and good thermal insulation properties, which helps to reduce the conduction of heat into the magnet and improve the thermal stability of the magnet. Aluminum silicate has a high specific surface area and a good pore structure, which enables aluminum silicate to adsorb and catalyze molecules and has good adsorption properties for fluorine.
[0025] Sodium silicate inorganic glue also has certain high temperature resistance, but its main characteristics lie in its bonding force and water resistance. It can maintain good bonding to the magnet material at high temperatures and enhance the stability of the magnet structure. Alumina inorganic glue has high hardness and wear resistance, which can enhance the wear resistance and impact resistance of the magnet surface. However, its high temperature resistance may be slightly inferior to that of aluminum silicate and sodium silicate. In addition, the adsorption capacity of sodium silicate inorganic glue and alumina inorganic glue for fluorine is weaker than that of aluminum silicate inorganic glue. Therefore, after comparison, it is found that sodium silicate inorganic glue is the preferred choice among the three. Preferably, the temperature range of the high temperature resistant inorganic adhesive is 1200-1500°C.
[0026] By adopting the above technical solution, if the tolerance temperature of the high temperature resistant inorganic glue is too low, the inorganic glue may fail during the sintering or subsequent high temperature operation of the magnet. This will cause the magnet to lose protection and be easily damaged by oxidation, corrosion, etc., thereby failing to further improve the magnetic properties of the high remanence and high coercivity NdFeB magnet.
[0027] NdFeB magnets with high remanence and high coercivity often face high temperature environments in industrial production, such as sintering temperatures that may be as high as 1045°C. In order to ensure that the magnet can work stably under these conditions, its protective material (i.e., high temperature resistant inorganic glue) needs to have a higher tolerance temperature. The range of 1200-1500°C can not only ensure protection during the sintering process, but also cope with the high temperature environment that may be encountered during the subsequent use of the magnet. However, the tolerance temperature may increase the manufacturing cost and such a high tolerance temperature is not required in practical applications. For this reason, the applicant finally determined after a lot of research and experimental verification that the tolerance temperature range of the high temperature resistant inorganic glue of this application is preferably above.
[0028] Preferably, the viscosity of the high temperature resistant inorganic glue is in the range of 300-600 mPa.s.
[0029] By adopting the above technical solution, for the high temperature resistant inorganic glue, the appropriate viscosity can ensure that it can be evenly covered in the high remanence and high coercivity NdFeB magnet during the coating or application process to form a multi-layer continuous and dense protective film. Too low viscosity may cause the inorganic glue to be too fluid, making it difficult to form a stable protective film in the magnet; while too high viscosity may affect the uniformity and density of the protective film, and even make it difficult to fully mix other components of the high remanence and high coercivity NdFeB magnet due to high viscosity. For this reason, the applicant finally determined after a lot of research and experimental verification that the viscosity range of the high temperature resistant inorganic glue of this application is preferably the above.
[0030] Preferably, the weight portion of the high temperature resistant inorganic glue is 0.05-0.1 parts.
[0031] By adopting the above technical scheme, if the weight of the high temperature resistant inorganic glue is too large, it may cause unevenness when mixed with other components of the high remanence and high coercivity NdFeB magnet, affecting the overall performance and stability of the magnet. Too small a weight may not be enough to completely cover the surface of the magnet, or the protective film formed may be too thin to provide sufficient protection. In addition, too low a weight of high temperature resistant inorganic glue affects the grain boundary diffusion of inorganic fluorides in the magnet, thereby affecting the remanence and intrinsic coercivity of the magnet. For this reason, the applicant finally determined after a lot of research and experimental verification that the weight of the high temperature resistant inorganic glue of this application is preferably as above.
[0032] In a second aspect, the present application provides a method for preparing a high remanence and high coercivity NdFeB magnet, using the following technical solution: A method for preparing a high remanence and high coercivity NdFeB magnet, which is used to prepare the high remanence and high coercivity NdFeB magnet, comprises the following steps: Melting and spinning: Pr, Nd, Cer, B, Co, Ga, Ti, Al, Ga, Zr, and Fe are weighed according to the formula and smelted, and the obtained molten liquid is spun to obtain spinning sheets; Hydrogen crushing and grinding: the stripping sheet and the inorganic fluoride are subjected to hydrogen crushing, and then subjected to air flow milling to obtain magnetic powder; mixed pressing: high temperature resistant inorganic glue is added to the magnetic powder, mixed evenly to obtain mixed powder, and the mixed powder is placed under nitrogen protection for molding to obtain a pressed embryo; Sintering and tempering: the pressed green body is sintered and then subjected to a secondary tempering heat treatment to obtain a high remanence and high coercivity NdFeB magnet.
[0033] By adopting the above technical solution, the stripping pieces and inorganic fluorides are subjected to hydrogen cracking treatment and air flow mill grinding, which helps to further refine the microstructure of the stripping pieces and inorganic fluorides, facilitate the grain boundary diffusion of inorganic fluorides in the later stage, and improve the magnetic properties. Adding high-temperature resistant inorganic glue to the magnetic powder and mixing it evenly to obtain a mixed powder can ensure that the inorganic glue is evenly distributed in the magnetic powder, providing favorable conditions for subsequent compression molding. The entire preparation method has a complete process and precise control. From the preparation of raw materials to the final magnet preparation, it has undergone strict processing and optimization to ensure the quality and performance of the magnet.
[0034] In summary, this application has the following beneficial effects: 1. Since gallium is used to strengthen the mechanical properties of the grain boundary, and cobalt is used to adjust the electronic structure of the grain boundary, the synergistic effect of the two improves the performance of the grain boundary phase in an all-round way. The optimized grain boundary phase can not only improve the stability and corrosion resistance of the magnet, but also improve the remanence and coercive force by improving the magnetic flux distribution inside the magnet; 2. The present application achieves effective improvement of the magnetic properties of N33 NdFeB magnets by grain boundary diffusion of metal elements in inorganic fluorides, forming a protective film with high temperature resistant inorganic glue to reduce oxidation and corrosion, and adhering magnetic powder to improve structural stability, as well as adsorbing fluorine elements with high temperature resistant inorganic glue to reduce the concentration of fluorine elements at grain boundaries. DETAILED DESCRIPTION
[0035] The raw materials in this application include the following parts: Praseodymium-neodymium: commercially available products using praseodymium-neodymium alloys; Cerium: a commercial product with CAS No. 7440-45-1 was used; Boron: a commercial product with CAS No. 7440-42-8 was used; Cobalt: a commercial product with CAS No. 7440-48-4 was used; Gallium: a commercial product with CAS No. 7440-54-2 was used; Titanium: a commercial product with CAS No. 7440-32-6 was used; Aluminum: a commercially available product with CAS No. 7429-90-5 was used; Niobium: a commercial product with CAS No. 7440-03-1 was used; Zirconium: a commercial product with CAS No. 7440-67-7 was used; Iron: a commercially available product with CAS No. 7439-89-6 was used; Aluminum silicate inorganic glue: a commercial product with aluminum silicate as main component and CAS number 12141-46-7; Sodium silicate inorganic glue: a commercial product with the main component of sodium silicate and CAS number 1344-09-8 is used; Alumina inorganic glue: a commercial product with a main component of alumina and a CAS number of 11092-32-3; Calcium fluoride: a commercially available product with CAS number 7789-75-5; Sodium fluoride: a commercially available product with CAS number 7681-49-4; Potassium fluoride: a commercially available product with CAS number 7789-23-3; The present application is further described in detail below in conjunction with embodiments and comparative examples.
[0036] Example 1 A method for preparing a high remanence and high coercivity NdFeB magnet comprises the following steps: Melting and spinning: according to the formula, 221.5g of praseodymium and neodymium, 85g of cerium, 91g of boron, 1g of cobalt, 0.6g of gallium, 1.5g of titanium, 0.5g of aluminum, 1g of niobium, 0.5g of zirconium and 685g of iron are weighed and smelted, and the obtained molten liquid is spun to obtain spinning sheets; Hydrogen grinding: The spinning belt is hydrogen broken and then jet milled to obtain magnetic powder. The average particle size of the magnetic powder is 2.7μm, and 50% of the particle size is distributed in 3.5-3.6μm; Mixed pressing: The magnetic powder is placed under nitrogen protection for compression molding to obtain a pressed embryo; Sintering and tempering: the pressed blank is sintered at a sintering temperature of 1045°C and a sintering time of 5.5h. After the secondary tempering heat treatment, the first tempering temperature is 640°C and the tempering time is 3h. After that, the product is cooled to a temperature less than 100°C using argon gas. Then the second tempering heat treatment is started. The second tempering temperature is 640°C and the tempering time is 5h. After that, the product is cooled to room temperature using argon gas to obtain a high remanence and high coercivity NdFeB magnet.
[0037] Example 2-3 Example 2-3 Based on the preparation method of Example 1, the components of praseodymium, neodymium, cerium, cobalt and gallium in the formula are adjusted. The specific adjustments are shown in Table 1.
[0038] Comparative Examples 1-3 Comparative Examples 1-3 are based on the preparation method of Example 1, and the components of cobalt and gallium in the formula are adjusted. The specific adjustments are shown in Table 1.
[0039] Table 1 Raw materials and performance test table of praseodymium, neodymium, cerium, cobalt and gallium in the formulations of Examples 1-3 and Comparative Examples 1-3 Performance Test The high remanence and high coercivity NdFeB magnets of Examples 1-3 and Comparative Examples 1-3 were subjected to the following performance tests. The test results are shown in Table 1: 1. Remanence and intrinsic coercivity According to GB / T3217-2013 "Magnetic Test Methods for Permanent Magnet (Hard Magnet) Materials", the remanence (Br) and intrinsic coercivity (Hcj) of high remanence and high coercivity NdFeB magnets are tested.
[0040] Referring to Table 1, by comparing Examples 1-3 with Comparative Examples 1-3, it can be seen that compared with Comparative Example 3, the remanence and intrinsic coercivity of Examples 1-3 are much higher than those of Comparative Example 3, indicating that the addition of cobalt and gallium to high remanence and high coercivity NdFeB magnets can effectively improve the magnetic properties of high remanence and high coercivity NdFeB magnets; Similarly, the remanence and intrinsic coercivity of Examples 1-3 are higher than those of Comparative Examples 1-2; for Comparative Example 1, gallium is not added to the high remanence and high coercivity NdFeB magnet, and only cobalt is used to adjust the electronic structure near the grain boundary, and the degree of optimization of the grain boundary phase is limited, so that the magnetic properties of the high remanence and high coercivity NdFeB magnet are improved to a limited extent; for Comparative Example 2, cobalt is not added to the high remanence and high coercivity NdFeB magnet, and when gallium significantly improves the mechanical properties near the grain boundary, the electronic structure near the grain boundary does not change much, so that the magnetic properties of the high remanence and high coercivity NdFeB magnet are improved to a limited extent; Therefore, cobalt and gallium need to be added simultaneously to the high remanence and high coercivity NdFeB magnet to effectively improve the magnetic properties of the high remanence and high coercivity NdFeB magnet; in comparison, the magnetic properties of the high remanence and high coercivity NdFeB magnet of Example 1 are preferred among Examples 1-3.
[0041] Embodiment 4-5 Example 4-5 Based on the preparation method of Example 1, the amount of gallium added is adjusted, and the specific adjustment is shown in Table 2.
[0042] Comparative Example 4-5 Based on the preparation method of Example 1, the amount of gallium added was adjusted, and the specific adjustment is shown in Table 2.
[0043] The high remanence and high coercivity NdFeB magnets of Examples 4-5 and Comparative Examples 4-5 were subjected to the above performance tests, and the test results are shown in Table 2.
[0044] Table 2 Gallium addition amount and performance test table of Example 1, Examples 4-5 and Comparative Examples 4-5 project Example 1 Example 4 Example 5 Comparative Example 4 Comparative Example 5 Gallium / g 0.6 0.5 0.7 0.4 0.8 Br / kGs 16.52 14.21 15.66 13.47 13.95 HkDJ 14.74 12.86 14.07 12.10 12.63 Referring to Table 2, by comparing Example 1, Examples 4-5 and Comparative Examples 4-5, it can be seen that as the amount of gallium added continues to increase, the remanence and intrinsic coercivity of the high remanence and high coercivity NdFeB magnet both show a trend of first increasing and then decreasing. This may be because as the amount of gallium added continues to increase, gallium continuously strengthens the mechanical properties of the grain boundaries, thereby increasing the magnetic properties of the high remanence and high coercivity NdFeB magnet; when the amount of gallium added exceeds a certain range, it may change the chemical composition and physical properties of the grain boundary phase, resulting in a weakening of the pinning effect of the grain boundary phase on the main phase grains, thereby reducing the magnetic properties.
[0045] Embodiment 6-8 Example 6 Based on the preparation method of Example 1, 1.2 g of calcium fluoride and a spinning sheet were hydrogen-broken and then jet-milled to obtain magnetic powder; 0.8 g of inorganic aluminum silicate glue is added to the magnetic powder. The aluminum silicate glue has a temperature tolerance of 1500° C. and a viscosity of 500 mPa.s. The mixture is evenly mixed to obtain a mixed powder. The mixed powder is then compression molded under nitrogen protection to obtain a pressed embryo.
[0046] In Example 7-8, based on the preparation method of Example 6, the type of high temperature resistant inorganic glue is adjusted. The specific adjustments are shown in Table 3.
[0047] The high remanence and high coercivity NdFeB magnets of Examples 6-8 were subjected to the above performance tests, and the test results are shown in Table 3.
[0048] Table 3 Types and performance test table of high temperature resistant inorganic adhesives of Example 1 and Examples 6-8 project Example 1 Example 6 Example 7 Example 8 High temperature resistant inorganic adhesive type / Aluminum silicate Sodium silicate Alumina Br / kGs 16.52 17.97 17.41 17.13 HkDJ 14.74 15.92 15.46 15.24 Referring to Table 3, by comparing Example 1 with Examples 6-8, it can be seen that adding high temperature resistant inorganic glue to the high remanence and high coercivity NdFeB magnet can effectively improve the magnetic properties of the magnet. This may be due to the fact that the high temperature resistant inorganic glue forms a protective film to reduce oxidation and corrosion and adheres to magnetic powder to improve structural stability. This provides a more comprehensive and effective protection for the high remanence and high coercivity NdFeB magnet, thereby effectively improving the magnetic properties of the high remanence and high coercivity NdFeB magnet.
[0049] Comparing Examples 6-8, it is found that Example 6 has the best performance and is preferred. This may be because the aluminum silicate inorganic glue has excellent high-temperature stability, can maintain stable performance at extremely high temperatures, and reduce the oxidation and corrosion of the magnet at high temperatures. Aluminum silicate has a low thermal conductivity and good thermal insulation properties, which helps to reduce the conduction of heat to the inside of the magnet and improve the thermal stability of the magnet. Aluminum silicate has a high specific surface area and a good pore structure, which enables aluminum silicate to adsorb and catalyze molecules and should have good adsorption properties for fluorine elements.
[0050] Examples 9-10 In Examples 9-10, based on the preparation method of Example 6, the tolerance temperature of the inorganic aluminum silicate glue is adjusted. The specific adjustment is shown in Table 4.
[0051] Comparative Example 6-7 is based on the preparation method of Example 6, and the tolerance temperature of the aluminum silicate inorganic glue is adjusted. The specific adjustment is shown in Table 4.
[0052] The high remanence and high coercivity NdFeB magnets of Examples 9-10 and Comparative Examples 6-7 were subjected to the above performance tests, and the test results are shown in Table 4.
[0053] Table 4 Temperature tolerance and performance test table of the aluminum silicate inorganic glue of Example 6, Examples 9-10 and Comparative Examples 6-7 project Example 6 Example 9 Example 10 Comparative Example 6 Comparative Example 7 Tolerance temperature / ℃ 1500 1200 1400 1100 1600 Br / kGs 17.97 16.86 17.51 16.56 17.98 HkDJ 15.92 15.02 15.51 14.78 15.92 Referring to Table 4, by comparing Example 6, Examples 9-10 and Comparative Examples 6-7, it can be seen that as the tolerance temperature of the aluminum silicate inorganic glue continues to increase, the remanence and intrinsic coercivity of the high remanence and high coercivity NdFeB magnet both show a trend of continuously rising and then stabilizing. This may be because as the tolerance temperature of the aluminum silicate inorganic glue continues to increase, the aluminum silicate inorganic glue gradually stabilizes during the sintering of the high remanence and high coercivity NdFeB magnet, so that multiple protective films are formed in the magnet, thereby continuously improving the magnetic properties of the high remanence and high coercivity NdFeB magnet.
[0054] Examples 11-12 In Examples 11-12, based on the preparation method of Example 6, the viscosity of the aluminum silicate inorganic glue was adjusted, and the specific adjustment is shown in Table 5.
[0055] Comparative Examples 8-9 Comparative Examples 8-9 Based on the preparation method of Example 6, the viscosity of the aluminum silicate inorganic glue was adjusted, and the specific adjustment is shown in Table 5.
[0056] The high remanence and high coercivity NdFeB magnets of Examples 11-12 and Comparative Examples 8-9 were subjected to the above performance tests, and the test results are shown in Table 5 respectively.
[0057] Table 5 Viscosity and performance test table of aluminum silicate inorganic glue of Example 6, Examples 11-12 and Comparative Examples 8-9 Referring to Table 5, it can be seen from the comparison of Example 6, Examples 11-12 and Comparative Examples 8-9 that as the viscosity of the aluminum silicate inorganic glue continues to increase, the remanence and intrinsic coercivity of the high remanence and high coercivity NdFeB magnet both show a trend of first increasing and then decreasing. This may be because as the viscosity of the aluminum silicate inorganic glue continues to increase, the fluidity of the aluminum silicate inorganic glue continues to increase, and a stable protective film is gradually formed in the magnet, thereby increasing the magnetic properties of the high remanence and high coercivity NdFeB magnet; when the viscosity of the aluminum silicate inorganic glue exceeds a certain range, it may affect the uniformity and density of the protective film, and even make other components of the high remanence and high coercivity NdFeB magnet difficult to fully mix due to the high viscosity, thereby reducing the magnetic properties of the high remanence and high coercivity NdFeB magnet.
[0058] Examples 13-14 In Examples 13-14, based on the preparation method of Example 6, the amount of aluminum silicate inorganic glue added was adjusted, and the specific adjustments are shown in Table 6.
[0059] Comparative Examples 10-11 Comparative Examples 10-11 are based on the preparation method of Example 6, and the addition amount of the inorganic aluminum silicate glue is adjusted. The specific adjustment is shown in Table 6.
[0060] The high remanence and high coercivity NdFeB magnets of Examples 13-14 and Comparative Examples 10-11 were subjected to the above performance tests, and the test results are shown in Table 6.
[0061] Table 6 Addition amount and performance test table of aluminum silicate inorganic glue of Example 6, Examples 13-14 and Comparative Examples 10-11 Referring to Table 6, it can be seen from the comparison of Example 6, Examples 13-14 and Comparative Examples 10-11 that as the amount of aluminum silicate inorganic glue added continues to increase, the remanence and intrinsic coercivity of the high remanence and high coercivity NdFeB magnet both show a trend of first increasing and then decreasing. This may be because as the amount of aluminum silicate inorganic glue added continues to increase, the fluidity of the aluminum silicate inorganic glue continues to increase, and a stable protective film is gradually formed in the magnet. In addition, more aluminum silicate inorganic glue helps calcium fluoride to diffuse at the grain boundaries in the magnet, thereby increasing the magnetic properties of the high remanence and high coercivity NdFeB magnet. When the amount of aluminum silicate inorganic glue added exceeds a certain range, it may cause it to produce an uneven phenomenon when mixed with other components of the high remanence and high coercivity NdFeB magnet, thereby reducing the magnetic properties of the high remanence and high coercivity NdFeB magnet.
[0062] Examples 15-18 In Examples 15-16, based on the preparation method of Example 6, the type of inorganic fluoride is adjusted, and the specific adjustment is shown in Table 7.
[0063] Example 17 is based on the preparation method of Example 6, except that the aluminum silicate inorganic glue is removed and other conditions remain unchanged.
[0064] Example 18 is based on the preparation method of Example 6, except that calcium fluoride is removed and other conditions remain unchanged.
[0065] The high remanence and high coercivity NdFeB magnets of Examples 15-18 were subjected to the above performance tests, and the test results are shown in Table 7.
[0066] Table 7 Type and performance test data of inorganic fluoride of Example 6 and Examples 15-18 project Example 6 Embodiment 15 Example 16 Embodiment 17 Embodiment 18 Types of Inorganic Fluorides Calcium Fluoride Sodium fluoride Potassium fluoride Calcium Fluoride / Br / kGs 17.97 17.52 17.48 16.83 17.01 HkDJ 15.92 15.55 15.52 14.98 15.14 Referring to Table 7, it can be seen from Comparative Example 6 and Examples 15-18 that adding inorganic fluoride to high remanence high coercivity NdFeB magnets can effectively improve the magnetic properties of the magnet. The metal elements in the inorganic fluoride have excellent diffusivity and can effectively carry out grain boundary diffusion, which helps to improve the microstructure of the magnet and thus improve the magnetic properties. The grain boundary is the interface region between the magnet grains, and its structure and properties have an important influence on the overall performance of the magnet. Through the grain boundary diffusion of inorganic fluoride, the structure and performance of the grain boundary phase can be optimized, thereby enhancing the magnetic properties of the magnet.
[0067] Compared with Example 6, Example 6 has lower remanence and intrinsic coercivity. Therefore, calcium fluoride and aluminum silicate inorganic glue need to be added to the high remanence and high coercivity NdFeB magnet to effectively improve the magnetic properties of the high remanence and high coercivity NdFeB magnet. It may be because the calcium element in calcium fluoride can diffuse at the grain boundaries, but its fluorine element is more easily concentrated on the aluminum silicate inorganic glue than the calcium element. This selective distribution helps to reduce the concentration of fluorine at the grain boundaries and avoid the negative impact on magnetic properties.
[0068] Comparing Example 6 with Examples 15-16, it is found that Example 6 has the best performance and is preferred. This may be because calcium fluoride has a relatively high stability at high temperatures, but its diffusion process may involve ion exchange or solid phase diffusion. This means that Ca 2 + and F- ions may migrate directly through grain boundaries in the solid state. The diffusion of calcium fluoride may have a direct impact on the structure and properties of the grain boundary phase of the magnet, thereby affecting the magnetic properties and stability of the magnet.
[0069] Examples 19-20 In Examples 19-20, based on the preparation method of Example 6, the amount of calcium fluoride added was adjusted, and the specific adjustments are shown in Table 8.
[0070] Comparative Examples 12-13 Comparative Examples 12-13 are based on the preparation method of Example 6, except that the amount of calcium fluoride added is adjusted. The specific adjustments are shown in Table 8.
[0071] The high remanence and high coercivity NdFeB magnets of Examples 19-20 and Comparative Examples 12-13 were subjected to the above performance tests, and the test results are shown in Table 8.
[0072] Table 8 The addition amount and performance test data of calcium fluoride in Example 6, Examples 19-20 and Comparative Examples 12-13 project Example 6 Embodiment 17 Embodiment 18 Comparative Example 12 Comparative Example 13 Calcium fluoride / g 1.2 0.5 1.5 0.4 1.8 Br / kGs 17.97 16.21 17.30 15.54 16.15 HkDJ 15.92 14.49 15.35 13.89 14.44 Referring to Table 8, it can be seen from Example 6, Examples 19-20 and Comparative Examples 12-13 that as the amount of calcium fluoride added increases, the remanence and intrinsic coercivity of the high remanence and high coercivity NdFeB magnets show a trend of first increasing and then decreasing. This may be because as the amount of calcium fluoride added increases, the calcium ions participating in the grain boundary diffusion increase, which improves the effect of grain boundary diffusion, thereby increasing the magnetic properties of the high remanence and high coercivity NdFeB magnets. When the amount of calcium fluoride added exceeds a certain range, excessive addition of inorganic fluoride may cause excessive changes in the grain boundary structure, thereby causing a decrease in magnetic properties.
[0073] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A high remanence and high coercivity neodymium iron boron magnet, characterized in that: The invention comprises the following components in parts by weight: 21.1-22.15 parts of praseodymium and neodymium, 8.5-9.1 parts of cerium, 0.91 parts of boron, 0.05-0.15 parts of cobalt, 0.04-0.08 parts of gallium, 0.15 parts of titanium, 0.05 parts of aluminum, 0.1 parts of gallium, 0.05 parts of zirconium and 68.5 parts of iron.
2. The high remanence and high coercivity NdFeB magnet according to claim 1, characterized in that: The mass ratio of cobalt to gallium is 1:0.5-0.
7.
3. The high remanence and high coercivity NdFeB magnet according to claim 1, characterized in that: It also includes inorganic fluorides and high temperature resistant inorganic glues.
4. The high remanence and high coercivity NdFeB magnet according to claim 3, characterized in that: The inorganic fluoride includes at least one of calcium fluoride, sodium fluoride and potassium fluoride.
5. The high remanence and high coercivity NdFeB magnet according to claim 4, characterized in that: The weight portion of the inorganic fluoride is 0.05-0.15 parts.
6. The high remanence and high coercivity NdFeB magnet according to claim 3, characterized in that: The high temperature resistant inorganic glue comprises at least one of aluminum silicate inorganic glue, sodium silicate inorganic glue and aluminum oxide inorganic glue.
7. The high remanence and high coercivity NdFeB magnet according to claim 6, characterized in that: The high temperature resistant inorganic adhesive has a tolerable temperature range of 1200-1500°C.
8. The high remanence and high coercivity NdFeB magnet according to claim 6, characterized in that: The viscosity of the high temperature resistant inorganic glue is in the range of 300-600 mPa.s.
9. The high remanence and high coercivity NdFeB magnet according to claim 6, characterized in that: The weight portion of the high temperature resistant inorganic glue is 0.05-0.1 parts.
10. The method for preparing the high remanence and high coercivity NdFeB magnet according to any one of claims 1 to 9, characterized in that: The following steps are involved: Melting and spinning: weighing praseodymium, neodymium, cerium, boron, cobalt, gallium, titanium, aluminum, gallium, zirconium, and iron according to the formula amount for smelting, spinning the obtained molten liquid to obtain spinning sheets; Hydrogen crushing and grinding: the stripping pieces and the inorganic fluoride are subjected to hydrogen crushing, and then subjected to jet mill grinding to obtain magnetic powder; Mixing and pressing: adding high temperature resistant inorganic glue to the magnetic powder, mixing evenly to obtain mixed powder, and placing the mixed powder under nitrogen protection for compression molding to obtain a pressed embryo; Sintering and tempering: the pressed green body is sintered and then subjected to a secondary tempering heat treatment to obtain a high remanence and high coercivity NdFeB magnet.
Citation Information
Cited By
Anti-corrosion neodymium iron boron magnetic material and preparation process thereof
CN119943567A
A corrosion-resistant NdFeB magnetic material and its preparation process
CN119943567B
High-temperature-resistant high-residual-magnetism rare earth permanent magnet material and preparation process thereof
CN120527108A