Lithium iron phosphate positive pole piece and secondary battery
By using modified pyrrole compounds in the positive electrode material layer of lithium iron phosphate batteries for in situ polymerization, the conductive network and C-N conductive network are formed, and the performance deterioration of lithium iron phosphate batteries under low temperature conditions is solved, and the performance deterioration of lithium iron phosphate batteries is achieved at -20℃ high cycle performance and stable performance at room temperature.
Patent Information
- Application Number
- CN202411194623.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-11-08
AI Technical Summary
Lithium iron phosphate batteries exhibit poor circulation performance under low temperature conditions, especially at -20℃, its discharge capacity accounts for only about 30% of the room temperature, limiting its application in cold areas.
Using a positive electrode material layer including lithium iron phosphate positive electrode active material and modified pyrrole compound, polypyrrole compounds are prepared by in-situ polymerization to form a continuous conductive network, and N elements are introduced to build a C-N conductive network to enhance the conductivity and material contact tightness. , improve low temperature performance.
The circulation performance of lithium iron phosphate batteries at -20℃ is significantly improved, and the good low-temperature performance is ensured, while there is no significant negative impact on the normal temperature circulation performance, enhancing the overall conductivity and stability of the battery.
Smart Images

Figure BDA0005016921680000021 
Figure BDA0005016921680000031 
Figure BDA0005016921680000051
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of batteries, and in particular relates to a lithium iron phosphate positive electrode sheet and a secondary battery. Background Art
[0002] Lithium-ion batteries have been rapidly developed in the fields of plug-in hybrid electric vehicles, electric vehicles and large-scale energy storage devices due to their high energy density and long cycle life. Generally speaking, the performance of lithium-ion batteries is determined by the electrode materials. From the perspective of electrode materials, olivine-type lithium iron phosphate is considered to be one of the most promising cathode materials due to its high operating voltage, high theoretical capacity, low cost and environmental friendliness. In fact, lithium iron phosphate has been successfully used in hybrid vehicles and electric vehicles. However, the low intrinsic electronic conductivity and ion diffusion coefficient of lithium iron phosphate limit its wide application. The low conductivity is due to the lack of mixed valence and the high localization of ferrous or ferric ions caused by the low solubility of lithium iron phosphate and ferric phosphate, while the low lithium ion diffusion rate is due to the one-dimensional diffusion channel formed by lithium ions along the b-axis of the corner-sharing LiO6 octahedron. Therefore, researchers have been seeking ways to improve its electrochemical performance.
[0003] At present, lithium cobalt oxide batteries, ternary material batteries, lithium manganese oxide batteries, and lithium iron phosphate batteries are widely used in the market. Among them, lithium iron phosphate batteries are superior to other types of batteries in terms of electrochemical performance, including reversible capacity, stability, safety, cyclicity, and large current discharge capacity, as well as the price of raw materials. Especially in terms of cycle performance, the capacity retention rate of energy-type lithium iron phosphate batteries can reach more than 80% after 2000 cycles of 1C, which is much higher than that of lithium cobalt oxide batteries, ternary material batteries, and lithium manganese oxide batteries. However, lithium iron phosphate batteries have poor low-temperature performance. Although people have improved the low-temperature performance of lithium iron phosphate through various methods, such as doping with lithium, iron, and even phosphoric acid to improve the ion and electron conductivity, by improving the particle size and morphology of primary or secondary particles to control the effective reaction area, and by adding additional conductive agents to increase electronic conductivity, the inherent characteristics of lithium iron phosphate materials determine that its low-temperature performance is inferior to other positive electrode materials such as lithium manganese oxide. Lithium iron phosphate batteries have begun to be used in different fields. When used at low temperatures, their performance is poor. The discharge capacity at -20°C is only about 30% of that at room temperature, which limits their application in cold regions such as the north.
[0004] Therefore, providing a lithium iron phosphate battery with excellent low temperature performance becomes a problem to be solved. Summary of the invention
[0005] In view of this, the technical problem to be solved by the present invention is to provide a lithium iron phosphate positive electrode plate and a secondary battery. The lithium iron phosphate battery provided by the present invention has excellent low-temperature performance and can still maintain good cycle performance under -20°C conditions.
[0006] The present invention provides a lithium iron phosphate positive electrode plate, comprising a current collector and a positive electrode material layer which are compounded in sequence, wherein the positive electrode material layer comprises a lithium iron phosphate positive electrode active material and a polypyrrole compound, wherein the polypyrrole compound is prepared by in-situ polymerization of modified pyrrole;
[0007] The modified pyrrole has a structure shown in Formula I, Formula II or Formula III:
[0008]
[0009] R1 and R2 are independently selected from H, F, C1-C3 alkyl, substituted C1-C3 alkyl, C2-C4 alkenyl, substituted C2-C4 alkenyl, C2-C4 alkynyl, substituted C2-C4 alkynyl, C2-C4 alkoxy, substituted C2-C4 alkoxy, cyano, nitro, sulfonic acid, phenyl, hydroxyl or trifluoromethyl;
[0010] R3 and R4 are independently selected from hydrogen, F, C1-C3 alkyl, substituted C1-C3 alkyl, C2-C4 alkenyl, substituted C2-C4 alkenyl, C2-C4 alkynyl, substituted C2-C4 alkynyl, C2-C4 alkoxy, substituted C2-C4 alkoxy, trimethylsilyl, nitrogen-containing group or phosphorus-containing group;
[0011] R5 and R6 are independently selected from H, F, C1-C3 alkyl, and substituted C1-C3 alkyl.
[0012] Preferably, in the compound represented by formula I, formula II or formula III:
[0013] In the substituted C1-C3 alkyl, the substituents are independently selected from fluoro, cyano, nitro, methoxy or ethoxy;
[0014] In the substituted C2-C4 alkenyl, the substituents are independently selected from fluoro, cyano, nitro, methoxy or ethoxy;
[0015] In the substituted C2-C4 alkynyl, the substituents are independently selected from fluoro, cyano, nitro, methoxy or ethoxy;
[0016] In the substituted C2-C4 alkoxy group, the substituents are independently selected from fluoro, cyano, nitro, methoxy or ethoxy.
[0017] Preferably, R1 and R2 are independently selected from hydrogen, fluorine substituted C1-C3 alkyl;
[0018] R3 and R4 are independently selected from hydrogen, cyano-substituted C1-C3 alkyl, trimethylsilyl;
[0019] R5 and R6 are independently selected from H, F and methyl.
[0020] Preferably, the modified pyrrole is selected from one or more compounds having the following structures:
[0021]
[0022] Preferably, the positive electrode material layer includes a lithium iron phosphate active material layer and in-situ layers on both sides of the lithium iron phosphate active material layer;
[0023] The lithium iron phosphate active material layer includes a lithium iron phosphate positive electrode active material, a conductive agent and a binder, and a polypyrrole compound filled in the gaps between the positive electrode active material, the conductive agent and the binder;
[0024] The in-situ layer includes a conductive agent, a binder, and a polypyrrole compound filled in the gap between the conductive agent and the binder;
[0025] The thickness of the in-situ layer is 3-47 nm, and the thickness of the positive electrode material layer is 130±1 μm.
[0026] Preferably, the method for preparing the positive electrode material layer comprises the following steps:
[0027] Mixing lithium iron phosphate positive electrode active material, conductive agent, binder and modified pyrrole to obtain slurry;
[0028] After the slurry is coated on the surface of the positive electrode current collector, a polymerization reaction of the modified pyrrole is carried out in the presence of an initiator to obtain a polymerized electrode sheet;
[0029] Finally, the polymerized electrode is dried to obtain a positive electrode.
[0030] Preferably, the initiator is selected from (NH4)2S2O8.
[0031] Preferably, the polymerization reaction temperature is 50-100° C., and the polymerization reaction time is 1-12 hours.
[0032] Preferably, the mass ratio of the lithium iron phosphate positive electrode active material, the conductive agent, the binder and the modified pyrrole is 94-96.5:1.5-3:2-3:0.1-2.
[0033] The present invention also provides a secondary battery, comprising the above-mentioned positive electrode plate.
[0034] Compared with the prior art, the present invention provides a lithium iron phosphate positive electrode plate, including a current collector and a positive electrode material layer which are compounded in sequence, wherein the positive electrode material layer includes a lithium iron phosphate positive electrode active material and a polypyrrole compound, wherein the polypyrrole compound is prepared by in-situ polymerization of modified pyrrole. The polypyrrole compound is filled in the gaps between the main raw materials of the positive electrode material layer to form a continuous conductive network, and the in-situ polymerization is carried out between the lithium iron phosphate positive electrode active materials to increase the contact area of the conductive network and improve the conductive effect. Furthermore, the conductive network generated in situ by pyrrole polymerization introduces the N element to construct a CN conductive network. It is found through actual tests that the introduction of the N element can further increase the conductivity. The main reason for the poor low-temperature performance of LFP is that the material has poor low-temperature conductivity, weak ion conductivity, and the contact between the materials inside the plate in the low-temperature state is not tight, the transmission distance is long, and the battery polarization is large. After adding the in-situ polymer, the material is in close contact, the conductive distance is reduced, the conductive capacity is improved, and the overall low-temperature performance is improved. By in-situ polymerization of the polypyrrole compound in the gaps in the positive electrode material layer, the expansion of the material during the cycle process can be reduced, the conductivity of the positive electrode material during the low-temperature cycle process can be improved, and the low-temperature performance of the battery can be improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 This is a schematic structural diagram of the positive electrode material layer provided by the present invention. DETAILED DESCRIPTION
[0036] The present invention provides a lithium iron phosphate positive electrode plate, comprising a current collector and a positive electrode material layer which are compounded in sequence, wherein the positive electrode material layer comprises a lithium iron phosphate positive electrode active material and a polypyrrole compound, wherein the polypyrrole compound is prepared by in-situ polymerization of modified pyrrole;
[0037] The modified pyrrole has a structure shown in Formula I or Formula II:
[0038]
[0039] R1 and R2 are independently selected from H, F, C1-C3 alkyl, substituted C1-C3 alkyl, C2-C4 alkenyl, substituted C2-C4 alkenyl, C2-C4 alkynyl, substituted C2-C4 alkynyl, C2-C4 alkoxy, substituted C2-C4 alkoxy, cyano, nitro, sulfonic acid, phenyl, hydroxyl or trifluoromethyl;
[0040] Preferably, in the substituted C1~C3 alkyl, the substituents are independently selected from fluoro, cyano, nitro, methoxy or ethoxy; in the substituted C2~C4 alkenyl, the substituents are independently selected from fluoro, cyano, nitro, methoxy or ethoxy; in the substituted C2~C4 alkynyl, the substituents are independently selected from fluoro, cyano, nitro, methoxy or ethoxy; in the substituted C2~C4 alkoxy, the substituents are independently selected from fluoro, cyano, nitro, methoxy or ethoxy.
[0041] More preferably, R1 and R2 are independently selected from hydrogen and fluorine-substituted C1-C3 alkyl; even more preferably, R1 and R2 are independently selected from hydrogen and fluorinated ethyl.
[0042] In the present invention, the carbon chain length at the position of R1 is 2 to 3 carbon atoms longer than the carbon length at the position of R, so as to ensure that the modified pyrrole maintains the polarity of the polypyrrole after polymerization and improve the adhesion between the polypyrrole and the positive and negative electrodes. If the carbon chain length at the position of R1 is more than 3 carbon atoms longer than the carbon length at the position of R, the ring formed after in-situ polymerization is too large, the bond is easily broken, the chemical stability is poor, and the problem of disordered growth of the in-situ layer is brought about.
[0043] R3 and R4 are independently selected from hydrogen, F, C1-C3 alkyl, substituted C1-C3 alkyl, C2-C4 alkenyl, substituted C2-C4 alkenyl, C2-C4 alkynyl, substituted C2-C4 alkynyl, C2-C4 alkoxy, substituted C2-C4 alkoxy, trimethylsilyl, nitrogen-containing group or phosphorus-containing group.
[0044] Preferably, in the substituted C1~C3 alkyl, the substituents are independently selected from fluoro, cyano, nitro, methoxy or ethoxy; in the substituted C2~C4 alkenyl, the substituents are independently selected from fluoro, cyano, nitro, methoxy or ethoxy; in the substituted C2~C4 alkynyl, the substituents are independently selected from fluoro, cyano, nitro, methoxy or ethoxy; in the substituted C2~C4 alkoxy, the substituents are independently selected from fluoro, cyano, nitro, methoxy or ethoxy.
[0045] More preferably, R3 and R4 are independently selected from hydrogen, cyano-substituted C1-C3 alkyl, and trimethylsilyl. Further preferably, R3 and R4 are independently selected from hydrogen, cyano-substituted methyl, and trimethylsilyl.
[0046] R5 and R6 are independently selected from H, F, C1-C3 alkyl, substituted C1-C3 alkyl, preferably, in the substituted C1-C3 alkyl, the substituent is independently selected from fluoro, cyano, nitro, methoxy or ethoxy; more preferably, R5 and R6 are independently selected from H, F or methyl.
[0047] In some specific embodiments of the present invention, the modified pyrrole is selected from one or more compounds having the following structures:
[0048]
[0049]
[0050] In the present invention, the positive electrode material layer includes a lithium iron phosphate active material layer and in-situ layers on both sides of the lithium iron phosphate active material layer;
[0051] The lithium iron phosphate active material layer includes a lithium iron phosphate positive electrode active material, a conductive agent and a binder, and a polypyrrole compound filled in the gaps between the positive electrode active material, the conductive agent and the binder;
[0052] The in-situ layer includes a conductive agent, a binder, and a polypyrrole compound filled in the gap between the conductive agent and the binder;
[0053] The thickness of the in-situ layer is 3 to 47 nm, and can be 3, 5, 7, 9, 10, 15, 20, 25, 30, 35, 40, 45, 47, or any value between 3 and 47 nm. The thickness of the positive electrode material layer is 130±1 μm.
[0054] See also Figure 1 , Figure 1 This is a schematic structural diagram of the positive electrode material layer provided by the present invention. Figure 1 In the figure, T1 is the lithium iron phosphate active material layer, T2 is the positive electrode material layer, and the portion of T2 beyond the edges of both sides of T1 is the in-situ layer.
[0055] In the present invention, the polypyrrole compound is filled in the gaps of the main raw materials of the positive electrode material layer to form a continuous conductive network, and the in-situ polymerization is carried out between the lithium iron phosphate positive electrode active materials to increase the contact area and improve the conductive effect. Further, the conductive network generated in situ by pyrrole polymerization introduces the N element to construct a CN conductive network. Through actual testing, it is found that the introduction of the N element can further increase the conductivity. The in-situ layer has brittleness, rigidity and elasticity, and the subsequent rolling of the pole piece will cause the problem of crushing, and the extrusion of the material will cause the problem of material crushing. The polymerization in the coating process completes the shaping in the liquid stage, and the subsequent rolling deformation is less affected. The present invention can ensure the thickness of the in-situ layer by selecting a specific type of polypyrrole compound. The greater the thickness of the in-situ layer, the higher the internal resistance of the battery, and the greater the impact on the performance of the normal temperature cycle. The polypyrrole compound mentioned in the present invention has a high degree of polymerization and a stable polymerization process. The polymerization time can be controlled to be evenly distributed between the active materials of the positive electrode sheet, and the internal resistance of the battery is less affected, ensuring low-temperature circulation while not affecting the normal temperature circulation.
[0056] In the present invention, the positive electrode active material is a lithium iron phosphate positive electrode active material.
[0057] The conductive agent is selected from C-containing materials such as conductive carbon black (SP), carbon nanotubes (CNT), and graphene (Gr);
[0058] The binder is selected from one or more of polyvinylidene fluoride (PVDF), aqueous binder styrene butadiene rubber (SBR) emulsion and carboxymethyl cellulose (CMC), polyacrylic acid (PAA), polyacrylonitrile (PAN) and polyacrylate (ABR).
[0059] The thickness of the positive electrode material layer is 30-50 nm, and can be 30, 35, 40, 45, 50, or any value between 30 and 50 nm.
[0060] The method for preparing the positive electrode material layer comprises the following steps:
[0061] Mixing lithium iron phosphate positive electrode active material, conductive agent, binder and modified pyrrole to obtain slurry;
[0062] After the slurry is coated on the surface of the positive electrode current collector, a polymerization reaction of the modified pyrrole is carried out in the presence of an initiator to obtain a polymerized electrode sheet;
[0063] Finally, the polymerized electrode is dried to obtain a positive electrode.
[0064] Specifically, the present invention first prepares a slurry, and there is no particular limitation on the mixing method, and any mixing method known to those skilled in the art can be used. Preferably, a solvent is used in advance to prepare a 5wt% PVDF N-methylpyrrolidone (NMP) slurry, which is then mixed with a conductive agent, a positive electrode active material, and modified pyrrole to prepare a slurry.
[0065] After obtaining the slurry, the slurry is applied to the positive electrode fluid on a positive electrode coating machine. After the coating is completed, the modified pyrrole is initiated to undergo a polymerization reaction through an initiator device containing an initiator atmosphere to generate a carbon-containing polymer.
[0066] Wherein, the initiator atmosphere is a gasified initiator (NH4)2S2O8.
[0067] The polymerization reaction temperature is 50-100°C, and can be 50, 55, 60, 65, 70, 75, 80, 85, 90, 95, 100, or any value between 50 and 100°C. The polymerization reaction time is 1 to 12h, and can be 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, or any value between 1 and 12h.
[0068] The mass ratio of the lithium iron phosphate positive electrode active material to the modified pyrrole is 94-96.5:0.1-2, and can be 96.3:0.2, 96:0.5, 95.5:1, 94.5:2, or any value between 94-96.5:0.1-2.
[0069] In some specific embodiments of the present invention, the raw materials for preparing the positive electrode material layer include:
[0070] 94 to 96.5 parts of positive electrode active material;
[0071] 1.5 to 3 parts of conductive agent;
[0072] 2-3 parts of adhesive;
[0073] 0.1 to 2 parts of modified pyrrole.
[0074] The raw materials for preparing the positive electrode material layer provided by the present invention include 94 to 96.5 parts of positive electrode active materials, which can be 94, 94.5, 95, 95.5, 96, 96.5, or any value between 94 and 96.5 parts of positive electrode active materials; the positive electrode active material is preferably a lithium iron phosphate positive electrode active material.
[0075] The raw materials for preparing the positive electrode material layer provided by the present invention also include 1.5 to 3 parts of a conductive agent, which can be 1.5, 2, 2.5, 3, or any value between 1.5 and 3 parts. The present invention has no special restrictions on the type of the conductive agent, and any type of conductive agent known to those skilled in the art can be used. The conductive agent is preferably carbon nanotubes or conductive carbon black.
[0076] The raw materials for preparing the positive electrode material layer provided by the present invention also include 2 to 3 parts of a binder, which can be 2, 2.2, 2.4, 2.5, 2.6, 2.8, 3, or any value between 2 and 3 parts. The present invention has no special restrictions on the type of the binder, and any type of binder known to those skilled in the art can be used. The binder is selected from PVDF.
[0077] The raw material for preparing the positive electrode material layer provided by the present invention also includes 0.1 to 2 parts of modified pyrrole, which can be 0.1, 0.2, 0.4, 0.5, 0.6, 0.8, 1, 1.2, 1.4, 1.5, 1.6, 1.8, 2, or any value between 0.1 and 2 parts. The modified pyrrole is selected from the modified pyrrole described above.
[0078] In the present invention, the polymerization reaction equation is as follows:
[0079] The synthetic structural formula of formula I
[0080]
[0081] The synthetic structural formula of formula II
[0082]
[0083] The synthetic structural formula of formula III
[0084]
[0085] After the polymerization reaction is completed, a polymerized electrode will be obtained;
[0086] Next, the polymerized electrode is dried, rolled and die-cut to obtain a positive electrode.
[0087] The present invention also provides a secondary battery, comprising a positive electrode, a negative electrode, a separator and an electrolyte, wherein the positive electrode is the positive electrode sheet.
[0088] The negative electrode active material in the negative electrode includes one or more materials such as graphite and silicon carbon. The present invention has no special restrictions on the preparation method of the negative electrode, and the preparation method of the negative electrode known to those skilled in the art can be used. Preferably, the active material, the conductive agent, the binder, and the thickener are fully stirred and mixed in a deionized water solvent system in a certain proportion to obtain a negative electrode slurry, and the negative electrode slurry is coated on the current collector, and the negative electrode sheet is obtained after slitting, rolling, and die cutting, and the compaction density is 1.65g / cm 3 ;
[0089] The present invention does not limit the specific selection of the diaphragm. The diaphragms that can be used in batteries in the prior art are all suitable for constructing the lithium supplement diaphragm of the present invention, and should be reasonably selected and adjusted according to actual needs. For example, the diaphragm includes PE diaphragm (polyethylene diaphragm), PP diaphragm (polypropylene diaphragm), Al2O3 coated PP diaphragm (Al2O3 thickness 2μm, PP diaphragm 9μm), PVDF coated diaphragm (structure: Al2O3 / PVDF glue / PP diaphragm / Al2O3; Al2O3 thickness 1μm, PVDF glue 2μm, PP diaphragm 12μm, Al2O3 thickness 1μm)
[0090] The electrolyte is composed of an organic solvent, a lithium salt and an additive, wherein the organic solvent is at least one of dimethyl carbonate, ethyl methyl carbonate, methyl propyl carbonate, diethyl carbonate, ethylene carbonate, propylene carbonate, butylene carbonate, ethyl formate, ethyl acetate, ethyl propionate, ethyl butyrate, methyl propionate and tetrahydrofuran. The lithium salt electrolyte includes at least one of lithium fluoride, lithium nitrate, lithium hexafluorophosphate, lithium tetrafluoroborate, lithium bis(trifluoromethanesulfonyl)imide, lithium bis(fluorosulfonyl)imide, lithium bis(oxalate borate), lithium difluorooxalate borate and lithium difluorophosphate. The additive is selected from a film-forming additive and may be at least one of vinyl sulfate, vinylene carbonate, propylene sulfite, fluoroethylene carbonate, cyclohexylbenzene and vinyl ethylene carbonate. .
[0091] In order to further understand the present invention, the lithium iron phosphate positive electrode sheet and a secondary battery provided by the present invention are described below in conjunction with embodiments. The protection scope of the present invention is not limited by the following embodiments.
[0092] In the following examples, the initiator atmosphere is the gasified initiator (NH4)2S2O8.
[0093] Example 1
[0094] There are many literature references on the synthesis of pyrrole derivatives, which will not be elaborated here.
[0095] Prepare lithium iron phosphate positive electrode: CNT: PVDF: SP: pyrrole A-1 = 96.3%: 0.5%: 2%: 1%: 0.2% ratio of mixing, PVDF using 5% NMP slurry prepared in advance, the prepared slurry is coated on the positive electrode coater, after coating, through the initiator containing the initiator atmosphere, the modified pyrrole is initiated to polymerize to generate a carbon-nitrogen polymer conductive network, the initiation temperature is 45 ° C, the polymerization time is 1H, after the polymerization is completed, the electrode continues to pass through the drying room, after the electrode is dried, it is rolled and die-cut, the final electrode rolling thickness is maintained at 143μm, the upper and lower error fluctuations of 1μm.
[0096] According to SEM detection, the thickness of the in-situ polymerized conductive layer on the surface of the positive electrode is about 15nm, with an upper and lower error fluctuation of 2nm.
[0097] Example 2
[0098] Prepare lithium iron phosphate positive electrode: CNT: PVDF: SP: pyrrole A-1: = 96%: 0.5%: 2%: 1%: 0.5% ratio is mixed, PVDF uses 5% NMP slurry prepared in advance, the prepared slurry is coated on the positive electrode coater, after coating, the modified pyrrole is initiated to polymerize through an initiator containing an initiator atmosphere to generate a carbon-nitrogen polymer conductive network, the initiation temperature is 80°C, the polymerization time is 6H, after the polymerization is completed, the electrode continues to pass through the drying room, after the electrode is dried, it is rolled and die-cut, and the final rolled thickness of the electrode is maintained at 143μm, with an upper and lower error fluctuation of 1μm.
[0099] According to SEM detection, the thickness of the in-situ polymerized carbon layer on the surface of the positive electrode is about 20nm, with an upper and lower error fluctuation of 2nm.
[0100] Example 3
[0101] Prepare lithium iron phosphate positive electrode: CNT: PVDF: SP: pyrrole A-1 = 95.5%: 0.5%: 2%: 1%: 1% ratio of mixing, PVDF using 5% NMP slurry prepared in advance, the prepared slurry is coated on the positive electrode coater, after coating, through the initiator containing the initiator atmosphere, the modified pyrrole is initiated to polymerize to generate a carbon-nitrogen polymer conductive network, the initiation temperature is 100 ° C, the polymerization time is 12 hours, after the polymerization is completed, the electrode continues to pass through the drying room, after the electrode is dried, it is rolled and die-cut, the final electrode rolling thickness is maintained at 143μm, the upper and lower error fluctuations of 1μm.
[0102] According to SEM detection, the thickness of the in-situ polymerized carbon layer on the surface of the positive electrode is about 10nm, with an upper and lower error fluctuation of 2nm.
[0103] Example 4
[0104] Prepare lithium iron phosphate positive electrode: CNT: PVDF: SP: pyrrole A-1 = 94.5%: 0.5%: 2%: 1%: 2% ratio of mixing, PVDF using 5% NMP slurry prepared in advance, the prepared slurry is coated on the positive electrode coater, after coating, through the initiator containing the initiator atmosphere, the modified pyrrole is initiated to polymerize to form a carbon nitrogen polymer conductive network, the initiation temperature is 45 ° C, the polymerization time is 12 hours, after the polymerization is completed, the electrode continues to pass through the drying room, after the electrode is dried, it is rolled and die-cut, the final electrode rolling thickness is maintained at 143μm, the upper and lower error fluctuations of 1μm.
[0105] According to SEM detection, the thickness of the in-situ polymerized carbon layer on the surface of the positive electrode is about 30nm, with an upper and lower error fluctuation of 2nm.
[0106] Example 5
[0107] Prepare lithium iron phosphate positive electrode: CNT: PVDF: SP: pyrrole A-2 = 96%: 0.5%: 2%: 1%: 0.5% ratio of mixing, PVDF using 5% NMP slurry prepared in advance, the prepared slurry is coated on the positive electrode coater, after coating, through the initiator containing the initiator atmosphere, the modified pyrrole is initiated to polymerize to generate a carbon-nitrogen polymer conductive network, the initiation temperature is 45 ° C, the polymerization time is 6 hours, after the polymerization is completed, the electrode continues to pass through the drying room, after the electrode is dried, it is rolled and die-cut, the final electrode rolling thickness is maintained at 143μm, the upper and lower error fluctuations of 1μm.
[0108] According to SEM detection, the thickness of the in-situ polymerized carbon layer on the surface of the positive electrode is about 30nm, with an upper and lower error fluctuation of 2nm.
[0109] Example 6
[0110] Prepare lithium iron phosphate positive electrode: CNT: PVDF: SP: pyrrole A-3 = 96%: 0.5%: 2%: 1%: 0.5% ratio of mixing, PVDF using 5% NMP slurry prepared in advance, the prepared slurry is coated on the positive electrode coater, after coating, through the initiator containing the initiator atmosphere, the modified pyrrole is initiated to polymerize to generate a carbon-nitrogen polymer conductive network, the initiation temperature is 45 ° C, the polymerization time is 6 hours, after the polymerization is completed, the electrode continues to pass through the drying room, after the electrode is dried, it is rolled and die-cut, the final electrode rolling thickness is maintained at 143μm, the upper and lower error fluctuations of 1μm.
[0111] According to SEM detection, the thickness of the in-situ polymerized carbon layer on the surface of the positive electrode is about 5nm, which is reasonably suspected to be the polypyrrole conductive layer. The degree of in-situ polymerization is low, with an upper and lower error fluctuation of 2nm.
[0112] Example 7
[0113] Prepare lithium iron phosphate positive electrode: CNT: PVDF: SP: pyrrole A-4 = 96%: 0.5%: 2%: 1%: 0.5% ratio of mixing, PVDF using 5% NMP slurry prepared in advance, the prepared slurry is coated on the positive electrode coater, after coating, through the initiator containing the initiator atmosphere, the modified pyrrole is initiated to polymerize to generate a carbon nitrogen polymer conductive network, the initiation temperature is 45 ° C, the polymerization time is 6 hours, after the polymerization is completed, the electrode continues to pass through the drying room, after the electrode is dried, it is rolled and die-cut, the final electrode rolling thickness is maintained at 143μm, the upper and lower error fluctuations of 1μm.
[0114] According to SEM detection, the thickness of the in-situ polymerized carbon layer on the surface of the positive electrode is about 40nm, with an upper and lower error fluctuation of 2nm.
[0115] Example 8
[0116] Prepare lithium iron phosphate positive electrode: CNT: PVDF: SP: pyrrole A-5 = 96%: 0.5%: 2%: 1%: 0.5% ratio of mixing, PVDF using 5% NMP slurry prepared in advance, the prepared slurry is coated on the positive electrode coater, after coating, through the initiator containing the initiator atmosphere, the modified pyrrole is initiated to polymerize to generate a carbon-nitrogen polymer conductive network, the initiation temperature is 45 ° C, the polymerization time is 6 hours, after the polymerization is completed, the electrode continues to pass through the drying room, after the electrode is dried, it is rolled and die-cut, the final electrode rolling thickness is maintained at 143μm, the upper and lower error fluctuations of 1μm.
[0117] SEM detection shows that the thickness of the in-situ polymerized carbon layer on the surface of the positive electrode is about 30nm. SEM and DES tests show that there is a small amount of Si-containing substance in the outer layer of the in-situ polymerized layer. The thickness of the Si-containing layer is about 1-2nm, and the overall in-situ polymerized layer fluctuates by 2nm.
[0118] Example 9
[0119] Prepare lithium iron phosphate positive electrode: CNT: PVDF: SP: pyrrole A-6 = 96%: 0.5%: 2%: 1%: 0.5% ratio of mixing, PVDF using 5% NMP slurry prepared in advance, the prepared slurry is coated on the positive electrode coater, after coating, through the initiator containing the initiator atmosphere, the modified pyrrole is initiated to polymerize to generate a carbon nitrogen polymer conductive network, the initiation temperature is 45 ° C, the polymerization time is 6 hours, after the polymerization is completed, the electrode continues to pass through the drying room, after the electrode is dried, it is rolled and die-cut, the final electrode rolling thickness is maintained at 143μm, the upper and lower error fluctuations of 1μm.
[0120] According to SEM detection, the thickness of the in-situ polymerized carbon layer on the surface of the positive electrode is about 45nm, with an upper and lower error fluctuation of 2nm.
[0121] Comparative Example 1
[0122] Preparation of lithium iron phosphate positive electrode: CNT: PVDF: SP: unmodified pyrrole = 96%: 0.5%: 2%: 1%: 0.5% ratio of mixing, PVDF using 5% NMP slurry prepared in advance, the prepared slurry is coated on the positive electrode coater, after coating, through the initiator containing the initiator atmosphere, the modified pyrrole is initiated to polymerize to form a carbon-nitrogen polymer conductive network, the initiation temperature is 45 ° C, the polymerization time is 6 hours, after the polymerization is completed, the electrode continues to pass through the drying room, after the electrode is dried, it is rolled and die-cut, the final electrode rolling thickness is maintained at 143μm, the upper and lower error fluctuations of 1μm.
[0123] According to SEM detection, the thickness of the in-situ polymerized carbon layer on the surface of the positive electrode is about 30nm, with an upper and lower error fluctuation of 2nm.
[0124] Comparative Example 2
[0125] Prepare lithium iron phosphate positive electrode: CNT: PVDF: SP = 96.5%: 0.5%: 2%: 1% ratio of mixing, PVDF using 5% NMP slurry prepared in advance, the prepared slurry is coated on the positive electrode coater, after coating, through the initiator containing the initiator atmosphere, the modified pyrrole is initiated to polymerize, to generate a carbon nitrogen polymer conductive network, the initiation temperature is 45 ° C, the polymerization time is 6 hours, after the polymerization is completed, the electrode continues to pass through the drying room, after the electrode is dried, it is rolled and die-cut, the final electrode rolling thickness is maintained at 143μm, the upper and lower error fluctuations of 1μm.
[0126] According to SEM detection, the thickness of the in-situ polymerized carbon layer on the surface of the positive electrode is about 30nm, with an upper and lower error fluctuation of 2nm.
[0127] Comparative Example 3
[0128] Step 1: In-situ polymerization of LFP material
[0129] Lithium iron phosphate positive electrode material with D50 = 8.7 μm was mixed with pyrrole at a mass ratio of 1:0.05 and heated in a tube furnace at a heating temperature of 45 °C and a heating rate of 1 °C / min. (NH4)2S2O was continuously introduced during the reaction. 8, The reaction time was 6 hours, and the reaction products were collected and crushed for the second time and pulverized to finally obtain in-situ polymerized lithium iron phosphate with a D50 of about 9.5 μm. SEM observation showed that some particles of LFP were broken due to the crushing operation.
[0130] Step 2: Polymerized LFP cathode preparation
[0131] In-situ polymerized lithium iron phosphate: CNT: PVDF: SP = 96.5%: 0.5%: 2%: 1% ratio is mixed, PVDF uses 5% NMP slurry prepared in advance, the prepared slurry is coated on the positive electrode coater, after coating is completed, it passes through the drying room, the electrode is dried, and then rolled and die-cut. The final rolled thickness of the electrode is maintained at 143μm, with an upper and lower error fluctuation of 1μm.
[0132] SEM examination showed that no smooth in-situ polymerized conductive layer was observed on the surface of the positive electrode sheet, and due to the rolling pressure, cracks appeared in the in-situ layer on the surface of the LFP positive electrode material.
[0133] Comparative Example 4
[0134] Step 1: Prepare LFP cathode
[0135] Prepare lithium iron phosphate positive electrode: CNT: PVDF: SP = 96.5%: 0.5%: 2%: 1% ratio of mixing, PVDF using 5% NMP slurry prepared in advance, the prepared slurry is coated on the positive electrode coater, after coating, through the initiator containing the initiator atmosphere, the modified pyrrole is initiated to polymerize, to generate a carbon nitrogen polymer conductive network, the initiation temperature is 45 ° C, the polymerization time is 6 hours, after the polymerization is completed, the electrode continues to pass through the drying room, after the electrode is dried, it is rolled and die-cut, the final electrode rolling thickness is maintained at 143μm, the upper and lower error fluctuations of 1μm.
[0136] Step 2: In-situ polymerization of LFP positive electrode surface
[0137] The prepared positive electrode plate is coated for the second time on the positive electrode coater, that is, after coating, modified pyrrole is sprayed on the surface of the plate, and then the modified pyrrole is polymerized through an initiator device containing an initiator atmosphere to generate a carbon-nitrogen polymer conductive network. The initiation temperature is 45°C and the polymerization time is 1H. After the polymerization is completed, the plate continues to pass through the drying room. After the plate is dried, it is rolled and die-cut. The final rolled thickness of the plate is maintained at 143μm, with an upper and lower error fluctuation of 1μm.
[0138] According to SEM detection, the thickness of the in-situ polymerized conductive layer on the surface of the positive electrode is about 1μm, with an upper and lower error fluctuation of 50nm.
[0139] The preparation and testing methods of lithium batteries are as follows:
[0140] (1) Highly compacted artificial natural composite graphite was selected as the negative electrode material, and graphite, CMC, conductive agent, and binder were mixed evenly in a ratio of 94:1:3:2 to prepare a negative electrode sheet with a compaction density of 1.65 g / cm3, which was subsequently used for testing;
[0141] (2) The positive and negative electrode sheets are stacked to form soft-pack batteries, and the electrolytes prepared in Examples 1-9 and Comparative Examples 1-4 are injected into the batteries. After formation and capacity separation, the electrical performance of the batteries is tested at a low temperature of -20°C. Three soft packs are taken for each test, and the test results are averaged.
[0142] The specific test method is as follows:
[0143] After the soft pack is filled with liquid, the rated capacity is 2.5Ah and the filling coefficient is 6g / Ah. After the filling, it is formed, aged, and divided. After standing, a three-gram soft pack with a similar capacity is selected to calculate the first effect, test the internal resistance and open-circuit voltage, and then transferred to a constant temperature test room with a fixture, a voltage range of 2.5-3.65V, and a 1C cycle test for 500 weeks.
[0144] The battery is formed according to the following steps: 0.1C constant current charging to 3.0V, 0.2C constant current charging to 3.3V, the formed battery is first aged, then vacuum sealed, and then capacity divided according to the following steps: 0.5C constant current discharge to 2.5V, 0.5C constant current constant voltage charging to 3.65V, constant current discharge to 2.5V, cross-current charging to 3.3V, first effect = (constant current discharge total capacity / constant current constant voltage charging capacity + formation charging capacity) * 100%.
[0145] The test results are shown in Table 1 below:
[0146] Table 1
[0147]
[0148]
[0149] Through the analysis of the electrochemical test data of Examples 1-4, it was found that the in-situ layer of pyrrole derivatives and dopamine hydrochloride was a carbon-containing polymer with a thickness of about 10-30 nm. This part of the polymer has a relatively large relationship with the reactant ratio, polymerization temperature, and polymerization time. After experimental verification, it was found that the polymer obtained under the reaction conditions of Example 4 had obvious performance advantages in subsequent electrochemical tests. It is speculated that the main reason is that the relatively thick carbon-containing polymer (i.e., the in-situ layer) greatly improved the conductivity of the positive electrode material during the low-temperature test, alleviating the problem of poor low-temperature conductivity of the LFP material. In addition, according to the above examples, the reaction conditions of the subsequent pyrrole derivatives were determined to continue the reaction conditions of Example 4.
[0150] By comparing Example 4 with Comparative Examples 1 and 2, it can be found that the electrochemical performance of the carbon-containing polymer formed by the pyrrole derivative of the additive after polymerization is significantly improved compared with the normal pyrrole and the polypyrrole layer formed by dopamine hydrochloride and the comparative example 2 without adding pyrrole. The main reason is speculated to be that the in-situ cured polymer is significantly superior to polypyrrole and the comparative example 2 without conductive material in terms of ion transport and conductivity. In summary, the pyrrole derivative A-1 is better than pyrrole for low-temperature cycles.
[0151] By comparing Example 4 with Example 5, it can be found that although the capacity retention rate of the pyrrole derivative A-2 introduced with -CN is relatively close to that of A-1 in Example 4 in the low-temperature discharge stage, the impedance of the SEI film formed due to the unsaturated bond brought by the cyano group is relatively high, and it is obviously not as good as the performance of the pyrrole derivative A-1 in the DCR and room temperature cycle stages. In summary, the introduction of cyano groups has a relatively general effect on the improvement of low-temperature performance.
[0152] By comparing Example 4 with Example 6, it can be found that the capacity retention rate of the low-temperature discharge stage of the pyrrole derivative A-3 without double bonds is significantly lower than that of the derivative A-1. It is speculated that the distribution of the in-situ polymer is not uniform enough, resulting in significantly worse conductivity than that of Example 4. In addition, by comparing Example 6 with Comparative Example 1, it can be found that the pyrrole polymer without any treatment has obvious performance differences compared with the pyrrole polymer containing asymmetric carbon chains. It is speculated that the in-situ polymer with asymmetric carbon chains has a larger polarity and a stronger electron transmission ability, which brings relatively excellent conductivity and improves low-temperature cycle performance.
[0153] By comparing Example 4 with Example 7, it can be found that the asymmetric long chain of the pyrrole derivative is lengthened and the F-containing group is introduced, resulting in a higher DCR value of the soft pack in Example 7. In the subsequent normal temperature cycle process, the battery may generate more heat, and some solvents or additives may decompose at high temperature, resulting in relatively poor performance at both normal temperature and low temperature cycles. Therefore, the long chain of the pyrrole derivative should be subject to certain restrictions, and the increase in chain length will affect the overall internal resistance of the soft pack.
[0154] By comparing Example 4 with Example 8, the main purpose of introducing trimethylsilyl groups into the pyrrole derivative A-5 is to generate a layer of Si-containing inorganic layer material outside the in-situ polymerization layer, so as to increase the contact tightness between the in-situ polymerization layer and the positive and negative electrodes and the diaphragm, and make the electron transmission closer. It was later found that after the silicate layer material was formed outside the in-situ layer, the irregularity of the silicate layer affected the shape of the in-situ polymerization layer to a certain extent, resulting in serious lithium precipitation in the low-temperature cycle stage, which ultimately affected the subsequent low-temperature cycle performance.
[0155] By comparing Example 4 with Example 9, the pyrrole derivative A-6 undergoes a ring-forming reaction at the R1 and R2 positions in the general formula, satisfying the original design that R1 has 2-3 more carbons than R2. Finally, it is found that the derivative A-6 has the same problem as the derivative A-3. After the carbon chain length or carbon content increases, the overall resistance of the soft package is affected, which affects the normal temperature cycle. Therefore, the comprehensive performance cannot be compared with the pyrrole derivative A-1. However, by comparing the derivative A-6 with Comparative Examples 1 or 2, it can still be found that the modified pyrrole derivative of this patent is significantly better than the comparative example in both normal temperature cycle and low temperature cycle.
[0156] Through the data analysis of Comparative Example 2, Comparative Example 1 and Example 2, it can be found that directly carrying out in-situ polymerization on the material surface and then coating the positive electrode plate has advantages in terms of first effect and capacity performance. It is speculated that the active contact area increased due to material breakage, the lithium insertion and extraction ratio was optimized, and the number was increased, resulting in the soft package showing an increase in first effect and capacity. However, in the later room temperature cycle test, it was found that due to material breakage, the contact area increased, and the side reactions intensified, resulting in a decrease in the later cycle retention rate. In the low-temperature cycle test, it was found that the capacity retention rate decreased, but it was better than that of Comparative Example 1 without adding pyrrole, indicating that the carbon-nitrogen conductive network constructed by pyrrole will improve the low-temperature performance, but due to the breakage of the material, the overall performance is not as good as Example 2.
[0157] Through the data analysis of Comparative Example 4 and Comparative Example 1, it can be found that directly adding an in-situ conductive layer on the surface of the LFP pole piece in the later stage has basically no obvious effect on the improvement of low-temperature cycling, and the 500-week cycle retention rate is only increased by about 2%. In addition, since the thickness of the conductive layer is relatively thick, and there is no conductive connection structure between the internal materials of the pole piece, the membrane impedance of the soft-pack battery is ultimately increased, and the capacity retention rate is reduced in the normal temperature cycle stage. Taking all factors into consideration, the solution of coating the in-situ conductive layer on the outside of the LFP positive electrode has certain differences in performance compared with the solution of this patent.
[0158] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A lithium iron phosphate positive electrode plate, characterized in that: It comprises a current collector and a positive electrode material layer which are compounded in sequence, wherein the positive electrode material layer comprises a lithium iron phosphate positive electrode active material and a polypyrrole compound, wherein the polypyrrole compound is prepared by in-situ polymerization of modified pyrrole; The modified pyrrole has a structure shown in Formula I, Formula II or Formula III: R1 and R2 are independently selected from H, F, C1-C3 alkyl, substituted C1-C3 alkyl, C2-C4 alkenyl, substituted C2-C4 alkenyl, C2-C4 alkynyl, substituted C2-C4 alkynyl, C2-C4 alkoxy, substituted C2-C4 alkoxy, cyano, nitro, sulfonic acid, phenyl, hydroxyl or trifluoromethyl; R3 and R4 are independently selected from hydrogen, F, C1-C3 alkyl, substituted C1-C3 alkyl, C2-C4 alkenyl, substituted C2-C4 alkenyl, C2-C4 alkynyl, substituted C2-C4 alkynyl, C2-C4 alkoxy, substituted C2-C4 alkoxy, trimethylsilyl, nitrogen-containing group or phosphorus-containing group; R5 and R6 are independently selected from H, F, C1-C3 alkyl, and substituted C1-C3 alkyl.
2. The positive electrode sheet according to claim 1, characterized in that: In the compound of the structure shown in Formula I, Formula II or Formula III: In the substituted C1-C3 alkyl, the substituents are independently selected from fluoro, cyano, nitro, methoxy or ethoxy; In the substituted C2-C4 alkenyl, the substituents are independently selected from fluoro, cyano, nitro, methoxy or ethoxy; In the substituted C2-C4 alkynyl, the substituents are independently selected from fluoro, cyano, nitro, methoxy or ethoxy; In the substituted C2-C4 alkoxy group, the substituents are independently selected from fluoro, cyano, nitro, methoxy or ethoxy.
3. The positive electrode sheet according to claim 1, characterized in that: R1 and R2 are independently selected from hydrogen and fluorine substituted C1-C3 alkyl groups; R3 and R4 are independently selected from hydrogen, cyano-substituted C1-C3 alkyl, trimethylsilyl; R5 and R6 are independently selected from H, F and methyl.
4. The positive electrode sheet according to claim 1, characterized in that: The modified pyrrole is selected from one or more compounds having the following structures:
5. The positive electrode sheet according to claim 1, characterized in that: The positive electrode material layer includes a lithium iron phosphate active material layer and in-situ layers on both sides of the lithium iron phosphate active material layer; The lithium iron phosphate active material layer includes a lithium iron phosphate positive electrode active material, a conductive agent and a binder, and a polypyrrole compound filled in the gaps between the positive electrode active material, the conductive agent and the binder; The in-situ layer includes a conductive agent, a binder, and a polypyrrole compound filled in the gap between the conductive agent and the binder; The thickness of the in-situ layer is 3-47 nm, and the thickness of the positive electrode material layer is 130±1 μm.
6. The positive electrode sheet according to claim 1, characterized in that: The method for preparing the positive electrode material layer comprises the following steps: Mixing lithium iron phosphate positive electrode active material, conductive agent, binder and modified pyrrole to obtain slurry; After the slurry is coated on the surface of the positive electrode current collector, a polymerization reaction of the modified pyrrole is carried out in the presence of an initiator to obtain a polymerized electrode sheet; Finally, the polymerized electrode is dried to obtain a positive electrode.
7. The positive electrode sheet according to claim 6, characterized in that: The initiator is selected from (NH4)2S2O8.
8. The positive electrode sheet according to claim 6, characterized in that: The polymerization reaction temperature is 50-100° C., and the polymerization reaction time is 1-12 hours.
9. The positive electrode sheet according to claim 6, characterized in that: The mass ratio of the lithium iron phosphate positive electrode active material, the conductive agent, the binder and the modified pyrrole is 94-96.5:1.5-3:2-3:0.1-2.
10. A secondary battery, characterized in that: The invention comprises the positive electrode sheet as described in any one of claims 1 to 9.
Citation Information
Cited By
Lithium iron phosphate material as well as preparation method and application thereof
CN120622452A