Phosphorus-carbon composite negative electrode material and preparation method and application thereof

Phosphorus carbon materials were solved by using the ternary phosphide AxL1-xMyP of porous carbon support and its carbon clad structure in secondary ion batteries, combining the alloying of Ge, Sn and Na and the reaction of Se, Te and Na. The issues of energy density and cycle life have achieved efficient electrochemical performance improvement.

CN118919676AActive Publication Date: 2024-11-08INST OF CHEM CHINESE ACAD OF SCI
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410962110.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-11-08
Estimated Expiration
2044-07-18

AI Technical Summary

Technical Problem

The negative electrode material in existing secondary ion batteries has low energy density and short cycle life, making it difficult to meet the needs of energy storage batteries, especially phosphorus-carbon materials have limitations in circulation performance.

Method used

Porous carbon is used as a carrier to carry ternary phosphide AxL1-xMyP, and a composite capsule structure is formed through a carbon coating layer to improve conductivity and capacity. At the same time, the alloying of Ge, Sn and Na and the Se, Te and Na Reaction, enhances the reaction kinetics of Na+ and inhibits volume expansion.

Benefits of technology

It significantly improves the conductivity and specific capacity of phosphorus-carbon composite materials, enhances cycle stability, the first Coulomb efficiency of lithium-ion and sodium-ion batteries exceeds 80%, the charging specific capacity exceeds 1500mAh/g, and the cyclic capacity retention rate of 200 cycles exceeds 85. %.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118919676A_ABST
    Figure CN118919676A_ABST
Patent Text Reader

Abstract

The invention relates to a phosphorus-carbon composite negative electrode material which is of a composite capsule structure and comprises porous carbon, a ternary phosphide AxL1-xMyP loaded in porous carbon channels and a carbon coating layer, in the ternary phosphide AxL1-xMyP, A is any one of Fe, Co and Ni, L is Ge or Sn, M is Se or Te, x is more than or equal to 0.1 and less than or equal to 0.5, and y is more than or equal to 0.5 and less than or equal to 1.5. Compared with a single metal phosphide and a binary metal phosphide, the ternary phosphide AxL1-xMyP disclosed by the invention has the advantages that the conductivity, the specific capacity and the cycling stability of the material can be remarkably improved. The phosphorus-carbon composite negative electrode material prepared by the method disclosed by the invention is applied to a secondary ion battery and shows good electrochemical performance, the first coulombic efficiency in lithium ions and sodium ions exceeds 80% or above, the charging specific capacity exceeds 1500mAh / g, and the 200-circle circulation capacity retention rate exceeds 85%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of secondary ion battery negative electrode materials, and specifically relates to a phosphorus-carbon composite negative electrode material and a preparation method and application thereof. Background Art

[0002] Under the national dual-carbon strategic goal, energy storage devices are a core battlefield. In order to meet the growing demand for energy storage batteries in consumer electronics, power tools, mobile devices and other fields, secondary ion batteries with high energy density and safety are one of the important directions for the development of the next generation of efficient energy storage devices. However, the types of electrode materials used in traditional secondary ion batteries are limited, and the capacity is low, which makes it difficult to meet the current demand for energy storage batteries. Therefore, the development of the next generation of high-energy-density negative electrode materials has become a hot topic in current research and an important development direction for future large-scale energy storage battery technology.

[0003] The Li3P, Na3P and K3P alloys formed by phosphorus, lithium, sodium and potassium have a high capacity of up to 2596 mAh g -1 The theoretical capacity of red phosphorus is almost higher than that of the negative electrode materials of commercial secondary ion batteries, so phosphorus is considered to be one of the most promising negative electrode materials. Red phosphorus (RP) has the advantages of abundant reserves, commercial availability, chemical stability, and easy control. However, the conductivity of red phosphorus is extremely low (about 10 -12 S m -1 ) and is accompanied by a large volume expansion (>300%) during the charge and discharge process, which results in a low cycle life when red phosphorus is used as a negative electrode for secondary batteries. Despite some disadvantages, red phosphorus is still being studied in depth as a negative electrode material for secondary batteries in consideration of safety and practicality. Currently, the most widely studied phosphorus-based materials include metal phosphides and phosphorus-carbon composites.

[0004] Phosphorus can form metal phosphides with other transition metals, which can improve the conductivity of the material and effectively buffer the volume effect during the charge and discharge process, thereby improving the electrochemical performance and stability of the material. Professor Kim's research group first reported Sn4P3 as a negative electrode material for sodium ion batteries. The prepared Sn4P3 alloy negative electrode material has a reversible capacity of 718mAh g -1, and the capacity retention rate is high (Advanced Materials 2014, 26 (24): 4139-4144). Professor Liu's research group used a chemical deposition method to deposit metal Ni2P on the surface of red phosphorus particles, and adjusted the deposition thickness to prepare RP@Ni-P materials with a core-shell structure. The in-situ formed Ni2P has a strong contact and high conductivity with red phosphorus, ensuring the integrity of the electrode structure and alleviating the volume expansion of red phosphorus (Energy & Environmental Science 2015, 8 (12): 3531-3538). The above results show that by forming an alloy with a conductive metal element, the conductivity of phosphorus can be effectively improved, the volume expansion can be alleviated, and the electrochemical activity of the material as a negative electrode material for sodium ion batteries can be improved. However, since alloying reduces the phosphorus loading, the capacity of metal phosphides is relatively low. In contrast, carbon materials have outstanding conductivity and diverse structures, making them the first choice for phosphorus-carbon negative electrode materials. On the one hand, the composite of phosphorus and carbon materials, with carbon materials as carriers, effectively prevents the agglomeration of phosphorus particles and increases the phosphorus loading. Secondly, the excellent electrical conductivity of carbon materials can improve the electrical conductivity of composite materials.

[0005] Professor Sun's research group found that the PC bond remained stable during the cycle, ensuring good contact between phosphorus and carbon, giving the composite material a higher initial discharge capacity. However, the exposure of phosphorus has limited the cycling performance of the phosphorus-carbon material (Nano Letters 2014, 14(8), 4573-4580).

[0006] Therefore, the development of a phosphorus-carbon negative electrode material with high capacity, high first coulombic efficiency and high cycle performance is the key to achieving commercial applications and providing technical support for the development of high-energy-density secondary ion batteries. Summary of the invention

[0007] The present invention provides a phosphorus-carbon composite negative electrode material and a preparation method thereof, which are applied to lithium ion batteries and sodium ion batteries and have high coulombic efficiency, reversible capacity and excellent cycle stability.

[0008] To achieve the above object, the present invention adopts the following technical solutions:

[0009] A phosphorus-carbon composite negative electrode material having a composite capsule structure, comprising porous carbon, a ternary phosphide A loaded in the porous carbon pores, x L 1-x M y P and a carbon coating layer; the ternary phosphide A x L 1-x M yIn P, A is any one of Fe, Co and Ni, L is Ge or Sn, M is Se or Te, 0.1≤x≤0.5, 0.5≤y≤1.5.

[0010] A is a group VIII transition metal element, L is a group IVA post-transition metal, and M is a non-metallic element. The inventor unexpectedly found that the ternary phosphide formed by the three matching can significantly improve the conductivity and specific capacity of the material compared to single metal phosphides and binary metal phosphides. In addition, during the electrochemical sodiumization process, Ge and Sn in L can react with Na to form the corresponding alloys NaGe and Na 15 Sn4; Se and Te in M ​​can react with Na to form corresponding compounds Na2Se and Na2Te; these alloys and compounds can produce synergistic effects with Na3P generated during electrochemical sodiumization, effectively increasing the Na + reaction kinetics; at the same time, Na3P can act as a buffer to prevent the aggregation of Ge and Se nanocrystals during the alloying process, thereby reducing the volume expansion; Na + The improvement of reaction kinetics and the effective suppression of volume expansion during alloying make the battery have good cycle stability. Similarly, in lithium batteries, corresponding alloys and compounds can also be formed, thereby improving the electrochemical performance of the battery.

[0011] Furthermore, the ternary phosphide A x L 1-x M y In P, A is Ni, L is Sn, and M is Se.

[0012] Furthermore, the ternary phosphide A x L 1-x M y P, 0.2≤x≤0.4, 0.8≤y≤1.2.

[0013] Furthermore, the pore size distribution of the porous carbon is as follows: the volume proportion of micropores (pore size <2nm) is 60-90%, preferably 70-80%; the volume proportion of mesopores (pore size 2-50nm) is 10-40%, preferably 20-30%.

[0014] Furthermore, the pore volume of the porous carbon is 0.6 to 1.5 m 3 / g, specific surface area is 800~2100m 2 / g, and particle size D50 is 2 to 10 μm.

[0015] Furthermore, in the phosphorus-carbon composite negative electrode material, porous carbon accounts for 30wt% to 50wt%, and ternary phosphide A x L 1-x M yP accounts for 50wt% to 70wt%, and the rest is a carbon coating layer.

[0016] In a second aspect, the present invention provides a method for preparing the phosphorus-carbon composite negative electrode material, comprising the following steps:

[0017] (S1) Press A x L 1-x M y P stoichiometric ratio, dissolving A salt and L salt in a solvent to form a mixed solution; adding the element A in the A salt and the porous carbon at a ratio of 1 mmol: (5-10) g to the porous carbon, and obtaining porous carbon loaded with A ions and L ions by impregnation adsorption and centrifugal drying;

[0018] (S2) subjecting the porous carbon loaded with A ions and L ions to heat treatment in a reducing atmosphere to reduce the A ions and L ions, and obtaining the porous carbon loaded with metal A and metal L after cooling;

[0019] (S3) Press A x L 1-x M y The stoichiometric ratio of A, L, and M in P is obtained by mixing the M source with the porous carbon loaded with metal A and metal L to obtain a mixture; the mixture and the phosphorus source are heat-treated at 500-600°C for 2-6h; and then subjected to temperature control treatment to obtain A x L 1-x M y P-supported porous carbon;

[0020] (S4) A x L 1-x M y The P-loaded porous carbon is carbon-coated by a vapor deposition method to obtain the phosphorus-carbon composite negative electrode material.

[0021] Furthermore, in step (S1), the A salt is a nitrate and / or chloride of A, and the L salt is a nitrate and / or chloride of L; and the solvent is at least one of ethanol, isopropanol, and water.

[0022] Furthermore, in step (S1), the amount ratio of the porous carbon to the mixed solution is 1 g: (10-20) mL; and the impregnation adsorption is performed for 24-48 hours.

[0023] Furthermore, in step (S2), the reducing atmosphere includes hydrogen, and preferably, the hydrogen gas volume fraction is 5-20%; preferably, the reducing atmosphere is a hydrogen-argon mixed atmosphere; and the heat treatment conditions are: 300-600° C. for 3-6 hours.

[0024] Furthermore, in step (S3), the ratio of the total molar number of the A element in the A salt, the L element in the L salt, and the M element in the M source to the molar number of the P element in the phosphorus source is 1:(5-10), that is, the molar ratio of (A+L+M):P is 1:(5-10); the phosphorus source is red phosphorus or a phosphide; the phosphide is at least one of ammonium dihydrogen phosphate, sodium dihydrogen phosphate, and triphenylphosphine.

[0025] Furthermore, in step (S3), when the phosphorus source is red phosphorus: the heat treatment is a vacuum heat treatment; the temperature control treatment is a four-stage temperature control treatment: the first stage is cooled to 440-460°C and kept warm for 1-10 hours; the second stage is cooled to 410-430°C and kept warm for 1-10 hours; the third stage is cooled to 400-410°C, kept warm for 1-10 hours and then cooled to room temperature; the fourth stage is heated from room temperature to 280-400°C, kept warm for 10-40 hours and then cooled to room temperature; the cooling rates of the first, second and third stages are 0.1-1°C / min, and the heating rate of the fourth stage is 1-10°C / min;

[0026] When the phosphorus source is a phosphide: the heat treatment is a heat treatment under an inert atmosphere; the inert atmosphere is nitrogen and / or argon; and the temperature control treatment is natural cooling to room temperature.

[0027] In step (S3), when the phosphorus source is red phosphorus, the first stage is cooled to 440-460°C for 1-10 hours and the second stage is cooled to 410-430°C for 1-10 hours, so that the excess red phosphorus is slowly and evenly deposited on the porous carbon substrate when it is reduced from high temperature to near the sublimation point; the third stage is cooled to 400-410°C for 1-10 hours and then cooled to room temperature, so that the red phosphorus can be completely condensed and deposited; after three stages of cooling, the excess red phosphorus is converted into white phosphorus and deposited on the porous carbon substrate. Then the fourth stage is heated from room temperature to 280-400°C for 10-40 hours, so that the deposited white phosphorus is sublimated and converted into red phosphorus to avoid the presence of toxic white phosphorus.

[0028] The process of the carbon coating layer in step (S4) is well known to those skilled in the art, such as using a carbon source gas for vapor deposition to obtain the carbon coating, wherein the carbon source gas is selected from at least one of C1-4 alkanes, C2-4 alkenes, and C2-4 alkynes.

[0029] In a third aspect, the present invention also provides the use of the above-mentioned phosphorus-carbon composite negative electrode material in lithium-ion batteries and sodium-ion batteries.

[0030] Compared with the prior art, the present invention has the following beneficial effects:

[0031] 1) Compared with single metal phosphides and binary metal phosphides, the ternary phosphide A of the present invention x L 1-x My P can significantly improve the conductivity and specific capacity of the material. In addition, during the electrochemical sodium, lithium or potassium process, Ge and Sn in L can react with Na, Li or K to form corresponding alloys; Se and Te in M ​​can react with Na and Li to form corresponding compounds; these alloys and compounds can produce synergistic effects with Na3P generated during electrochemical sodium or Li3P generated during electrochemical lithium, which can effectively improve the corresponding Na + or Li + reaction kinetics; at the same time, Na3P and Li3P can act as buffers to prevent Ge and Se nanocrystals from aggregating during the alloying process, thereby reducing volume expansion; the improvement of the reaction kinetics of the corresponding ions and the effective suppression of volume expansion during the alloying process make the battery have good cycle stability.

[0032] 2) Due to the ternary phosphide A x L 1-x M y P is filled in the pores of the porous carbon, and its outward expansion is constrained by the outer shell of the carbon layer. When it expands inward, the presence of the porous inner core provides a buffer for its inward expansion. Therefore, the phosphorus-carbon composite negative electrode material provided in the present application can effectively suppress the structural rupture caused by the volume change of phosphorus, avoid the large loss of active sites, and improve the cycle stability.

[0033] 3) The phosphorus-carbon composite negative electrode material prepared by the method of the present invention is used in secondary ion batteries and exhibits good electrochemical properties. The first coulomb efficiency of lithium ions and sodium ions is more than 80%, the charge capacity is more than 1500mAh / g, and the capacity retention rate after 200 cycles is more than 85%. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 This is the XRD diagram of the phosphorus-carbon composite negative electrode material prepared in Example 1 of the present invention.

[0035] Figure 2 This is a SEM image of the phosphorus-carbon composite negative electrode material prepared in Example 1 of the present invention.

[0036] Figure 3 This is a TEM image of the phosphorus-carbon composite negative electrode material prepared in Example 1 of the present invention.

[0037] Figure 4 This is the charge and discharge curve of the phosphorus-carbon composite negative electrode material prepared in Example 1 of the present invention when used as the negative electrode of a sodium ion battery. DETAILED DESCRIPTION

[0038] The present invention will be further described below in conjunction with specific embodiments, but the present invention is not limited to the following embodiments.

[0039] The experimental methods described in the following examples are conventional methods unless otherwise specified; the reagents and materials described are commercially available unless otherwise specified.

[0040] The particle size D50 of porous carbon is 4.6 μm, and the specific surface area is about 1800 m 2 / g pore volume about 1.2cm 3 / g.

[0041] The furnace size of the CVD tube furnace is: 6 cm in diameter and 100 cm in length.

[0042] Example 1 (A x L 1-x M y In P, A is Fe, L is Ge, M is Se, x=0.1, y=0.5)

[0043] The specific steps are:

[0044] (S1) 0.1 mmol of ferric chloride FeCl2 and 0.9 mmol of GeCl4 were dissolved in 5 ml of pure water to form a mixed solution; 0.5 g of porous carbon was added to the mixed solution, ultrasonically stirred and immersed for 24 h, and centrifuged to obtain a Fe-loaded 2+ and Ge 4+ of porous carbon.

[0045] (S2) will load Fe 2+ and Ge 4+ The porous carbon was placed in a tube furnace, heated to 300°C at a heating rate of 5°C / min in a 10% hydrogen-argon atmosphere, and thermally reduced for 5 h, and then cooled to room temperature to obtain a porous carbon material loaded with Fe and Ge;

[0046] (S3) Fe and Ge loaded porous carbon were mixed with 0.5mmol selenium powder and 0.3g red phosphorus powder to obtain a mixture; the mixture was placed in a sealed polymerization tube with a vacuum degree of 0.01-10Pa and heated to 500℃ at a heating rate of 5℃ / min and kept warm for 5h; then a four-stage temperature control treatment was performed, the first stage: cooling to 440℃ at 0.1℃ / min and keeping warm for 2h; the second stage: cooling to 425℃ at 0.1℃ / min and keeping warm for 2h; the third stage: cooling to 416℃ at 0.1℃ / min, keeping warm for 2h and then cooling to room temperature; the fourth stage: heating to 300℃ at 5℃ / min, keeping warm for 30h, and naturally cooling to room temperature to obtain Fe 0.1 Ge 0.9 Se 0.5 P-supported porous carbon;

[0047] (S4) Fe 0.1 Ge 0.9 Se 0.5The porous carbon loaded with P was placed in a CVD furnace with a rotation speed of 20 rpm. Helium was introduced at a flow rate of 6 L / min. After the temperature was raised to 500 °C in a helium environment, acetylene gas was introduced at a flow rate of 3 L / min and maintained at 500 °C for vapor deposition for 3 h. The carbon particles formed after the decomposition of acetylene gas were deposited on Fe 0.1 Ge 0.9 Se 0.5 The surface of the porous carbon loaded with P forms a carbon coating layer, and finally a phosphorus-carbon composite negative electrode material is obtained.

[0048] The XRD pattern of the phosphorus-carbon composite negative electrode material prepared in Example 1 is as follows: Figure 1 As shown in the SEM images Figure 2 As shown in the TEM image Figure 3 shown.

[0049] Example 2 (A x L 1-x M y In P, A is Co, L is Ge, M is Te, x=0.1, y=0.5)

[0050] The rest is the same as Example 1, except that the types of A, L, and M are different, A is Co, L is Ge, and M is Te. The specific steps are:

[0051] (S1) 0.1 mmol of cobalt nitrate (Co(NO3)2·6H2O) and 0.9 mmol of GeCl4 were dissolved in 5 ml of pure water to form a mixed solution; 0.5 g of porous carbon was added to the mixed solution, ultrasonically stirred and immersed for 24 h, and centrifuged to obtain a Co-loaded 2+ and Ge 4+ of porous carbon.

[0052] (S2) Load Co 2+ and Ge 4+ The porous carbon was placed in a tube furnace, heated to 400°C at a heating rate of 5°C / min in a 10% hydrogen-argon atmosphere, and thermally reduced for 4 hours, and then cooled to room temperature to obtain a Co and Ge loaded porous carbon material;

[0053] (S3) Co and Ge loaded porous carbon were mixed with 0.5 mmol tellurium powder and 0.3 g red phosphorus powder to obtain a mixture; the mixture was placed in a sealed polymerization tube with a vacuum degree of 0.01-10 Pa and heated to 550°C at a heating rate of 5°C / min and kept warm for 4 hours; then a four-stage temperature control treatment was performed, the first stage: cooling to 440°C at 0.1°C / min and keeping warm for 1 hour; the second stage: cooling to 425°C at 0.1°C / min and keeping warm for 4 hours; the third stage: cooling to 416°C at 0.1°C / min, keeping warm for 3 hours and then cooling to room temperature; the fourth stage: heating to 300°C at 5°C / min, keeping warm for 30 hours, and naturally cooling to room temperature to obtain Co 0.1 Ge 0.9 Te 0.5 P-supported porous carbon;

[0054] (S4) Co 0.1 Ge 0.9 Te 0.5 The P-loaded porous carbon was placed in a CVD furnace and carbon-coated by a vapor deposition method. The specific process was the same as in Example 1, and finally a phosphorus-carbon composite negative electrode material was obtained.

[0055] Example 3 (A x L 1-x M y In P, A is Ni, L is Sn, M is Se, x=0.1, y=0.5)

[0056] The specific steps are:

[0057] The rest is the same as Example 1, except that the types of A, L, and M are Ni, L is Sn, M is Se, x=0.1, y=0.05, and the specific steps are:

[0058] (S1) Take 0.1mmol Ni(NO3)2·6H2O and 0.9mmol SnCl2·2H2O, dissolve them in 8ml pure water to form a mixed solution; add 0.5g porous carbon to the mixed solution, stir and immerse for 24h with ultrasonic stirring, and centrifuge and dry to obtain Ni-loaded 2+ and Sn 2+ of porous carbon.

[0059] (S2) Ni 2+ and Sn 2+ The porous carbon of the porous carbon was placed in a tube furnace, heated to 600°C at a heating rate of 5°C / min for 3h under a 10% hydrogen-argon atmosphere, and then cooled to room temperature to obtain a Ni and Sn loaded porous carbon material;

[0060] (S3) The porous carbon loaded with Ni and Sn was mixed with 0.5 mmol of selenium powder and 1.2 g of sodium dihydrogen phosphate to obtain a mixture; the mixture was placed in a sealed polymerization tube with a vacuum degree of 0.01 to 10 Pa and heated to 550° C. at a heating rate of 5° C. / min for 4 h; and then naturally cooled to room temperature to obtain Ni 0.1 Sn 0.9 Se 0.5 P-supported porous carbon;

[0061] (S4) Ni 0.1 Sn 0.9 Se 0.5 The P-loaded porous carbon was placed in a CVD furnace and carbon-coated by a vapor deposition method. The specific process was the same as in Example 1, and finally a phosphorus-carbon composite negative electrode material was obtained.

[0062] Example 4 (A x L 1-x M y In P, A is Ni, L is Sn, M is Te, x=0.1, y=0.5)

[0063] The rest is the same as Example 1, except that the types of A, L, and M are Ni, L is Sn, M is Te, x=0.1, y=0.05, and the specific steps are:

[0064] (S1) Take 0.1mmol Ni(NO3)2·6H2O and 0.9mmol SnCl2·2H2O, dissolve them in 8ml pure water to form a mixed solution; add 0.5g porous carbon to the mixed solution, stir and immerse for 24h with ultrasonic stirring, and centrifuge and dry to obtain Ni-loaded 2+ and Sn 2+ of porous carbon.

[0065] (S2) Ni 2+ and Sn 2+ The porous carbon of the porous carbon was placed in a tube furnace, heated to 600°C at a heating rate of 5°C / min for 3h under a 10% hydrogen-argon atmosphere, and then cooled to room temperature to obtain a Ni and Sn loaded porous carbon material;

[0066] (S3) Ni and Sn loaded porous carbon were mixed with 0.5 mmol tellurium powder and 1.2 g ammonium dihydrogen phosphate to obtain a mixture; the mixture was placed in a sealed polymerization tube with a vacuum degree of 0.01-10 Pa and heated to 600°C at a heating rate of 5°C / min for 3 h; then naturally cooled to room temperature to obtain Ni 0.1 Sn 0.9 Te 0.5 P-supported porous carbon;

[0067] (S4) Ni 0.1Sn 0.9 Te 0.5 The P-loaded porous carbon was placed in a CVD furnace and carbon-coated by a vapor deposition method. The specific process was the same as in Example 1, and finally a phosphorus-carbon composite negative electrode material was obtained.

[0068] Example 5 (A x L 1-x M y In P, A is Fe, L is Ge, M is Se, x=0.2, y=0.8)

[0069] The specific steps are:

[0070] The rest is the same as Example 1, except that the ratio of A, L, and M is different, x=0.2, y=0.8, and accordingly, Fe 0.2 Ge 0.8 The stoichiometric ratios of the chemical elements corresponding to Se are prepared in step (S1) and step (S3), and finally a phosphorus-carbon composite negative electrode material is obtained.

[0071] Example 6 (A x L 1-x M y In P, A is Fe, L is Ge, M is Se, x=0.2, y=1.2)

[0072] The rest is the same as Example 1, except that the ratio of A, L, and M is different, x=0.2, y=1.2, and accordingly, Fe 0.2 Ge 0.8 Se 1.2 The corresponding stoichiometric ratios of the chemical elements are mixed in step (S1) and step (S3), and finally a phosphorus-carbon composite negative electrode material is obtained.

[0073] Example 7 (A x L 1-x M y In P, A is Fe, L is Ge, M is Se, x=0.3, y=1.2)

[0074] The rest is the same as Example 1, except that the ratio of A, L, and M is different, x=0.3, y=1.2, and accordingly, Fe 0.3 Ge 0.7 Se 1.2 The corresponding stoichiometric ratios of the chemical elements are mixed in step (S1) and step (S3), and finally a phosphorus-carbon composite negative electrode material is obtained.

[0075] Example 8 (A x L 1-x M y In P, A is Fe, L is Ge, M is Se, x=0.4, y=1.5)

[0076] The rest is the same as Example 1, except that the ratio of A, L, and M is different, x=0.4, y=1.5, and accordingly, Fe 0.4 Ge 0.6 Se 1.5 The corresponding stoichiometric ratios of the chemical elements are mixed in step (S1) and step (S3), and finally a phosphorus-carbon composite negative electrode material is obtained.

[0077] Example 9 (A x L 1-x M y In P, A is Fe, L is Ge, M is Se, x=0.5, y=1.5)

[0078] The rest is the same as Example 1, except that the ratio of A, L, and M is different, x=0.5, y=1.5, and accordingly, Fe 0.5 Ge 0.5 Se 1.5 The corresponding stoichiometric ratios of the chemical elements are mixed in step (S1) and step (S3), and finally a phosphorus-carbon composite negative electrode material is obtained.

[0079] Comparative Example 1

[0080] The rest is the same as Example 1, except that the types of A, L, and M are different. A is Zn, L is Mn, and M is V. Accordingly, the Zn 0.1 Mn 0.9 V 0.5 The corresponding stoichiometric ratios of the chemical elements are mixed in step (S1) and step (S3), and finally a phosphorus-carbon composite negative electrode material is obtained.

[0081] Comparative Example 2

[0082] The rest is the same as Example 1, except that A and L are the same metal Fe, i.e., the binary metal phosphorus FeSe 0.5 P, accordingly, according to FeSe 0.5 The stoichiometric ratios of the chemical elements corresponding to P are prepared in step (S1) and step (S3), and finally a phosphorus-carbon composite negative electrode material is obtained.

[0083] Testing and analysis

[0084] The electrochemical properties of the phosphorus-carbon composite negative electrode materials prepared in the above-mentioned embodiments and comparative examples were tested according to the following method: the prepared phosphorus-carbon composite negative electrode material, carbon black and carboxymethyl cellulose (CMC) and styrene-butadiene rubber (SBR) composite binder were mixed in a mass ratio of 8:1:1 to form a slurry (wherein the mass ratio of CMC and SBR is 2:3), the slurry was uniformly coated on a copper foil current collector, and vacuum dried for 12 hours to form a working electrode; sodium flakes (lithium flakes or potassium flakes) were used as counter electrodes, glass fiber membranes (purchased from Whatman, UK) or Celgard membranes were used as diaphragms, 1 mol / L NaPF6 (1 mol / L LiPF6, or 1 mol / L KPF6) (the solvent was a mixture of ethylene carbonate and dimethyl carbonate in a volume ratio of 1:1) was used as an electrolyte, 1% VC and 5% FEC by volume were added to the electrolyte, and button batteries were assembled in an argon atmosphere in a Braun inert gas glove box in Germany.

[0085] The charge and discharge curve of the phosphorus-carbon composite negative electrode material prepared in Example 1 as the negative electrode of a sodium ion battery is as follows: Figure 4 shown.

[0086] The battery assembled above was subjected to charge and discharge tests on a LAND charge and discharge tester, and the data are shown in Table 1.

[0087] Table 1 Electrochemical performance test

[0088]

[0089]

[0090] In summary, it can be seen from the embodiments and comparative examples that the phosphorus-carbon composite negative electrode material prepared by the method of the present invention is used in a secondary ion battery, and the secondary ion battery exhibits a relatively high first coulombic efficiency and capacity. The first coulombic efficiency in lithium ion and sodium ion tests is more than 80%, the charge specific capacity exceeds 1500mAh / g, and the capacity retention rate after 200 cycles exceeds 85%.

[0091] The applicant declares that the present invention illustrates the detailed preparation method of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned detailed preparation method, that is, it does not mean that the present invention must rely on the above-mentioned detailed preparation method to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of various raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. A phosphorus-carbon composite negative electrode material, characterized in that: It is a composite capsule structure, including porous carbon and ternary phosphide A loaded in the porous carbon pores. x L 1-x M y P and a carbon coating layer; the ternary phosphide A x L 1-x M y In P, A is any one of Fe, Co and Ni, L is Ge or Sn, M is Se or Te, 0.1≤x≤0.5, 0.5≤y≤1.

5.

2. The method according to claim 1, characterized in that: The ternary phosphide A x L 1-x M y In P, A is Ni, L is Sn, and M is Se.

3. The method according to claim 1, characterized in that: The ternary phosphide A x L 1-x M y P, 0.2≤x≤0.4, 0.8≤y≤1.

2.

4. The method according to claim 1, characterized in that: The pore volume of the porous carbon is 0.6 to 1.5 m 3 / g, specific surface area is 800~2100m 2 / g, and particle size D50 is 2 to 10 μm.

5. The method according to claim 1, characterized in that: In the phosphorus-carbon composite negative electrode material, porous carbon accounts for 30wt% to 50wt%, and the ternary phosphide A x L 1-x M y P accounts for 50wt% to 70wt%, and the rest is a carbon coating layer.

6. The method for preparing the phosphorus-carbon composite negative electrode material according to any one of claims 1 to 5, characterized in that: The following steps are involved: (S1) Press A x L 1-x M y P stoichiometric ratio, dissolving A salt and L salt in a solvent to form a mixed solution; adding the element A in the A salt and the porous carbon at a ratio of 1 mmol: (5-10) g to the porous carbon, and obtaining porous carbon loaded with A ions and L ions by impregnation adsorption and centrifugal drying; (S2) subjecting the porous carbon loaded with A ions and L ions to heat treatment in a reducing atmosphere to reduce the A ions and L ions, and obtaining the porous carbon loaded with metal A and metal L after cooling; (S3) Press A x L 1-x M y The stoichiometric ratio of A, L, and M in P is obtained by mixing the M source with the porous carbon loaded with metal A and metal L to obtain a mixture; the mixture and the phosphorus source are heat-treated at 500-600°C for 2-6h; and then subjected to temperature control treatment to obtain A x L 1-x M y P-supported porous carbon; (S4) A x L 1-x M y The P-loaded porous carbon is carbon-coated by a vapor deposition method to obtain the phosphorus-carbon composite negative electrode material.

7. The preparation method according to claim 6, characterized in that: In step (S1), the A salt is a nitrate and / or chloride of A, and the L salt is a nitrate and / or chloride of L; the solvent is at least one of ethanol, isopropanol, and water; the amount ratio of the porous carbon to the mixed solution is 1g: (10-20)mL; and the immersion adsorption is immersion adsorption for 24-48h.

8. The preparation method according to claim 6, characterized in that: In step (S2), the reducing atmosphere includes hydrogen, and preferably, the volume fraction of hydrogen gas is 5-20%; preferably, the reducing atmosphere is a hydrogen-argon mixed atmosphere; the heat treatment conditions are: 300-600° C. for 3-6 hours.

9. The preparation method according to claim 6, characterized in that: In step (S3), the ratio of the total molar number of the A element in the A salt, the L element in the L salt, and the M element in the M source to the molar number of the P element in the phosphorus source is 1:(5-10); the phosphorus source is red phosphorus or a phosphide; the phosphide is at least one of ammonium dihydrogen phosphate, sodium dihydrogen phosphate, and triphenylphosphine.

10. Use of the phosphorus-carbon composite negative electrode material according to any one of claims 1 to 5 in lithium ion batteries and sodium ion batteries.

Citation Information

Patent Citations

  • Sodium-ion battery negative electrode material and preparation method thereof

    CN107093712A

  • Bimetal phosphide / carbon material, negative electrode material, lithium ion battery and method

    CN112397696A

  • Vanadium-cobalt-nickel ternary phosphide as well as preparation method and application thereof

    CN115652356A

  • Phosphorus-carbon cathode material based on red phosphorus and preparation method thereof

    US20240258523A1

  • New phosphorus-carbon negative electrode material based on red phosphorus and preparation method

    WO2024087740A1