Chromium oxide positive electrode with core-shell structure and preparation method of chromium oxide positive electrode
By doping metal elements in chromium oxide and coating garnet electrolyte to form a core-shell structure chromium oxide positive electrode, the problems of low discharge capacity and instability of chromium oxide materials are solved, and high discharge specific capacity and excellent The cycle stability is suitable for new energy and military battery applications.
Patent Information
- Application Number
- CN202411161000.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-22
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-08-22
AI Technical Summary
The low discharge specific capacity, poor rate performance and cycle stability of chromium oxide cathode materials limit their application in the fields of new energy vehicles and military power supplies.
The core-shell structure chromium oxide positive electrode material is used to form the MxCr8-xO21-@LLZAO structure by doping the third cycle, fourth cycle and transition metal elements into the chromium oxide, and using the garnet electrolyte LLZAO as the cladding layer. Improve its discharge capacity and cycle stability.
It significantly improves the discharge specific capacity and rate performance of the chromium oxide positive electrode, enhances the cycle stability, is simple and easy to operate, and is suitable for the modification of other lithium-ion battery oxide positive electrode materials.
Smart Images

Figure CN118919643A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of lithium ion batteries and relates to a core-shell structure chromium oxide positive electrode and a preparation method thereof. Background Art
[0002] In recent years, with the continuous expansion of new energy vehicles and military power applications, the requirements for the energy density, power characteristics and other performance of lithium batteries have become increasingly higher. The key to the performance of lithium batteries lies in the selection of positive electrode materials. Currently, the energy density of commercially available positive electrode materials such as LiCoO2, LiFePO4, LiMn2O4, and ternary positive electrodes (NCM, NCA) is difficult to exceed 300Wh / kg and their development has reached a bottleneck. Chromium oxide (Cr8O 21 ) as a positive electrode material for lithium batteries, with high theoretical specific capacity (~642mAh / g), high voltage platform (3.0V, vs Li + / Li), and its lithium storage capacity is higher than other transition metal oxide materials, so it has attracted widespread attention from researchers. 21 It is mainly obtained by high-temperature solid-phase heat treatment of raw material CrO3. Affected by heat treatment temperature, time, heating rate and other conditions, it is difficult to obtain a single chromium oxide product, resulting in its discharge specific capacity being far less than the theoretical capacity. At the same time, the irreversible capacity loss of the chromium oxide positive electrode in the first cycle is very large, which greatly limits its practical application.
[0003] At present, the modification research around related issues mainly includes the following parts: (1) regulating the structural composition of chromium oxide by changing the process conditions (calcination temperature, time, atmosphere, calcination times, etc.); (2) stabilizing the structure of chromium oxide by adding metal oxides (such as Al2O3, TiO2, etc.) to coat and improve the rate performance; (3) reducing the dissolution of chromium oxide in the electrolyte by doping exogenous elements in chromium oxide to replace chromium ions, thereby improving its electrochemical performance. However, the above methods have not fundamentally improved the problems of low discharge capacity, poor rate performance and cycle stability of chromium oxide. In actual measurements, chromium oxide positive electrodes generally only cycle at a small rate below 0.1C, with a first-cycle discharge capacity of less than 400mAh / g and poor cycle stability, which further limits the commercial and military applications of this material.
[0004] Therefore, it is particularly important and challenging to develop a simple and easy method to improve the discharge specific capacity, rate performance and cycle stability of chromium oxide positive electrode. Summary of the invention
[0005] The purpose of the present invention is to solve the problems of low discharge specific capacity, poor rate performance and cycle stability of chromium oxide positive electrode materials, and to provide a core-shell structure chromium oxide positive electrode and a preparation method thereof.
[0006] To achieve the above purpose, the technical solution adopted by the present invention is as follows:
[0007] A core-shell structure chromium oxide positive electrode, the chemical formula of the positive electrode is M x Cr 8-x O 21 -@LLZAO, including doped M x Cr 8-x O 21 The inner core and the garnet electrolyte LLZAO coating shell layer, wherein M is one or more of Zn, Mg, Ca, Ta, Ge, Nb, Sb, Sn, Ti and Ga, and 0≤x≤1.
[0008] Furthermore, the chemical formula of the LLZAO is Li 7-3x La3Zr2Al x O 12 , where 0≤x≤0.3, the thickness of the coating shell depends on LLZAO and M x Cr 8-x O 21 The stoichiometric ratio of the mass ratio is 1 to 10:100.
[0009] A method for preparing the above-mentioned core-shell structure chromium oxide positive electrode, the method comprising:
[0010] S1. Weighing CrO3 powder and doped metal salt raw materials according to a metering ratio, mixing and grinding to make the raw materials evenly dispersed, placing them in a tube furnace, calcining them at high temperature in an oxidizing atmosphere, grinding them after cooling, sieving the powder, washing with water to remove unreacted CrO3, and vacuum drying to obtain the doped chromium oxide active material;
[0011] S2, weighing the doped chromium oxide, surfactant and LLZAO garnet powder according to the metering ratio, mixing and grinding, placing in a tube furnace, calcining at high temperature in an oxidizing atmosphere, grinding after cooling and sieving the powder to obtain M x Cr 8-x O 21 -@LLZAO core-shell structure positive electrode material.
[0012] Furthermore, in step S1, the doping metal salt is one of metal acetate, oxalate, sulfate or nitrate.
[0013] Furthermore, in step S1, the high temperature calcination is carried out at a temperature of 270°C to 300°C, for a time of 12 to 24 hours, and at a heating rate of 1 to 10°C / min.
[0014] Furthermore, in steps S1 and S2, the grinding is planetary ball milling, the ball milling speed is 300-500 rpm, the time is 6-24 hours, and the ball-to-material ratio is 1 / 2-1 / 3.
[0015] Furthermore, in steps S1 and S2, the oxidizing atmosphere is oxygen or air, and the mesh size of the sieving is 400 to 1000 meshes.
[0016] Furthermore, in step S2, the surfactant is one of PVP, PEG, PVA, and SDBS, and the mass ratio of the surfactant to the doped chromium oxide is 1 to 5:100.
[0017] Furthermore, in step S2, the high temperature calcination temperature is 320°C to 400°C, the heating rate is 1 to 10°C / min, and the time is 6 to 24 hours.
[0018] Compared with the prior art, the beneficial results of the present invention are:
[0019] (1) The metal elements doped into the doped chromium oxide core designed in the core-shell structure chromium oxide positive electrode material provided by the present invention include elements from the third period, the fourth period and the fifth period, and also include transition metal elements. The doped elements are of a wide variety and have universal applicability, and can be extended to other lithium-ion battery oxide positive electrode systems for electrode material modification.
[0020] (2) The garnet electrolyte coating layer of the present invention has high mechanical strength, which can inhibit the volume expansion of the chromium oxide positive electrode particles during the cycle, protect the structure of the positive electrode active material particles during the cycle, thereby ensuring the stability of the cycle process. At the same time, it acts as an ion conductor to promote the Li+ transfer between the electrolyte and the positive electrode particles. + transmission efficiency.
[0021] (3) The doping element of the present invention replaces Cr 3+ The sites improve the discharge capacity and rate performance of chromium oxide, and the designed coating stabilizes the electrochemical cycle of the material. This method adopts simple grinding and calcination treatment, which is simple to operate, has obvious effects, and can be easily extended to other battery material modification systems. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 Zn in Example 1 0.75 Cr 7.5 O 21 -First cycle discharge capacity diagram of battery assembled with LLZAO cathode material at 0.047C (30mA / g) and 1C;
[0023] Figure 2 Zn in Example 1 0.75 Cr 7.5 O21 -100-cycle discharge capacity diagram of the battery assembled with LLZAO positive electrode material at 0.047C (30mA / g);
[0024] Figure 3 Cr8O in Comparative Example 1 21 The first cycle discharge specific capacity diagram of the battery assembled with the positive electrode material at 0.047C (30mA / g) and 1C;
[0025] Figure 4 Cr8O in Comparative Example 1 21 100-cycle discharge capacity diagram of the battery assembled with the positive electrode material at 0.047C (30mA / g). DETAILED DESCRIPTION
[0026] The technical scheme of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are only a part of the embodiments of the invention, rather than all the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in the field without making creative work belong to the protection scope of the present invention. If the specific conditions are not specified in the embodiments, they are carried out according to the conventional conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified in the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0027] The present invention introduces Cr 3+ Metal elements with similar ionic radius replace Cr8O 21 The lowest valence state of Cr in the cathode material 3+ , does not destroy Cr8O 21 The LLZAO garnet electrolyte coating layer is introduced to improve the discharge capacity of Li + On the other hand, LLZAO as a coating layer has good mechanical strength, which inhibits the volume expansion of the positive electrode particles during the cycle and protects the structure of the chromium oxide positive electrode material. This core-shell structure modification strategy enables the chromium oxide positive electrode material to have high discharge specific capacity, excellent rate performance and excellent cycle stability.
[0028] Example 1
[0029] Weigh 0.219g of zinc acetate dihydrate and 1g of chromium trioxide, grind for 10 minutes to mix the blocky chromium trioxide and zinc acetate dihydrate evenly, dry grind with a planetary ball mill for 12 hours, the ball mill speed is 400rpm, and the ball-to-material ratio is 1 / 3. The mixed powder after ball milling is placed in a tubular furnace, and high-purity oxygen is introduced into the tubular furnace. The temperature is increased to 270°C at a heating rate of 5°C / min, and the temperature is kept for 12 hours. After cooling to room temperature, it is taken out. The heat-treated sample is ground into uniform fine powder, dispersed in 10ml of deionized water, and magnetically stirred for 10 minutes to fully dissolve the unreacted chromium trioxide and zinc acetate dihydrate in the deionized water. The aqueous solution is removed by suction, and the washing process is repeated three times. The washed material is moved into a vacuum oven and dried at 60°C for 24 hours to remove residual water in the sample to obtain Zn 0.75 Cr 7.5 O 21 Positive electrode material: 0.02g PVP, 0.05g LLZAO and 1g Zn 0.75 Cr 7.5 O 21 The mixture was mixed and ground for 10 min, then planetary ball milled for 6 h, placed in a tube furnace with air atmosphere, heated to 350 °C at a heating rate of 5 °C / min, kept at this temperature for 18 h, cooled to room temperature and taken out to obtain Zn 0.75 Cr 7.5 O 21 -LLZAO.
[0030] Zn 0.75 Cr 7.5 O 21 -LLZAO positive electrode active material, Super P conductive carbon black and PVDF were dissolved in N-methylpyrrolidone (NMP) in a mass ratio of 8:1:1 and stirred for 24 hours. The slurry was coated on the Al current collector with a coater and placed in a vacuum oven and dried at 120°C for 24 hours to obtain a core-shell structure chromium oxide positive electrode. 1M LiPF6+EC / DEC / DMC (1:1:1) was used as the electrolyte, the prepared chromium oxide positive electrode, PP separator and metallic lithium were used as the negative electrode, and a CR2025 button cell was assembled. The charge and discharge performance of the battery was tested at 30mA / g (0.047C) and 1C, and the voltage test range was 1.5-4.5V.
[0031] Example 2
[0032] Weigh 0.030g of magnesium sulfate and 1g of chromium trioxide, grind for 10 minutes to mix the blocky chromium trioxide and magnesium sulfate evenly, dry grind for 12 hours with a planetary ball mill, the ball mill speed is 350rpm, the ball-to-material ratio is 1 / 3, and the mixed powder after ball milling is placed in a tubular furnace. High-purity oxygen is introduced into the tubular furnace, and the temperature is increased to 270°C at a heating rate of 5°C / min. Keep it warm for 12 hours, cool it down to room temperature and take it out. Grind the heat-treated sample into uniform fine powder, disperse it in 10ml of deionized water, and stir it magnetically for 10 minutes to fully dissolve the unreacted chromium trioxide and magnesium sulfate in the deionized water. Filter and remove the aqueous solution, and repeat the washing process three times. Move the washed material into a vacuum oven and dry it at 60°C for 24 hours to remove the residual water in the sample to obtain Mg 0.2 Cr 7.9 O 21 Positive electrode material: 0.02g PVA, 0.1g LLZAO and 1g Mg 0.2 Cr 7.9 O 21 The mixture was mixed and ground for 10 min, then planetary ball milled for 6 h, placed in a tube furnace with air atmosphere, heated to 320 °C at a heating rate of 5 °C / min, kept at this temperature for 12 h, cooled to room temperature and taken out to obtain Mg 0.2 Cr 7.9 O 21 -LLZAO.
[0033] The positive electrode preparation and battery assembly test are the same as in Example 1.
[0034] Example 3
[0035] Weigh 0.081g of calcium acetate and 1g of chromium trioxide, grind for 10 minutes to mix the blocky chromium trioxide and calcium acetate evenly, dry grind for 12 hours with a planetary ball mill, the ball mill speed is 350rpm, and the ball-to-material ratio is 1 / 3. The mixed powder after ball milling is placed in a tubular furnace, and high-purity oxygen is introduced into the tubular furnace. The temperature is increased to 270°C at a heating rate of 5°C / min, and the temperature is kept for 12 hours. After cooling to room temperature, it is taken out. The heat-treated sample is ground into uniform fine powder, dispersed in 10ml of deionized water, and magnetically stirred for 10 minutes to fully dissolve the unreacted chromium trioxide and calcium acetate in the deionized water. The aqueous solution is removed by suction, and the washing process is repeated three times. The washed material is moved into a vacuum oven and dried at 60°C for 24 hours to remove residual water in the sample to obtain Ca 0.4 Cr 7.8 O 21 Positive electrode material: 0.05g SDBS, 0.03g LLZAO and 1g Ca 0.4 Cr 7.8 O 21The mixture was mixed and ground for 10 min, then planetary ball milled for 12 h, placed in a tube furnace, high-purity oxygen was introduced into the tube furnace, and the temperature was increased to 380 ° C at a heating rate of 5 ° C / min, kept at this temperature for 12 h, cooled to room temperature and taken out to obtain Ca 0.4 Cr 7.8 O 21 -LLZAO.
[0036] The positive electrode preparation and battery assembly test are the same as in Example 1.
[0037] Comparative Example 1
[0038] Weigh 1g of chromium trioxide powder, grind it for 10 minutes, place it in a tube furnace, introduce high-purity oxygen, heat it to 270℃ at a heating rate of 10℃ / min, keep it warm for 24 hours, cool it down to room temperature and take it out. Grind the heat-treated sample into uniform fine powder, disperse it in 10ml deionized water, stir it magnetically for 10 minutes to fully dissolve the unreacted chromium trioxide in the deionized water, filter it to remove the aqueous solution, and repeat the washing process three times. Move the washed material into a vacuum oven and dry it at 60℃ for 24 hours to remove the residual water in the sample to obtain pure Cr8O 21 Positive electrode material.
[0039] The positive electrode preparation and battery assembly test are the same as in Example 1.
[0040] Table 1. Comparison of the first cycle discharge capacity and discharge rate of Examples 1 to 3 and Comparative Example 1
[0041]
[0042] Figures 1-2 The discharge capacity and cycle performance of the doped positive electrode material at different rates in Example 1 are shown in FIG. Figure 3-4 Conventional Cr8O 21 Discharge capacity and cycle performance at two rates. 21 The first cycle discharge capacity at 30mA / g (0.047C) is 355mAh / g, and the first cycle discharge capacity at 1C is 287mAh / g, which is much smaller than Cr8O 21 The theoretical discharge capacity of the battery is 642mAh / g. After different doping and coating, the first cycle discharge capacity of the battery in the three embodiments at 30mA / g (0.047C) exceeds 400mAh / g. Under the condition of 1C high rate discharge, it also has an ultra-high discharge capacity of >350mAh / g. At the same time, after 100 cycles, it has a higher specific discharge capacity than Cr8O 21Better cycle stability. It is proved that the preparation method of core-shell structure chromium oxide positive electrode material significantly improves the discharge capacity, rate performance and cycle stability of chromium oxide, which has certain guiding and reference significance for the research and modification of chromium oxide and other oxide positive electrode materials.
[0043] The embodiments described above are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0044] Without departing from the principles of the present invention, several improvements and substitutions made within the technical scope disclosed by the present invention should be included in the protection scope of the present invention.
Claims
1. A core-shell structure chromium oxide positive electrode, characterized in that: The chemical formula of the positive electrode material is M x Cr 8-x O 21 -@LLZAO, including doped M x Cr 8-x O 21 The inner core and the garnet electrolyte LLZAO coating shell layer, wherein M is one or more of Zn, Mg, Ca, Ta, Ge, Nb, Sb, Sn, Ti and Ga, and 0≤x≤1.
2. The core-shell structure chromium oxide positive electrode according to claim 1, characterized in that: The chemical formula of the LLZAO is Li 7-3x La3Zr2Al x O 12 , where 0≤x≤0.3, the thickness of the coating shell depends on LLZAO and M x Cr 8-x O 21 The stoichiometric ratio of the mass ratio is 1 to 10:
100.
3. A method for preparing a core-shell structured chromium oxide positive electrode according to claim 1 or 2, characterized in that: The method is: S1. Weighing CrO3 powder and doped metal salt raw materials according to a metering ratio, mixing and grinding to make the raw materials evenly dispersed, placing them in a tube furnace, calcining them at high temperature in an oxidizing atmosphere, grinding them after cooling, sieving the powder, washing with water to remove unreacted CrO3, and vacuum drying to obtain the doped chromium oxide active material; S2, weighing the doped chromium oxide, surfactant and LLZAO garnet powder according to the metering ratio, mixing and grinding, placing in a tube furnace, calcining at high temperature in an oxidizing atmosphere, grinding after cooling and sieving the powder to obtain M x Cr 8- x O 21 -@LLZAO core-shell structure positive electrode material.
4. The method for preparing a core-shell structured chromium oxide positive electrode according to claim 3, characterized in that: In step S1, the doped metal salt is one of metal acetate, oxalate, sulfate or nitrate.
5. The method for preparing the core-shell structure chromium oxide positive electrode according to claim 3, characterized in that: In step S1, the high temperature calcination temperature is 270°C to 300°C, the time is 12 to 24 hours, and the heating rate is 1 to 10°C / min.
6. The method for preparing a core-shell structured chromium oxide positive electrode according to claim 3, characterized in that: In steps S1 and S2, the grinding is planetary ball milling, the ball milling speed is 300-500 rpm, the time is 6-24 hours, and the ball-to-material ratio is 1 / 2-1 / 3.
7. The method for preparing a core-shell structured chromium oxide positive electrode according to claim 3, characterized in that: In steps S1 and S2, the oxidizing atmosphere is oxygen or air, and the mesh size of the sieving is 400 to 1000 meshes.
8. The method for preparing a core-shell structured chromium oxide positive electrode according to claim 3, characterized in that: In step S2, the surfactant is one of PVP, PEG, PVA, and SDBS, and the mass ratio of the surfactant to the doped chromium oxide is 1 to 5:
100.
9. The method for preparing a core-shell structured chromium oxide positive electrode according to claim 3, characterized in that: In step S2, the high temperature calcination temperature is 320°C to 400°C, the heating rate is 1 to 10°C / min, and the time is 6 to 24 hours.
Citation Information
Patent Citations
Garnet-type ion conductor-coated high-nickel ternary positive electrode material, preparation method and lithium ion battery obtained by preparation
CN109904427A
Composite material and preparation method thereof
CN111816856A
Lithium ion battery positive electrode material and preparation method thereof, lithium ion battery positive electrode and all-solid-state lithium battery
CN113353988A
Positive electrode material and battery comprising same
CN115832252A