Preparation method and application of dry-process self-supporting membrane with low binder content and high toughness
By using micron-level conductive passivator and multi-level structural conductive material in the dry self-supporting film, the conductive network is formed, and the problem of insufficient toughness and conductivity caused by low adhesive content is solved, and the diaphragm is significantly improved Mechanical and electrical properties.
Patent Information
- Application Number
- CN202411016533.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-28
- Publication Date
- 2024-11-08
AI Technical Summary
When the binder content of the existing dry self-support film is low, the toughness and electronic conductivity are insufficient, which affects the forming and performance of the electrode film.
The adhesive passivation treatment is carried out by micron-level conductive passivation agent, and the three-dimensional bonding network structure is formed through airflow crushing and hot rolling processes, combining sheet, granular and fibrous nanoconductive materials with multi-level structures. Conductive network to improve the toughness and electrical properties of the diaphragm.
The maximum fracture tensile strength and electrical conductivity of the dry self-supporting film are significantly improved, the contact impedance between the electrode active particles is reduced, and the mechanical and electrical properties of the diaphragm are enhanced.
Smart Images

Figure CN118919660A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of battery preparation, and in particular to a method for preparing a dry-process self-supporting film with low binder content and high toughness and application thereof. Background Art
[0002] The scale manufacturing technology of lithium-ion batteries (power batteries, energy storage batteries) and sodium-ion batteries mainly adopts the traditional wet process. The dry process is a comprehensive upgrade of the traditional wet process. In the manufacturing process, the dry process has fewer technical steps, lower manufacturing costs and energy consumption, and the raw materials are environmentally friendly and more suitable for large-scale production; in terms of battery performance, dry batteries can achieve higher energy density, and the battery's electrical and mechanical properties are better; in the application end, dry batteries are more suitable for the manufacturing needs of new generation batteries such as solid-state batteries and 4680.
[0003] However, in the process of preparing electrodes by dry process, the binder exists in a fibrous state. The higher the binder content, the stronger the bonding force of the membrane, which can more firmly combine the active material with other inactive materials, and promote the conduction of lithium ions at the interface. However, the binder does not have electronic conductivity, which is not conducive to the electronic conduction of the electrode. Therefore, the amount of binder added needs to be reduced, but too low an amount of binder added affects the difficulty of forming and the toughness of the electrode during the preparation of the membrane; in addition, conductive materials need to be added to improve the electronic conductivity of the membrane. The morphology, amount and order of addition of the conductive material have an important influence on the final state of the material. Therefore, the amount of binder added, the fibrous state and the amount of conductive agent added are very critical to the forming and performance of the membrane.
[0004] In summary, it is very important to prepare a dry self-supporting membrane with low binder content, strong toughness, high electronic conductivity and good fiberization degree.
[0005] Patent CN 117038866 A discloses a dry self-supporting membrane and its preparation method and application. The preparation method obtains the above-mentioned dry self-supporting membrane by reasonably regulating the mixing process and the membrane calendering process. The thickness of the dry self-supporting membrane is 50-70 microns, which is smaller than the traditional thickness and has a small resistance range, which can improve the cycle stability of the assembled battery. However, the dry self-supporting membrane obtained in this patent, with the total mass of active materials, conductive agents and binders as 100%, the active materials account for 90-96%, and the rest are conductive agents and binders, for example, the conductive agent accounts for 1-6%, and the binder accounts for 1-5%. However, the patent has the following problems: the overall proportion of the conductive agent and binder in the obtained self-supporting membrane is 4-10%, and it is believed that the dry self-supporting membrane prepared only by regulating the mixing process is limited in improving the ion transport performance and the tensile strength of the membrane. Summary of the invention
[0006] In view of the technical problems existing in the prior art, the present invention proposes a method for preparing a dry self-supporting film with low binder content and strong toughness and its application, so as to improve the structural strength and electrical properties of the self-supporting film.
[0007] In order to achieve the above object, the technical solution of the present invention is achieved as follows: A method for preparing a dry self-supporting film with low binder content and high toughness comprises the following steps: (1) Mixing the active material and the conductive material uniformly; (2) passivating the binder with a conductive passivator in micron-sized particles to obtain a passivated binder; (3) Mix the materials obtained in step (1) and step 2 and stir again to make them uniform; (4) grinding the material after the treatment in step (3) by air flow, and then performing a heating treatment; (5) The material after the heat treatment in step (4) is subjected to hot roller pressing to obtain a dry self-supporting membrane.
[0008] The electrode active material in step (1) is a positive electrode active material or a negative electrode active material; the positive electrode active material mainly includes LiMxO2 (M=Co, Ni, Mn), LiMn2O4, LiFePO4, LiNi 1–y–z Mn y Co z O2 (NMC) (y, z are arbitrary values from 0 to 1), LiMnPO4, LiCoPO4, Li3V2(PO4)3, Na x MO2 (M is a transition metal atom, 0<X≤1), Na x M1[M2(CN)6] (M is a transition metal atom, such as Mn, Ni, Co, Zn, Cu and Fe, 0<x≤2), etc., Na x M y (XaOb) z Z w (M is a transition metal atom, X is phosphorus, sulfur, tungsten, etc., and Z is F, OH, etc.); the negative electrode active materials mainly include graphite, carbon-based materials hard carbon, soft carbon, amorphous carbon, etc.
[0009] The conductive material is a fibrous conductive material or a lamellar conductive material; the fibrous conductive material includes flexible metal fibers, flexible vapor grown carbon fibers (VGCF) or flexible carbon nanotubes (CNTs); the lamellar conductive material includes rigid micron conductive graphite or graphene (GN); the conductive graphite is preferably SFG series and KS series.
[0010] In step (2), the conductive passivating agent is carbon black (CB) and metal powder; the carbon black (CB) includes rigid micron-sized conductive graphite, Super-P (SP), acetylene black (AB) or Ketjen black (KB); the binder is a combination of a non-fiberized particle binder and a fiberizable binder; The passivation process is to accelerate the stirring of the binder and the conductive passivator together; the stirring parameters are: 1) the revolution speed is 500-700 rpm, the time is 5-15 min, and the revolution speed ratio is 65-75%; 2) the revolution speed is 1200-1800 rpm, the time is 5-15 min, and the revolution speed ratio is 70-90%.
[0011] The raw materials of the dry self-supporting film have the following mass percentages: electrode active material 99-92wt%; binder 0.5-5wt%; conductive passivator 0.4-2wt%; conductive material 0.1-1wt%; the mass ratio of non-fibrous particle binder to fiberized binder is 0-2:0.5-5; the conductive passivator covers more than 90% of the surface area of the binder particles, and the covering thickness is 0.1-1000μm.
[0012] The non-fibrous particle binder is any one or more of polyvinyl pyrrolidone (PVP), polyethylene glycol (PEG), polyvinylidene fluoride (PVDF), thermoplastic polyamide (PA), suspended polytetrafluoroethylene (PTFE) and its modified products, cellulose, cellulose acetate (CA), methyl cellulose (MC), ethyl cellulose (EC), hydroxypropyl cellulose (HPC), hydroxyethyl cellulose (HEC), nitrocellulose (CN), carboxymethyl cellulose (CMC), carboxyethyl cellulose (CEC), carboxypropyl cellulose, carboxymethyl isopropyl cellulose, sodium cellulose, sodium nitrocellulose and sodium carboxyalkyl cellulose.
[0013] The fiberizable binder is any one or more of polytetrafluoroethylene (PTFE) or its modified substance, polyvinylidene fluoride (PVDF) or its modified substance, ethylene-tetrafluoroethylene copolymer (E-TFE), polyvinylidene fluoride (PVDF), styrene-butadiene rubber, polyethylene oxide, poly(vinylidene fluoride-hexafluoropropylene), polyacrylonitrile (PAN), (methyl) polyacrylonitrile, polyacrylic acid (PAA), polymethyl methacrylate (PMMA), modified polymethyl methacrylate and polystyrene (PS).
[0014] The mixing and stirring in step (3) includes the following steps: 1) the revolution speed is 100-3000rpm, the time is not less than 5min, and the revolution speed ratio is 50%-200%; 2) the revolution speed is 600rpm-3000rpm, the time is not less than 15min, and the revolution speed ratio is 30%-150%; 3) the revolution speed is 600rpm-3000rpm, the time is not less than 10min, and the revolution speed ratio is 50%-200%.
[0015] In the step (4), the air flow pressure of the air flow pulverization is 0.2-0.8 MPa; the feeding pressure of the air flow pulverization is greater than the pulverization pressure; the temperature of the heating treatment is 40-80° C., and the time is 60-180 min.
[0016] The hot rolling process in step (5) is as follows: the pressure is 1 to 100 tons; the temperature is 60 to 180° C.; the gap between the hot rolling rollers is 0 to 2 mm, and the hot rolling is performed 2 to 3 times.
[0017] The dry self-supporting film with low binder content and strong toughness prepared by the above method has a maximum tensile strength at break of not less than 1Mpa; the maximum tensile strength at break of the dry self-supporting film is greater than 3Mpa; preferably, the maximum tensile strength at break of the dry self-supporting film is 3-6Mpa; the thickness is 30-500μm; the surface of the film is uniform, smooth, without curling, holes, wrinkles, cracks, pits, protrusions, dark marks, black spots, linear marks and other defects; A self-supporting membrane electrode pole piece is formed by hot pressing and compounding the above-mentioned dry process self-supporting membrane and foil current collector, and the temperature of the hot roller is 100-200°C.
[0018] The present invention has the following beneficial effects: (1) The total amount of binder in the present invention is not more than 5%. The advantage is that the fiberized binder and the non-fibrous binder are interwoven to form a three-dimensional bonding network structure, which can not only achieve a more uniform distribution of the active substances in the electrode membrane, but more importantly, the non-fibrous binder has stronger adhesion, thereby improving the maximum tensile strength of the dry self-supporting membrane.
[0019] (2) This is because the present invention uses a multi-level structure of flaky, granular, and fibrous nano-conductive materials as additives to prevent the fiberized materials from agglomerating, stratifying, segregating, and bridging during the production and transportation process.
[0020] (3) In the present invention, the conductive passivator is passivated in the binder, and the passivation layer acts as a conductor to enhance the conductivity of the active material, which not only improves the stability of the binder, but also inhibits the decomposition of the electrolyte. Even after the binder is fibrillated, the passivation layer will still adhere to the surface of the binder due to the interaction between molecules, thereby enhancing the electronic conduction channel and improving the conductivity of the membrane.
[0021] (4) The zero-dimensional conductive passivator (KB, SP, Cabot, etc.) in the present invention has a small particle size and can contact the active particle material in a point-to-point manner; the one-dimensional conductive material (CNTs, carbon fiber, etc.) has a large aspect ratio and can contact the active material particles in a point-to-line manner. During the dispersion process, it can form a entangled cross-linked network structure, forming a large number of conductive contact sites between the active particles, thereby reducing the contact impedance between the active particles of the electrode; adding a conductive agent between the active materials can reduce the internal resistance of the battery, especially when a composite conductive agent composed of multiple phases is added, a "point, line, and surface" transport conductive network can be constructed between the active particles and the conductive agent, forming a synergistic, complementary, and stimulating effect, which can greatly improve the conductive effect. In addition, the linear shape of the one-dimensional conductive material can also enhance the toughness and strength of the diaphragm.
[0022] (5) The present invention adopts heating treatment to reduce the unevenness in the first two mixing processes and greatly reduce the molding defect problem of the fibrous network structure in the step-by-step hot pressing process. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0024] Figure 1 Flow chart for the preparation of dry self-supporting electrode sheets.
[0025] Figure 2 This is the picture after the adhesive is passivated.
[0026] Figure 3 This is the picture after the air flow crushing treatment of Example 1.
[0027] Figure 4 This is the picture after the air flow crushing treatment of Example 2.
[0028] Figure 5 This is the picture after air flow crushing treatment of Comparative Example 1.
[0029] Figure 6 This is the picture after air flow crushing treatment of comparative example 2.
[0030] Figure 7 This is the picture after air flow crushing treatment of comparative example 3.
[0031] Figure 8 This is the picture after air flow crushing treatment of comparative example 4.
[0032] Fig. 9 This is a scanning electron microscope image of the cross section of the dry-process self-supporting membrane obtained in Example 1.
[0033] Fig.10 This is a scanning electron microscope image of the cross section of the dry-process self-supporting membrane obtained in Example 2.
[0034] Fig.11 This is a scanning electron microscope image of the cross section of the dry-process self-supporting membrane obtained in Comparative Example 3.
[0035] Fig.12 This is a scanning electron microscope image of the cross section of the dry self-supporting membrane obtained in Comparative Example 4.
[0036] Fig.13 It is a tensile strength test diagram of Examples 1-2 and Comparative Examples 1-4.
[0037] Fig.14 These are resistivity test diagrams of Examples 1-2 and Comparative Examples 1-4. DETAILED DESCRIPTION
[0038] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0039] Example 1 The self-supporting membrane of this embodiment is composed of the following components in mass ratio: Active material NCM811: fiberizable binder PTFE: conductive passivator SP: fibrous conductive material VGCF=95:4:0.8:0.2.
[0040] The membrane preparation method is as follows Figure 1 As shown, the specific steps are: (1) The active material NCM811 and the conductive material are mixed uniformly by high shear: 1) the revolution speed is 300 rpm, the time is 5 min, and the revolution speed ratio is 0.7; 2) the revolution speed is 1000 rpm, the time is 10 min, and the revolution speed ratio is 80%; (2) Passivation treatment of the binder: The binder and the conductive passivator are stirred together at an accelerated speed: the stirring parameters are: 1) revolution speed 600 rpm, time 10 min, revolution speed ratio 70%; 2) revolution speed 1500 rpm, time 10 min, revolution speed ratio 80%; the picture of the binder after passivation is as follows Figure 2 As shown; (3) The materials in (1) and (2) are uniformly stirred and mixed: 1) the revolution speed is 1000 rpm, the time is 10 min, and the revolution speed ratio is 100%; 2) the revolution speed is 2000 rpm, the time is 15 min, and the revolution speed ratio is 120%; 3) the revolution speed is 1500 rpm, the time is 10 min, and the revolution speed ratio is 120%.
[0041] (4) The material in (3) was subjected to air flow pulverization, with the feed air flow pressure of 0.6 MPa, the pulverization pressure of 0.4 MPa, and the feed rate of 10 kg / h. After air flow pulverization, the scanning electron microscope showed that Figure 3 As shown; (5) Keep the material in (4) at 60°C for 1 h; (6) The material in (5) was subjected to step-by-step hot roller pressing: the rolling temperature was 100°C, the rolling thickness was 140±5 μm, and a dry self-supporting film was prepared.
[0042] Example 2 This embodiment provides a self-supporting membrane, which is different from Embodiment 1 in that the raw materials and mass ratio are different. The mass ratio of the raw materials is: active substance NCM811: fiberizable binder PTFE: non-fiberizable binder PVP: conductive passivator KB: fibrous conductive material CNTS = 97.25:0.5:0.25:0.5:1.
[0043] The remaining preparation steps are the same as those in Example 1.
[0044] Comparative Example 1 This comparative example provides a self-supporting membrane, which is different from Example 1 in that no conductive material is added. The specific raw material composition mass ratio is: active substance NCM811: fiberizable binder PTFE: conductive passivator SP = 95:4:1. Except for the step of adding the conductive material, the other steps are the same as Example 1 to prepare a dry self-supporting membrane.
[0045] Comparative Example 2 This comparative example provides a self-supporting membrane, which is different from Example 1 in that the binder is not passivated. The specific raw material composition mass ratio is: active substance NCM811: fiberizable binder PTFE: conductive material VGCF = 95:4:1. Except for the binder passivation step, the other steps are the same as Example 1 to prepare a dry self-supporting membrane.
[0046] Comparative Example 3 This comparative example provides a self-supporting membrane, which is different from Example 2 in that no conductive material is added, and the specific raw material composition mass ratio is: active substance NCM811: fiberizable binder PTFE: non-fiberizable binder PVP: conductive passivator KB = 97.25:0.5:0.25:1.5.
[0047] Except for the step of adding the conductive material, the remaining steps are the same as those in Example 2 to prepare a dry process self-supporting membrane.
[0048] Comparative Example 4 This comparative example provides a self-supporting membrane, which differs from Example 2 in that no conductive passivator is added, and the specific raw material composition mass ratio is: active substance NCM811: fiberizable binder PTFE: non-fibrous particle binder PVP: fibrous conductive material CNTS = 97.25:0.5:0.25:1.5.
[0049] Except for the step of adding the conductive passivating agent for passivation, the remaining steps are the same as those in Example 2 to prepare a dry process self-supporting membrane.
[0050] Figure 3 and Figure 4 These are pictures of the fiberized materials after airflow pulverization in Example 1 and Example 2. It can be seen that the materials are "flocculated", with obvious fibrous substances and a certain viscosity, which indicates that the binder is fiberized; Figure 5-8 The figures respectively correspond to the materials after the airflow pulverization treatment of comparative examples 1 to 4, except that Figure 5 and Figure 7 It can be seen that the material is in the form of large "lumps", and there is a certain degree of viscosity between the large "lumps". Figure 6 and Figure 8 The "lump" is smaller, with more and more obvious fiber strands; Fig. 9 and Fig.10 The cross-sectional SEM images of the self-supporting films of Example 1 and Example 2 respectively show that a high content of binder or a high content of fibrous conductive material is conducive to forming a good three-dimensional cross-linked network in the film. The fiber filaments are relatively long and have no breaks in the middle. The fiber filaments tightly connect the active particles and the conductive agent to form an electrode film. The most obvious thing is that many fine conductive carbon black particles are connected in series in the fiber filaments, which greatly enhances the electronic conduction effect of the electrode. Fig.11 and Fig.12 These are the cross-sectional SEM images of the self-supporting membranes of Comparative Example 3 and Comparative Example 4, from which it can be seen that the fiber distribution is relatively sparse, the active material particles and the fibrous material are distributed separately, and cannot penetrate well to form a network structure.
[0051] Fig.13 The following is a graph showing the tensile strength test data of the dry-process self-supporting films obtained in Examples 1 and 2 and Comparative Examples 1-4. The test standard refers to the test standard GB / T 36363-2018 for polyolefin separators for lithium-ion batteries. The sample length is 60 mm, the gauge length is 50 mm, the width is 15 mm, and the thickness is 155 ± 3 μm. As shown in the figure, the dry-process self-supporting films obtained in Examples 1 and 2 have high tensile strength (5 Mpa) and elongation at break (about 14 mm), and the mechanical properties of the films are good; the dry-process self-supporting films obtained in Comparative Examples 1-4 have low fracture strength (less than 3 Mpa) and elongation at break (less than 10 mm); Fig.14 The resistivity test graph of the dry-process self-supporting film obtained in the comparative examples is shown in FIG. 1. The binders of Example 1 and Example 2 are passivated and a conductive material is added. The conductivity of the obtained dry-process self-supporting film is very small, about 25 mΩ / cm, while the resistivity of Comparative Examples 1-4 is about 300 mΩ / cm or more; The passivation layer formed by the conductive passivator on the bonding surface will still adhere to the surface of the adhesive due to the interaction force between molecules, thereby enhancing the electronic conductive channel and improving the conductivity of the membrane. In the present invention, a multi-level structured nano-conductive material is used as an additive to prevent the fiberized material from agglomerating, stratifying, segregating, and bridging during the production and transportation process.
[0052] Zero-dimensional conductive passivators (KB, SP, Cabot, etc.) have a small particle size and can contact the electrode active particle material in a point-to-point manner; one-dimensional conductive materials (CNTs, carbon fiber, etc.) have a large aspect ratio and can contact the active material particles in a point-to-line manner. During the dispersion process, they can form a tangled cross-linked network structure, forming a large number of conductive contact sites between the active particles, thereby reducing the contact impedance between the electrode active particles; adding a conductive agent between the active materials can reduce the internal resistance of the battery, especially when a composite conductive agent composed of multiple phases is added, a "point, line, and surface" transport conductive network can be constructed between the active particles and the conductive agent, forming a synergistic, complementary, and stimulating effect that can greatly improve the conductive effect. In addition, the linear shape of the one-dimensional conductive material can also enhance the toughness and strength of the diaphragm.
[0053] Example 3 The self-supporting membrane of this embodiment is composed of the following components in mass ratio: Active material NCM811: fibrillable binder polyethylene oxide: non-fibrillable binder PEG: conductive passivator AB: fibrous conductive material CNTs = 92:3:2:2:1.
[0054] The steps of the membrane preparation method are as follows: (1) The active material NCM811 and the conductive material are mixed uniformly by high shear: 1) the revolution speed is 300 rpm, the time is 5 min, and the revolution speed ratio is 0.7; 2) the revolution speed is 1000 rpm, the time is 10 min, and the revolution speed ratio is 80%; (2) Passivating the binder: accelerating stirring of the binder and the conductive passivator: stirring parameters are: 1) revolution speed 600 rpm, time 10 min, revolution speed ratio 70%; 2) revolution speed 1500 rpm, time 10 min, revolution speed ratio 80%; (3) The materials in (1) and (2) are uniformly stirred and mixed: 1) the revolution speed is 100 rpm, the time is 60 min, and the revolution speed ratio is 50%; 2) the revolution speed is 3000 rpm, the time is 15 min, and the revolution speed ratio is 30%; 3) the revolution speed is 600 rpm, the time is 40 min, and the revolution speed ratio is 300%.
[0055] (4) The material in (3) was subjected to air flow pulverization, with the feed air flow pressure of 0.8 MPa, the pulverizing pressure of 0.4 MPa, and the feed rate of 10 kg / h; (5) Keep the material in (4) at a high temperature of 60°C for 3 hours; (6) The material in (5) was subjected to step-by-step hot roller pressing: the rolling temperature was 180°C, the rolling thickness was 140±5 μm, and a dry self-supporting film was prepared.
[0056] Example 4 The self-supporting membrane of this embodiment is composed of the following components in mass ratio: Active material NCM811: fiberizable binder PAN: conductive passivator KB: fibrous conductive material flexible metal fiber copper = 99: 0.5: 0.1: 0.4.
[0057] The steps of the membrane preparation method are as follows: (1) The active material NCM811 and the conductive material are mixed uniformly by high shear: 1) the revolution speed is 300 rpm, the time is 5 min, and the revolution speed ratio is 0.7; 2) the revolution speed is 1000 rpm, the time is 10 min, and the revolution speed ratio is 80%; (2) Passivating the binder: accelerating stirring of the binder and the conductive passivator: stirring parameters are: 1) revolution speed 600 rpm, time 10 min, revolution speed ratio 70%; 2) revolution speed 1500 rpm, time 10 min, revolution speed ratio 80%; (3) The materials in (1) and (2) are uniformly stirred and mixed: 1) the revolution speed is 3000 rpm, the time is 5 min, and the revolution speed ratio is 200%; 2) the revolution speed is 600 rpm, the time is 90 min, and the revolution speed ratio is 150%; 3) the revolution speed is 3000 rpm, the time is 10 min, and the revolution speed ratio is 50%.
[0058] (4) The material in (3) is subjected to air flow pulverization, the feed air flow pressure is 0.2 Mpa, and the pulverization pressure is 0.2 Mpa; (5) Keep the material in (4) at 80°C for 6 hours; (6) The material in (5) was subjected to step-by-step hot roller pressing: the rolling temperature was 60°C, the rolling thickness was 140±5 μm, and a dry self-supporting film was prepared.
[0059] Example 5 The self-supporting membrane of this embodiment is composed of the following components in mass ratio: Active material NCM811: fiberizable binder styrene-butadiene rubber: non-fiberizable particle binder PA: conductive passivator metal powder copper powder: fibrous conductive material flexible metal fiber copper fiber = 98:0.2:0.5:0.3:1.
[0060] The steps of the membrane preparation method are as follows: (1) The active material NCM811 and the conductive material are mixed uniformly by high shear: 1) the revolution speed is 300 rpm, the time is 5 min, and the revolution speed ratio is 0.7; 2) the revolution speed is 1000 rpm, the time is 10 min, and the revolution speed ratio is 80%; (2) Passivating the binder: accelerating stirring of the binder and the conductive passivator: stirring parameters are: 1) revolution speed 500 rpm, time 15 min, revolution speed ratio 75%; 2) revolution speed 1800 rpm, time 15 min, revolution speed ratio 90%; (3) The materials in (1) and (2) are uniformly stirred and mixed: 1) the revolution speed is 3000 rpm, the time is 5 min, and the revolution speed ratio is 200%; 2) the revolution speed is 600 rpm, the time is 90 min, and the revolution speed ratio is 150%; 3) the revolution speed is 3000 rpm, the time is 10 min, and the revolution speed ratio is 50%.
[0061] (4) The material in (3) is subjected to air flow pulverization, the feed air flow pressure is 0.2 MPa, and the pulverization pressure is 0.2 MPa; (5) Keep the material in (4) at 80°C for 6 hours; (6) The material in (5) was subjected to step-by-step hot roller pressing: the rolling temperature was 60°C, the rolling thickness was 140±5 μm, and a dry self-supporting film was prepared.
[0062] Example 6 The self-supporting membrane of this embodiment is composed of the following components in mass ratio: Active material NCM811: fibrillable binder PMMA: non-fiberized particle binder HEC: conductive passivator KB: fibrous conductive material VGCF = 96:1:1:1:1.
[0063] The steps of the membrane preparation method are as follows: (1) The active material NCM811 and the conductive material are mixed uniformly by high shear: 1) the revolution speed is 300 rpm, the time is 5 min, and the revolution speed ratio is 0.7; 2) the revolution speed is 1000 rpm, the time is 10 min, and the revolution speed ratio is 80%; (2) Passivating the binder: accelerating stirring of the binder and the conductive passivator: stirring parameters are: 1) revolution speed 500 rpm, time 15 min, revolution speed ratio 75%; 2) revolution speed 1800 rpm, time 15 min, revolution speed ratio 90%; (3) The materials in (1) and (2) are uniformly stirred and mixed: 1) the revolution speed is 3000 rpm, the time is 5 min, and the revolution speed ratio is 200%; 2) the revolution speed is 600 rpm, the time is 90 min, and the revolution speed ratio is 150%; 3) the revolution speed is 3000 rpm, the time is 10 min, and the revolution speed ratio is 50%.
[0064] (4) The material in (3) is subjected to air flow pulverization, the feed air flow pressure is 0.2 MPa, and the pulverization pressure is 0.2 MPa; (5) Keep the material in (4) at 80°C for 6 hours; The material in (5) was subjected to step-by-step hot rolling: the rolling temperature was 60° C., the rolling thickness was 140±5 μm, and a dry self-supporting film was prepared.
[0065] Example 7 The self-supporting membrane of this embodiment is composed of the following components in mass ratio: Active material NCM811: fiberizable binder PAA: non-fiberizable binder CMC: conductive passivator AB: fibrous conductive material CNTs = 92:3:2:2:1.
[0066] The steps of the membrane preparation method are as follows: (1) The active material NCM811 and the conductive material are mixed uniformly by high shear: 1) the revolution speed is 300 rpm, the time is 5 min, and the revolution speed ratio is 0.7; 2) the revolution speed is 1000 rpm, the time is 10 min, and the revolution speed ratio is 80%; (2) Passivating the binder: accelerating stirring of the binder and the conductive passivator: stirring parameters are: 1) revolution speed 600 rpm, time 10 min, revolution speed ratio 70%; 2) revolution speed 1500 rpm, time 10 min, revolution speed ratio 80%; (3) The materials in (1) and (2) are uniformly stirred and mixed: 1) the revolution speed is 100 rpm, the time is 60 min, and the revolution speed ratio is 50%; 2) the revolution speed is 3000 rpm, the time is 15 min, and the revolution speed ratio is 30%; 3) the revolution speed is 600 rpm, the time is 40 min, and the revolution speed ratio is 300%.
[0067] (4) The material in (3) was subjected to air flow pulverization, with the feed air flow pressure of 0.8 MPa, the pulverizing pressure of 0.4 MPa, and the feed rate of 10 kg / h; (5) Keep the material in (4) at a high temperature of 60°C for 3 hours; (6) The material in (5) was subjected to step-by-step hot roller pressing: the rolling temperature was 180°C, the rolling thickness was 140±5 μm, and a dry self-supporting film was prepared.
[0068] Application Example 1 The dry self-supporting film obtained in Example 1 and the current collector foil are simultaneously fed into a hot pressing roller. Under the action of hot pressing, the film is bonded to the surface of the foil to form a dry self-supporting film electrode. The temperature of the hot roller is 100-200°C and the thickness of the film is 30-500μm.
[0069] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a dry self-supporting film with low binder content and strong toughness, It is characterized in that The steps include: (1) Mixing the active material and the conductive material uniformly; (2) passivating the binder with a conductive passivator in micron-sized particles to obtain a passivated binder; (3) mixing the materials obtained in step (1) and step 2 and stirring them again to make them uniform; (4) grinding the material after the treatment in step (3) by air flow, and then performing a heating treatment; (5) The material after the heat treatment in step (4) is subjected to hot roller pressing to obtain a dry self-supporting membrane.
2. The method for preparing a dry self-supporting film with low binder content and high toughness according to claim 1, It is characterized in that In step (1), the electrode active material is a positive electrode active material or a negative electrode active material; the conductive material is a fibrous conductive material or a lamellar conductive material; the fibrous conductive material is a flexible metal fiber, a flexible vapor-grown carbon fiber or a flexible carbon nanotube; the lamellar conductive material includes rigid micron conductive graphite or graphene; In step (2), the conductive passivator is carbon black powder or metal powder, and the carbon black powder includes conductive graphite, Super-P, acetylene black or Ketjen black; the binder is a combination of a non-fibrous particle binder and a fibrillable binder.
3. The method for preparing a dry self-supporting film with low binder content and high toughness according to claim 2, It is characterized in that The weight percentages of the raw materials of the dry self-supporting film are: 99-92wt% electrode active material; 0.5-5wt% binder; 0.4-2wt% passivator; 0.1-1wt% conductive material; the mass ratio of non-fibrous particle binder to fibrillable binder is 0-2:0.5-5; the passivator covers more than 90% of the surface area of the binder particles, and the coverage thickness is 0.1-1000μm.
4. The method for preparing a dry self-supporting film with low binder content and high toughness according to claim 2, It is characterized in that The non-fibrous particle binder is any one or more of polyvinyl pyrrolidone, polyethylene glycol, polyvinylidene fluoride, thermoplastic polyamide, suspended polytetrafluoroethylene and modified products thereof or cellulose and its derivatives; cellulose derivatives are cellulose acetate, methyl cellulose, ethyl cellulose, hydroxypropyl cellulose, hydroxyethyl cellulose, nitrocellulose, carboxymethyl cellulose, carboxyethyl cellulose, carboxypropyl cellulose, carboxymethyl isopropyl cellulose, sodium cellulose, sodium nitrate cellulose or sodium carboxyalkyl cellulose.
5. The method for preparing a dry self-supporting film with low binder content and high toughness according to claim 2, It is characterized in that The fiberizable binder is any one or more of polyfluoroethylene or its modified product, styrene-butadiene rubber, polyethylene oxide, polyacrylonitrile, (methyl) polyacrylonitrile, polyacrylic acid and its derivatives and polystyrene; the polyfluoroethylene is polytetrafluoroethylene, polyvinylidene fluoride, ethylene-tetrafluoroethylene copolymer, polyvinylidene fluoride or poly(vinylidene fluoride-hexafluoropropylene); the derivatives of polyacrylic acid include polymethyl methacrylate or modified polymethyl methacrylate.
6. The method for preparing a dry-process self-supporting film with low binder content and high toughness according to any one of claims 1 to 5, It is characterized in that The mixing and stirring in step (3) comprises the following steps: 1) The revolution speed is 100-3000rpm, the time is not less than 5min, and the revolution speed ratio is 50%-200%; 2) The revolution speed is 600rpm-3000rpm, the time is not less than 15min, and the revolution speed ratio is 30%-150%; 3) The revolution speed is 600rpm-3000rpm, the time is not less than 10min, and the revolution speed ratio is 50%-200%.
7. The method for preparing a dry-process self-supporting film with low binder content and high toughness according to claim 6, It is characterized in that In the step (4), the air flow pressure of the air flow pulverization is 0.2-0.8 MPa; the feeding pressure of the air flow pulverization is greater than the pulverization pressure; the temperature of the heating treatment is 40-80° C., and the time is 60-180 min.
8. The method for preparing a dry-process self-supporting film with low binder content and high toughness according to claim 7, It is characterized in that The hot rolling process in step (5) is as follows: the pressure is 1 to 100 tons; the temperature is 60 to 180° C.; the gap between the hot rolling rollers is 0 to 2 mm, and the hot rolling is performed 2 to 3 times.
9. A dry-process self-supporting film with low binder content and high toughness prepared by the method according to any one of claims 1 to 8, It is characterized in that The maximum tensile strength at break of the dry self-supporting film is not less than 1 MPa, and the thickness is 30-500 μm.
10. A self-supporting membrane electrode plate, It is characterized in that The dry process self-supporting film according to claim 9 is composited by hot pressing with a foil current collector.
Citation Information
Patent Citations
Composite conductive agent slurry for silicon-carbon negative electrode system and preparation method of composite conductive agent slurry
CN114068926A
Dry-method electrode preparation method, battery and dry-method electrode preparation device
CN116706074A
Dry-method electrode film with low binder content, preparation method and application thereof
CN116936735A
Binder, electrode film, electrode plate, battery and preparation method thereof
CN117374283A
Manufacturing method and preparation device for preparing positive plate of seawater battery by dry method
CN118173703A
Cited By
Film laminating glue for fibrillar self-supporting film and film laminating method
CN120574543A
Wide dry-process powder membrane preparation device and method
CN122125850A