Method for preparing high-quality CsPbBr3 perovskite thin film through inorganic metal salt modification
By using inorganic metal salt CsAc as an interface modification material in CsPbBr3 solar cells, the problems of interface defects and carrier recombination are solved, and the photoelectric efficiency and stability of all-inorganic perovskite CsPbBr3 solar cells are improved.
Patent Information
- Application Number
- CN202410996909.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-08
AI Technical Summary
All-inorganic perovskite CsPbBr3 solar cells have large open circuit voltage losses due to interface defects and carrier recombination, and the battery's photovoltaic performance is poor. New strategies are needed to passivate interface defects and suppress non-radiative recombination.
Inorganic metal salt CsAc is used as the interface modification material, and CsPbBr3 film is prepared by spin coating with SnO2 layer and multi-step spin coating to reduce the impurities and bottom interface defects, and improve the film quality and photoelectric efficiency.
By introducing the CsAc layer, the problem of insufficient Cs at the bottom interface is alleviated, and more stable crystals are formed, interface defects are reduced, and the photoelectric efficiency and stability of CsPbBr3 solar cells are improved.
Smart Images

Figure FT_1 
Figure FT_2 
Figure FT_3
Abstract
Description
Technical Field
[0001] The invention relates to an application of an inorganic metal salt CsAc in improving the efficiency of an all-inorganic perovskite CsPbBr3 perovskite solar cell and a method for preparing a CsPbBr3 solar cell by passivation using an inorganic material, and in particular to a method for preparing a CsPbBr3 solar cell with high efficiency by inorganic passivation. Background Art
[0002] In recent years, perovskite materials have become the focus of world attention due to their excellent photoelectric properties such as high absorption coefficient, low exciton binding energy, and long carrier diffusion length. In just over a decade, the photoelectric conversion efficiency of solar cells based on organic-inorganic hybrid perovskite semiconductor materials has increased from 3.8% to 26.1%. However, due to the high volatility of organic cations, organic-inorganic hybrid perovskites are prone to component degradation under high temperature and humid conditions. + and FA + Organic cations such as Cs may react with water molecules or form hydrates under thermal conditions, leading to device instability and degradation. + ) substituted organic cation (MA + / FA + ) showed better mechanical properties and water stability. Therefore, all-inorganic perovskite CsPbBr3 has become a hot topic among scholars.
[0003] CsPbBr3 is a direct bandgap semiconductor with good thermal stability, low trap state density, high carrier mobility under illumination, and high theoretical open circuit voltage (1.98V), which makes it suitable for use in light-driven chemical reactions and stacked solar cells. However, the wide-bandgap CsPbBr3 PSC has a large open circuit voltage loss, which is mainly due to the carrier recombination caused by defect states in the perovskite and the energy level barrier between interfaces that hinders the extraction of carriers, resulting in a large open circuit voltage loss and poor photovoltaic performance of the cell. Therefore, the future development of CsPbBr3 perovskite requires the careful design and preparation of basic functional layers such as perovskite layers and interfaces to inhibit charge recombination and reduce energy loss. Therefore, it is very important to develop new effective strategies such as composite engineering and interface engineering to passivate interface defects and inhibit non-radiative recombination. Summary of the invention
[0004] The present invention uses inorganic metal salt CsAc as an interface modification material to improve the efficiency and various photovoltaic properties of CsPbBr3PSC. CsAc can be used as a Cs source to solve the problem of insufficient precursor reaction. +First, it reacts with PbBr2 to generate CsPb2Br5, and then reacts with CsBr to form CsPbBr3, which reduces the impurities in the film and improves the film quality. - Can replace Br - , so that the tensile strain of the bottom interface is released, the generation of bottom interface defects is greatly reduced, and the photoelectric efficiency is improved.
[0005] The present invention comprises the following steps:
[0006] Step 1: The FTO conductive glass was ultrasonically treated with deionized water, anhydrous ethanol, acetone, and isopropanol for 10 minutes in sequence, and then dried with nitrogen and plasma cleaned for 10 minutes. Then, the SnO2 solution was spin-coated on the surface of the FTO conductive glass, and then annealed to obtain a substrate containing a SnO2 electron transport layer.
[0007] Step 2: First, prepare 0.02mol / L, 0.04mol / L, 0.06mol / L and 0.08mol / L CsAc solutions, stir them thoroughly, and then spin-coat them on SnO2 at 8000rpm for 30s, and then anneal them at 100℃ on a hot stage for 10min.
[0008] Step 3: CsPbBr3 film was prepared by two-step spin coating. In the first step, the PbBr2 film was spin coated. The prepared PbBr2 / DMF solution (1.0 mol / L) was stirred at 70°C for 30 min, and then spin coated on the ETL at a speed of 2000 rpm for 30 s. The prepared PbBr2 film was annealed at 95°C for 30 min. Then, an aqueous solution of CsBr was spin coated on it. Specifically, after the substrate was cooled, 150 μL of 1 mol / L CsBr aqueous solution was dropped on the PbBr2 film. After staying for 15 s, it was spin coated at 2000 rpm for 30 s, and then annealed at 270°C for 10 min. The obtained perovskite film was soaked in isopropanol for 30 min, and then dried again at 270°C for 15 min.
[0009] Step 4: After the surface of the prepared CsPbBr3 film is cleaned, a few electrodes are pasted on one side of the etched area with heat-resistant tape, and then carbon paste is applied on it and the excess carbon paste is scraped off with a scraper, and then it is placed on a hot plate at 120°C for annealing for 15 minutes. After annealing, a portion of the CsPbBr3 film is scraped off on the opposite side of the etched area with a scraper to serve as an electrode.
[0010] The present invention has the following advantages and beneficial effects: a method is proposed to solve the problem of interface impurities and strain by introducing a CsAc sacrificial layer. The method alleviates the problem of insufficient Cs at the bottom interface by spin-coating CsAc on the SnO2 layer, forms a more stable crystal, and alleviates the tensile stress at the bottom interface. The invention provides an effective strategy for preparing high-quality, low-defect, and high-stability CsPbBr3 PSCs. BRIEF DESCRIPTION OF THE DRAWINGS
[0011] The present invention is further described below in conjunction with the accompanying drawings and embodiments.
[0012] Figure 1 It is the molecular structure of the modifier cesium acetate (CsAc);
[0013] Figure 2 are SEM images of the top surface and cross section of the unmodified CsPbBr3 film and the CsPbBr3 film modified with CsAc;
[0014] Figure 3 is the back SEM image of the unmodified CsPbBr3 film and the CsPbBr3 film modified with CsAc;
[0015] Figure 4 This is the working principle diagram of the modifier CsAc modifying CsPbBr3 film;
[0016] Figure 5 are the back and front XRD patterns of the unmodified CsPbBr3 film and the CsPbBr3 film modified with CsAc;
[0017] Figure 6 The back GIXRD patterns of unmodified CsPbBr3 film and CsAc-modified CsPbBr3 film
[0018] Figure 7 They are the JV curves of unmodified CsPbBr3 film and CsPbBr3 film modified with CsAc, the conductivity of SnO2 under unmodified and different modification conditions, the MS graphs of unmodified CsPbBr3 film and CsAc modified CsPbBr3 film and the stability test graphs of the prepared CsPbBr3 devices. Specific implementation plan
[0019] 1. Preparation of unmodified perovskite films
[0020] The FTO conductive glass was ultrasonically treated with deionized water, anhydrous ethanol, acetone, and isopropanol for 10 minutes in sequence, dried with nitrogen gas, and plasma cleaned for 10 minutes. Then, a SnO2 solution was spin-coated on the surface of the FTO conductive glass and annealed to obtain a substrate containing a SnO2 electron transport layer.
[0021] PbBr2 (367 mg) was dissolved in 1 mL of N,N-dimethylformamide (DMF), heated at 70 ° C and stirred for 5 hours; CsBr (212.8 mg) was dissolved in 1 mL of deionized water. Stirred at 70 ° C for 30 minutes, then spin-coated on the ETL at 2000 rpm for 30 seconds, and the prepared PbBr2 film was annealed at 95 ° C for 30 minutes. After the substrate was cooled, 150 μL of 1 mol / L CsBr aqueous solution was dropped on the PbBr2 film, left for 15 seconds, and then spin-coated at 2000 rpm for 30 seconds, followed by annealing at 270 ° C for 10 minutes. The obtained perovskite film was soaked in isopropanol for 30 minutes, and then dried again at 270 ° C for 15 minutes.
[0022] 2. Preparation of perovskite films with modifiers
[0023] The FTO conductive glass was ultrasonically treated with deionized water, anhydrous ethanol, acetone, and isopropanol for 10 minutes in sequence, dried with nitrogen gas, and plasma cleaned for 10 minutes. Then, a SnO2 solution was spin-coated on the surface of the FTO conductive glass and annealed to obtain a substrate containing a SnO2 electron transport layer.
[0024] Prepare 0.02 mol / L, 0.04 mol / L, 0.06 mol / L and 0.08 mol / L CsAc solutions, stir them thoroughly, spin-coat them on SnO2 at 8000 rpm for 30 s, and then anneal them on a hot stage at 100°C for 10 min.
[0025] PbBr2 (367 mg) was dissolved in 1 mL of N,N-dimethylformamide (DMF), heated at 70 ° C and stirred for 5 hours; CsBr (212.8 mg) was dissolved in 1 mL of deionized water. Stirred at 70 ° C for 30 minutes, then spin-coated on the ETL at 2000 rpm for 30 seconds, and the prepared PbBr2 film was annealed at 95 ° C for 30 minutes. After the substrate was cooled, 150 μL of 1 mol / L CsBr aqueous solution was dropped on the PbBr2 film, left for 15 seconds, and then spin-coated at 2000 rpm for 30 seconds, followed by annealing at 270 ° C for 10 minutes. The obtained perovskite film was soaked in isopropanol for 30 minutes, and then dried again at 270 ° C for 15 minutes.
[0026] 3. Preparation of CsPbBr3 PSCs
[0027] After the surface of the prepared CsPbBr3 film is cleaned, several electrodes are pasted on one side of the etched area with heat-resistant tape, and then carbon paste is applied on it and the excess carbon paste is scraped off with a scraper, and then it is placed on a hot plate at 120°C for annealing for 15 minutes. After annealing, a portion of the CsPbBr3 film is scraped off on the opposite side of the etched area with a scraper to serve as an electrode.
Claims
1. CsAc modified CsPbBr3 perovskite solar cell device, characterized in that, CsAc regulates the crystallinity of the buried interface of CsPbBr3 films and releases the buried interface stress. The CsAc-assisted regulation is obtained by dissolving CsAc in water, stirring, filtering, spin coating, and then annealing.
2. Application of CsAc molecules in the nucleation and growth of all-inorganic perovskite thin film crystals.
3. The use according to claim 2, characterized in that: The perovskite film is a film used for a perovskite photoelectric device; the perovskite photoelectric device is selected from a perovskite solar cell, a perovskite light emitting diode or a perovskite photodetector.
4. A perovskite solar cell, characterized in that: A high-quality CsPbBr3 perovskite film comprising the CsAc-assisted growth described in claim 1.
5. The method for preparing the perovskite solar cell device according to claim 4, comprising the following steps: S1: First, soak the etched FTO conductive glass in detergent water and put it in an ultrasonic cleaner for 10 minutes. Then scrub the FTO conductive glass manually for 3 minutes until there are no foreign particles on the surface, and put it into the box with the etched area facing up for later use. After all the FTO conductive glass has been scrubbed, use the following sequence to ultrasonically clean it, each time for 10 minutes: tap water twice, deionized water twice, anhydrous ethanol twice, acetone once, and isopropanol once. After the ultrasound is over, use nitrogen to blow dry the isopropanol on the surface, and then put it in a clean porcelain boat for later use. S2: Before spin coating the SnO2 film, it must first be plasma cleaned for 15 minutes to remove surface impurities and make the FTO surface hydrophilic. Prepare the SnO2 solution in a clean glass vial. First, use a pipette to take 2 ml of water into the vial, and then use a pipette to take 450 μL of SnO2 aqueous solution (15%) and 300 μL of LiCl aqueous solution (17 mg / 4 mL) and add them in sequence. After stirring the prepared solution for half an hour, filter it with a nylon-66 filter membrane with a specification of 0.22 μm, and then it can be used for spin coating. Before spin coating, blow the conductive glass clean with an ear bulb, then evenly apply the SnO2 solution on the FTO surface, rotate at 4000 rpm for 30 seconds, and anneal the spin-coated substrate on a hot table at 170°C for 30 minutes. S3: First, prepare 0.02mol / L, 0.04mol / L, 0.06mol / L and 0.08mol / L CsAc solutions, stir them thoroughly, and then spin-coat them on SnO2 at 8000rpm for 30s, and then anneal them on a hot stage at 100℃ for 10min. S4: CsPbBr3 film was prepared by two-step spin coating. In the first step, the PbBr2 film was spin coated. The prepared PbBr2 / DMF solution (1.0 mol / L) was stirred at 70°C for 30 min, and then spin coated on the ETL at a speed of 2000 rpm for 30 s. The prepared PbBr2 film was annealed at 95°C for 30 min. Then, an aqueous solution of CsBr was spin coated on it. Specifically, after the substrate was cooled, 150 μL of 1 mol / L CsBr aqueous solution was dropped on the PbBr2 film. After staying for 15 s, it was spin coated at 2000 rpm for 30 s, and then annealed at 270°C for 10 min. The obtained perovskite film was soaked in isopropanol for 30 min, and then dried again at 270°C for 15 min. S5: The carbon electrode was prepared by tape scraping. After the surface of the prepared CsPbBr3 film was cleaned, several electrodes were pasted on one side of the etching area with heat-resistant tape, and then carbon paste was applied on it and the excess carbon paste was scraped off with a scraper. Then it was placed on a hot plate at 120°C for annealing for 15 minutes. After annealing, a part of the CsPbBr3 film was scraped off on the opposite side of the etching area with a scraper to serve as an electrode.
6. The method for growing CsPbBr3 thin film with CsAc assistance according to claim 5, characterized in that: A modification layer CsAc is added between the ETL and the perovskite layer.
7. The method for growing CsPbBr3 thin film with CsAc assistance according to claim 5, characterized in that: The amount of additive CsAc is 0.02 mol / L, 0.04 mol / L, 0.06 mol / L, 0.08 mol / L, and the annealing temperature is 100°C.
8. The method for growing CsPbBr3 thin film with CsAc assistance according to claim 5, characterized in that: In the step 4, the mass ratio of CsBr to PbBr2 is (212.8):(367), and the molar ratio is (1):(1).