Preparation method of silicon-carbon negative electrode material

By generating silicon-carbon precursors in a fluidized bed reactor and converting them into elemental silicon at high temperatures, the problem of destroying the porous carbon structure when silicon is embedded is solved, and the circulation performance of lithium-ion batteries is improved and the cost is reduced.

CN118919682APending Publication Date: 2024-11-08ZHEJIANG ZHONGNING SILICON INDUSTRY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410978670.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

In lithium-ion batteries, existing silicon-carbon composite materials will destroy the porous carbon skeleton structure when silicon nanoparticles are embedded, resulting in a degradation of battery circulation performance.

Method used

Silicon carbon precursor is generated by mixing porous carbon with water vapor in a fluidized bed reactor, followed by heating twice at high temperatures, using ammonia and silicon tetrafluoride to produce silica, followed by a reduction atmosphere The silica is converted into elemental silicon, leaving room for expansion to avoid damage to the porous carbon structure.

Benefits of technology

It effectively maintains the integrity of the porous carbon skeleton structure, improves the circulation performance of lithium-ion batteries, and reduces the preparation cost.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to a preparation method of a silicon-carbon negative electrode material, and belongs to the technical field of lithium battery materials. The method comprises the following steps: 1) mixing porous carbon with water vapor at high temperature and high pressure, and cooling to obtain wetted porous carbon; 2) successively mixing the wetted porous carbon obtained in the step 1) with ammonia gas and silicon tetrafluoride for reaction, and repeating for multiple times to obtain a silicon-carbon precursor; and 3) heating the precursor obtained in the step 2) twice, and cooling to obtain the silicon-carbon negative electrode material. Silicon tetrafluoride is used as a raw material, the source is rich, the price is low, and the silicon-carbon cost can be reduced; micropores in the obtained silicon-carbon product cannot be filled with silicon particles, a space is reserved for volume expansion of silicon, and a porous carbon skeleton structure cannot be damaged during lithium intercalation, so that the cycle performance of a battery is guaranteed; and pores are reserved around the silicon nanoparticles, so that an electrolyte infiltration channel and an ion shuttling channel are increased, and the power performance of the battery is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of lithium battery materials, and in particular relates to a method for preparing a silicon-carbon negative electrode material. Background Art

[0002] With the continuous development of electric vehicles, portable electronic devices and renewable energy, lithium-ion batteries, as a high energy density and lightweight battery technology, have been widely used. In lithium-ion batteries, the performance of the negative electrode material is directly related to the energy density, cycle life and safety of the battery. Silicon-carbon composite materials have become one of the research hotspots due to their high specific capacity and relatively low price.

[0003] After years of research and development, the method of preparing silicon-carbon composite materials by depositing nano-silicon in the micropores using porous carbon as a matrix through chemical vapor deposition (CVD) has become one of the mainstream methods. This method has low equipment requirements and is suitable for industrial production. The prepared silicon-carbon composite materials have achieved good results in overcoming volume expansion and contraction and improving circulation.

[0004] Patent CN117699772 discloses a method for preparing a porous carbon negative electrode material deposited by silane and its application, wherein a silicon-carbon composite material for an electrode is prepared by depositing porous carbon with silane, including mixing water or ethanol with the porous carbon material and heating and vacuum treatment to achieve sufficient gas removal, and adding a surfactant and a silane coupling agent to the water or ethanol to improve the wettability between the water or ethanol and the porous carbon, and then through the steps of inert gas replacement, rapid heating after the introduction of silane, etc., to prepare a negative electrode material of porous carbon deposited by silane. Patent CN116995219A discloses a porous silicon-carbon composite negative electrode material and its preparation method, wherein the composite material is obtained by compounding porous carbon and silicon source gas by plasma chemical vapor deposition, and the silicon source includes one of silane (SiH4), silicon tetrachloride (SiCl4) and silicon tetrafluoride (SiF4).

[0005] The above method for preparing silicon-carbon materials still has the following disadvantages: a portion of the smaller pores in the porous carbon are filled with silicon nanoparticles, leaving no room for expansion. When the silicon nanoparticles are embedded in lithium ions and expand in volume, the porous carbon skeleton structure will still be destroyed, thereby reducing the cycle performance of the battery. Summary of the invention

[0006] In order to overcome the above disadvantages, the present invention provides a method for preparing a silicon-carbon negative electrode material, which specifically comprises the following steps:

[0007] 1) Mixing porous carbon with water vapor at high temperature and high pressure, and cooling to obtain wet porous carbon;

[0008] 2) mixing the wet porous carbon obtained in step 1) with ammonia and silicon tetrafluoride in sequence to react, and repeating the process multiple times to obtain a silicon-carbon precursor;

[0009] 3) The precursor obtained in step 2) is heated twice and cooled to obtain a silicon-carbon negative electrode material.

[0010] The steps 1) and 2) are preferably carried out in a fluidized bed reactor.

[0011] In the step 1), the porous carbon is mixed with water vapor at 100-200°C and 0.1-1.5MPa(G) for 0.1-1h, and then cooled to 40-70°C. The weight ratio of the porous carbon to the water vapor is 1:(0.2-0.6). The porous carbon has good adsorption capacity. After mixing with high-temperature and high-pressure water vapor and cooling, the water vapor is liquefied and adsorbed in the micropores of the porous carbon.

[0012] In the step 2), the temperature is maintained at 40-70° C. The wet porous carbon is mixed with ammonia to form NH 3 ·H 2 O which is adsorbed in the micropores, and then mixed with silicon tetrafluoride to undergo a chemical reaction to generate silicon dioxide and ammonium fluoride. The generated silicon dioxide and ammonium fluoride are attached in situ in the pores. The chemical reaction involved is:

[0013] 4NH3·H2O+SiF4→SiO2+4NH4F+2H2O

[0014] The wet porous carbon is mixed with ammonia and silicon tetrafluoride in succession and circulated for multiple times. Each cycle step takes 6-20 minutes and is repeated 5-20 times. The weight of ammonia and silicon tetrafluoride used in each cycle is 0.03-0.1 times and 0.05-0.2 times the weight of the porous carbon, respectively. The molar ratio of the total amount of ammonia, the total amount of silicon tetrafluoride and the amount of water vapor is preferably 4:1:(2-2.1). Under this condition, the materials are balanced, the reaction is completed, the water content of the obtained silicon-carbon precursor is the lowest, and the burden of subsequent heating is small.

[0015] In the step 3), the silicon-carbon precursor is transferred to a heating furnace, heated to 100-120°C for the first time, and kept warm for 1-4 hours. The residual gas that has not been completely reacted volatilizes, and the ammonium fluoride also sublimates and escapes. Inert gas is introduced to assist the ammonium fluoride to escape completely. The only remaining thing is porous carbon and silicon dioxide in the pores. Then, it is heated to 1000-1400°C for a second time in a reducing atmosphere and kept warm for 1-10 hours. The silicon dioxide is reduced to elemental silicon, and the temperature is lowered to obtain a silicon-carbon negative electrode material. If the second heating temperature is too high, silicon carbide is easily generated, and if the temperature is too low, the silicon dioxide cannot be reduced.

[0016] The reducing atmosphere is a mixture of inert gas and hydrogen, wherein the volume proportion of hydrogen in the mixture is 5-10%.

[0017] Furthermore, the gas discharged from the first heating system mainly contains ammonium fluoride, inert gas and a small amount of silicon tetrafluoride, ammonia and water vapor. After cooling, gas-solid separation can obtain ammonium fluoride, which is also an important industrial raw material. Preferably, the gas-solid separation can be performed using a cyclone separator or a filter separator.

[0018] The porous carbon is prepared by high-temperature carbonization of biomass, polymer or a mixture of the two, for example, using one or more of coconut shell, straw, rice husk, wood, bamboo, bagasse, nut shell, polyaniline, polycarbazole, polythiophene, polypyrrole, polythiazine and polyaromatic amine as raw materials, and treating at 700-900° C. for 1-12 hours under inert atmosphere protection.

[0019] The silicon tetrafluoride is abundant in source and cheap in price, for example, it is derived from the byproduct of the reaction of fluorosilicate and concentrated sulfuric acid to produce hydrogen fluoride, or the byproduct of the phosphate fertilizer production process.

[0020] The SiO2 generated by the reaction of NH3·H2O and SiF4 is nanoscale and evenly dispersed in the porous carbon micropores. It is understandable that ammonium fluoride is deposited in the micropores together with silicon dioxide, and ammonium fluoride occupies part of the space, so that silicon dioxide cannot fill the micropores, and ammonium fluoride sublimates and escapes, leaving space. Furthermore, silicon dioxide is reduced to elemental silicon during the second heating, and the volume is further reduced, freeing up some space. In both cases, space is reserved for silicon expansion, so that the volume expansion of silicon after embedding lithium does not destroy the porous carbon skeleton, and it can be restored to its original state after de-lithiation, so it can maintain good cycle performance.

[0021] Furthermore, after the second heating, the porous carbon undergoes partial microcrystallization, which makes the structure more stable and is also beneficial to improving the battery cycle performance.

[0022] The beneficial effects of the present invention are:

[0023] (1) The present application uses silicon tetrafluoride as raw material, which is abundant in source and cheap, and is conducive to reducing the cost of silicon carbon; (2) The silicon particles in the obtained silicon carbon product will not fill the micropores, leaving space for the volume expansion of silicon, and the porous carbon skeleton structure will not be destroyed when lithium is embedded, thereby ensuring the battery cycle performance; (3) Pores are left around the silicon nanoparticles, which increase the electrolyte infiltration channels and ion shuttle channels, which is conducive to improving the battery power performance; (4) The by-product ammonium fluoride can also be sold separately, further improving the comprehensive benefits of the preparation method. DETAILED DESCRIPTION

[0024] A method for preparing a silicon-carbon negative electrode material:

[0025] 1) In a fluidized bed reactor, the porous carbon is mixed with 0.2-0.6 times the weight of water vapor at 100-200° C. and 0.1-1.5 MPa (G) for 0.1-1 h, and then cooled to 40-70° C. to obtain wet porous carbon;

[0026] 2) mixing the wet porous carbon obtained in step 1) with 0.03-0.1 times by weight of ammonia and 0.05-0.2 times by weight of silicon tetrafluoride, reacting at 40-70° C. for 6-20 minutes, repeating 5-20 times to obtain a silicon-carbon precursor;

[0027] 3) The silicon-carbon precursor obtained in step 2) is transferred to a heating furnace, heated to 100-120°C, and introduced with inert gas for 1-4 hours, then kept at 1000-1400°C for 1-10 hours in a mixed atmosphere of hydrogen and inert gas, and cooled to obtain a silicon-carbon negative electrode material.

[0028] The technical solution of the present invention is further described in detail below in conjunction with specific embodiments.

[0029] Example 1

[0030] A method for preparing a silicon-carbon negative electrode material:

[0031] 1) In a fluidized bed reactor, 1000 g of porous carbon was mixed with 350 g of water vapor at 140 ° C and 0.3 MPa (G) for 0.5 h, and then cooled to 60 ° C to obtain wet porous carbon;

[0032] 2) The wet porous carbon obtained in step 1) was mixed with 54.4 g of ammonia and 83.3 g of silicon tetrafluoride, and reacted at 60° C. for 10 min, and repeated 12 times to obtain a silicon-carbon precursor;

[0033] 3) The silicon-carbon precursor obtained in step 2) was transferred to a heating furnace, heated to 110°C, and nitrogen was introduced for 2 hours, then kept at 1200°C for 6 hours in a hydrogen-nitrogen mixed atmosphere with a hydrogen volume ratio of 8%, and cooled to obtain 1200g of silicon-carbon negative electrode material with a silicon content of 21%.

[0034] Example 2

[0035] A method for preparing a silicon-carbon negative electrode material:

[0036] 1) In a fluidized bed reactor, 1000 g of porous carbon was mixed with 210 g of water vapor at 110 ° C and 0.1 MPa (G) for 1 h, and then cooled to 45 ° C to obtain wet porous carbon;

[0037] 2) The wet porous carbon obtained in step 1) was mixed with 78.4 g of ammonia and 120 g of silicon tetrafluoride, and reacted at 45° C. for 20 min, and the mixture was repeated 5 times to obtain a silicon-carbon precursor;

[0038] 3) The silicon-carbon precursor obtained in step 2) was transferred to a heating furnace, heated to 100°C, and nitrogen was introduced for 3 hours, then kept at 1100°C for 5 hours in a hydrogen-nitrogen mixed atmosphere with a hydrogen volume percentage of 5%, and cooled to obtain 1100 g of silicon-carbon negative electrode material with a silicon content of 13.4%.

[0039] Example 3

[0040] A method for preparing a silicon-carbon negative electrode material:

[0041] 1) In a fluidized bed reactor, 1000 g of porous carbon was mixed with 540 g of water vapor at 180 ° C and 0.9 MPa (G) for 0.3 h, and then cooled to 70 ° C to obtain wet porous carbon;

[0042] 2) The wet porous carbon obtained in step 1) was mixed with 50.6 g of ammonia and 77.5 g of silicon tetrafluoride, and reacted at 70° C. for 6 min, and repeated 20 times to obtain a silicon-carbon precursor;

[0043] 3) The silicon-carbon precursor obtained in step 2) was transferred to a heating furnace, heated to 120°C, and argon was introduced for 4 hours, then kept at 1400°C for 10 hours in a hydrogen-argon mixed atmosphere with a hydrogen volume ratio of 10%, and cooled to obtain 1360g of silicon-carbon negative electrode material with a silicon content of 29.2%.

[0044] Comparative Example

[0045] In a fluidized bed reactor, 1000 g of porous carbon was contacted with 330 g of monosilane gas at 750° C. for 4 h to obtain 1200 g of silicon-carbon material with a silicon content of 22%.

[0046] Experimental example

[0047] The silicon-carbon material obtained in the above embodiments and comparative examples was mixed with 200% graphite as the negative electrode, and lithium iron phosphate was used as the positive electrode to make a 2Ah soft-pack battery. The cycle performance was tested (charging cut-off voltage 3.65V, discharging cut-off voltage 2.5V, 1C charging / 1C discharging, room temperature). The results are listed in the table below.

[0048] Initial capacity / mAh Cycle 300th cycle capacity / mAh 300th week retention rate Example 1 2044 2021 98.9% Example 2 2256 2239 99.2% Example 3 2130 2117 99.4% Comparative Example 2165 2046 94.5%

[0049] It can be seen from the data in the table that the cycle performance of the silicon-carbon product of the embodiment of the present application is significantly better than that of the comparative product, indicating that the technical solution of the present application overcomes the problem that silicon fills the smaller micropores of porous carbon, resulting in the destruction of the porous carbon skeleton structure during circulation.

Claims

1. A method for preparing a silicon-carbon negative electrode material, characterized in that The following steps are involved: 1) Mixing porous carbon with water vapor at high temperature and high pressure, and cooling to obtain wet porous carbon; 2) mixing the wet porous carbon obtained in step 1) with ammonia and silicon tetrafluoride in sequence to react, and repeating the process multiple times to obtain a silicon-carbon precursor; 3) The precursor obtained in step 2) is heated twice and cooled to obtain a silicon-carbon negative electrode material.

2. The method according to claim 1, characterized in that In the step 1), the weight ratio of porous carbon to water vapor is 1:(0.2-0.6), and the mixing conditions are temperature 100-200° C., pressure 0.1-1.5 MPa(G), and mixing time 0.1-1 h.

3. The method according to claim 1, characterized in that In the step 2), the step of mixing the wet porous carbon with ammonia and silicon tetrafluoride successively takes 6-20 minutes each time and is repeated 5-20 times.

4. The method according to claim 3, characterized in that The weight of ammonia and silicon tetrafluoride used each time is 0.03-0.1 times and 0.05-0.2 times the weight of the porous carbon, respectively.

5. The method according to claim 1, characterized in that The first heating in step 3) is at a temperature of 100-120° C. for 1-4 hours, and the second heating is at a temperature of 1000-1400° C. for 1-10 hours.

6. The method according to claim 5, characterized in that During the first heating, an inert gas is passed through.

7. The method according to claim 5, characterized in that The second heating is performed in a reducing atmosphere, which is a mixture of inert gas and hydrogen, wherein the volume proportion of hydrogen in the mixture is 5-10%.

8. The method according to claim 1, characterized in that In the step 1), the porous carbon is prepared by high-temperature carbonization of one or more of biomass and polymer.

9. The method according to claim 8, characterized in that The biomass is selected from at least one of coconut shells, straws, rice husks, wood, bamboo, bagasse, and nut shells, and the polymer is selected from at least one of polyaniline, polycarbazole, polythiophene, polypyrrole, polythiazine, and polyaromatic amine.

10. The method according to claim 8, characterized in that The high temperature carbonization is carried out at 700-900° C. for 1-12 hours under the protection of an inert atmosphere.