Low-residual alkali sodium ion battery layered positive electrode active material and preparation method thereof
By incorporating Ti4+ and Ca2+ into the layered oxide, the degree of Na+ sintering is increased and the cladding layer is formed, which solves the high pH and residual alkali problems during high-temperature sintering of layered oxides, and improves the conductivity and corrosion resistance. It extends the battery life and reduces safety risks.
Patent Information
- Application Number
- CN202411226318.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-03
- Publication Date
- 2024-11-08
AI Technical Summary
Laminated oxides form high pH and residual alkali during high temperature sintering, resulting in side reactions with the electrolyte, reducing the life of the battery cell and increasing safety hazards, and it is difficult for Na+ ions to completely burn into the material lattice, affecting the electron conductivity and use. life.
By adding high-priced Ti4+ and Ca2+ to the layered sodium-electric material, the degree to which Na+ is burned into the material lattice is reduced, the residual sodium on the surface of the material is reduced, and a special coating layer is formed by high-temperature sintering and ball milling are used to suppress the side. Reaction and corrosion.
It effectively reduces residual sodium on the surface of the material, enhances conductivity and corrosion resistance, reduces side reactions, extends the service life of the battery cell and improves safety.
Smart Images

Figure CN118919715A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of sodium ion batteries, and in particular relates to a low-residual-alkali sodium ion battery layered positive electrode active material and a preparation method thereof. Background Art
[0002] Layered oxide (Na x TMO2) is a potential sodium ion battery cathode material. This material has high energy density and good cycle performance and is considered to be an important component in the future new energy field.
[0003] In the context of the country's vigorous advocacy and support for new energy, green travel and low-carbon environmental protection have become important guarantees for the sustainable development of society and economy. Layered oxides, as a positive electrode material for sodium-ion batteries, can be used to replace traditional lithium-ion batteries, thereby reducing dependence on limited lithium resources. In addition, layered oxides have the advantages of low cost, simple preparation, and environmental friendliness, making them a material with bright prospects in the field of new energy. In the future, with the continuous development of new energy technologies, layered oxides, as an excellent positive electrode material for sodium-ion batteries, will be more widely used and promoted in the field of new energy. At the same time, for social and economic sustainable development, the application of layered oxides will further promote the realization of green travel and low-carbon environmental protection.
[0004] However, during the high-temperature sintering process of layered oxides, Na + The layer causes the material to have a higher pH and residual alkali, and many side reactions will occur when it comes into contact with the electrolyte, producing gases such as hydrogen fluoride, carbon monoxide, carbon dioxide, and phosphorus oxyfluoride, which reduces the service life of the battery cell and greatly increases the safety hazards of the battery cell during use.
[0005] Due to Na x Na in TMO2 materials + The ion radius is large (r = 0.113nm), and it is difficult to convert Na + It is completely burned into the material lattice, which makes its pH and residual alkali on the surface too high. The electronic conductivity of the positive electrode material and the intrinsic conductivity inside the particles will also be affected. After the liquid injection and formation are completed, the positive electrode material reacts with the electrolyte to produce gas, which affects the service life and safety of the battery cell and limits the practical application of the battery cell. Summary of the invention
[0006] The purpose of the present invention is to overcome the above problems existing in the prior art, provide a low residual alkali sodium ion battery layered positive electrode active material and a preparation method thereof, by high temperature sintering inside the layered sodium electric material doped with high valence Ti 4+ and Ca 2+ , increase Na + The degree of burning into the material's crystal lattice reduces the residual sodium on the material's surface.
[0007] In order to achieve the above technical objectives and the above technical effects, the present invention is implemented through the following technical solutions:
[0008] In a first aspect, the present invention provides a layered positive electrode active material for a low-residual alkali sodium ion battery, wherein the molecular formula of the layered positive electrode active material is Na x Ni 0.25 Fe 0.30 Mn 0.30 Ti 0.10 Ca 0.05 O2;
[0009] Among them, 0.7 <x<1。
[0010] In a second aspect, the present invention further provides a method for preparing a layered positive electrode active material for a sodium ion battery with low residual alkali provided by an embodiment of the first aspect of the present invention, the method comprising the following steps:
[0011] S1: adding a sodium source, a ternary precursor, a titanium source and a calcium source into a high-speed mixer for mixing and stirring to prepare a mixed material;
[0012] S2: using a ball mill to ball mill the mixed material, pouring the ball-milled mixed material into a sagger, moving it into an atmosphere furnace, sintering it in an oxygen atmosphere, cooling it after sintering, and preparing a sintered product;
[0013] S3: pour the sintered product into a crusher for crushing, sieve it after crushing, use a permanent magnetic iron removal rod to remove impurities from the sieved sintered product, and crush it with a jet mill to obtain a layered positive electrode active material.
[0014] Furthermore, in step S1, the specific process of the mixing and stirring treatment is: adding the sodium source, the ternary precursor, the titanium source and the calcium source into a high-speed mixer, first mixing and stirring at a speed of 300 r / min for 10 minutes, and then mixing and stirring at a speed of 700 r / min for 20 minutes to prepare a mixed material.
[0015] Further, in step S1, in step S1, the molar ratio of the sodium source, the ternary precursor, the titanium source and the calcium source is (0.6-1.0): (0.6-2.0): (0.1-1.0): (0.10-1.0).
[0016] Furthermore, the sodium source includes any one of sodium carbonate, sodium nitrate, sodium bicarbonate, sodium oxalate or sodium acetate, or a combination of at least two thereof.
[0017] Furthermore, the ternary precursor is a nickel-iron-manganese ternary precursor of model LPXS-NFM-1201 produced by Lepu.
[0018] Furthermore, the titanium source includes any one of titanium oxide, titanium hydroxide or titanium carbonate, or a combination of at least two of them.
[0019] Furthermore, the calcium source includes any one of calcium carbonate, calcium hydroxide, calcium bicarbonate or calcium oxide, or a combination of at least two thereof.
[0020] Furthermore, in step S2, during the sintering process, the sintering temperature is 500-900°C, and the sintering time is 10-20h.
[0021] Furthermore, in step S3, the sieve opening is not less than 300 meshes.
[0022] Compared with the prior art, the present invention has the following beneficial effects:
[0023] 1. The present invention provides a layered positive electrode active material for a low-residual alkali sodium ion battery and a preparation method thereof, wherein a high-valent Ti is doped into the layered sodium battery material by high-temperature sintering. 4+ and Ca 2+ , increase Na + The degree of burning into the material's crystal lattice reduces the residual sodium on the material's surface.
[0024] 2. Use high temperature solid phase method for sintering. During the sintering process, part of titanium source and calcium source are coated on the surface of the material, changing the microstructure of the surface of the material, which not only makes Na + The degree of burning into the material lattice increases, effectively reducing Na + It can effectively prevent the material from being corroded by the electrolyte.
[0025] 3. In the present invention, during the sintering process, a portion of Ti 4+ Doped into the material lattice, occupying the original iron site, improving the conductivity of the material, and having the effect of increasing capacity; a part of Ca 2+ After being incorporated into the lattice, it occupies the Na + sites, reducing the electronic band gap of the material, improving the conductivity of the material, suppressing the energy barrier, and promoting the Na+ extraction and embedding rate.
[0026] 4. By doping Ti inside the layered oxide 4+ and Ca 2+ , reducing the electronic band gap of the material, suppressing the energy barrier, increasing the lattice constant of the material, and improving the conductivity of the material, while also increasing the Na + The degree to which the material is burned into the crystal.
[0027] 5. By adding Ti during the sintering process of layered oxides 4+ and Ca 2+ , creatively utilizing Ti that is not incorporated into the material 4+ and Ca 2+ , forming a special coating layer on the surface of the material, which effectively protects the positive electrode material while lowering the pH of the material, inhibiting the side reaction between the material and the electrolyte, and reducing gas production. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] The drawings described herein are used to provide a further understanding of the present invention and constitute a part of this application. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:
[0029] Figure 1 This is a flow chart of a method for preparing a layered positive electrode active material for a low-residual alkali sodium ion battery provided by the present invention;
[0030] Figure 2 is a scanning electron microscope image of the layered positive electrode material prepared in Example 1 of the present invention;
[0031] Figure 3 This is the XRD diagram of the layered positive electrode material prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0032] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0033] The embodiment of the present invention provides a layered positive electrode active material for a sodium ion battery with low residual alkali. The molecular formula of the layered positive electrode active material is Na x Ni 0.25 Fe 0.30 Mn 0.30 Ti 0.10 Ca 0.05 O2, of which 0.7 <x<1。
[0034] An embodiment of the present invention further provides a method for preparing the above-mentioned low-residual alkali sodium ion battery layered positive electrode active material, the preparation method comprising the following steps:
[0035] S1: adding the sodium source, the ternary precursor, the titanium source and the calcium source into a high-speed mixer, first mixing and stirring at a speed of 300 r / min for 10 min, and then mixing and stirring at a speed of 700 r / min for 20 min to prepare a mixed material;
[0036] Wherein, in step S1, the molar ratio of the sodium source, the ternary precursor, the titanium source and the calcium source is (0.6-1.0): (0.6-2.0): (0.1-1.0): (0.10-1.0);
[0037] The sodium source includes any one of sodium carbonate, sodium nitrate, sodium bicarbonate, sodium oxalate or sodium acetate, or a combination of at least two thereof;
[0038] The ternary precursor is a nickel-iron-manganese ternary precursor of model LPXS-NFM-1201 produced by Lepu;
[0039] Among them, LPXS-NFM-1201 ternary precursor is a hydroxide of nickel iron manganese with a general structural formula of Ni a Fe b Mn c (OH)2; where a, b, and c satisfy the following relationship:
[0040] a+b+c=1;
[0041] 0.28 <a<0.30;
[0042] 0.34 <b<0.36;
[0043] 0.34 <c<0.36;
[0044] The titanium source includes any one of titanium oxide, titanium hydroxide or titanium carbonate or a combination of at least two thereof; the calcium source includes any one of calcium carbonate, calcium hydroxide, calcium bicarbonate or calcium oxide or a combination of at least two thereof;
[0045] S2: using a ball mill to ball-mill the mixed material, pouring the ball-milled mixed material into a sagger, moving it into an atmosphere furnace, sintering it in an oxygen atmosphere, cooling it after sintering, and preparing a sintered product;
[0046] In the sintering process, the sintering temperature is 500-900°C and the sintering time is 10-20h;
[0047] S3: pour the sintered product into a crusher for crushing, sieve it after crushing, use a permanent magnetic iron removal rod to remove impurities from the sieved sintered product, and crush it with a jet mill to obtain a layered positive electrode active material.
[0048] Wherein, in step S3, the sieve aperture is not less than 300 meshes.
[0049] Since titanium source and calcium source are added to the mixed material, a special coating layer can be formed on the surface of the prepared layered positive electrode active material, thereby protecting the layered positive electrode active material, thereby inhibiting the side reaction between the material and the electrolyte, reducing gas production, and solving the problem in the prior art that the positive electrode material is prone to side reaction with the electrolyte to produce gas, thereby affecting the service life and safety of the battery cell.
[0050] The following examples and comparative examples are used to describe the low residual alkali sodium ion battery layered positive electrode active material and its preparation method provided by the present invention in detail. In the following examples and comparative examples, unless otherwise specified, all raw materials can be obtained from the market. Among them, the ternary precursors in Examples 1-5 and Comparative Example 1 are all nickel-iron-manganese ternary precursors of model LPXS-NFM-1201 produced by Lepu, with a structural formula of Ni a Fe b Mn c (OH)2, wherein a=0.294; b=0.353; c=0.353.
[0051] Example 1
[0052] This embodiment provides a method for preparing a layered positive electrode active material for a low-residual alkali sodium ion battery. The specific process of the preparation method is as follows:
[0053] Weigh 216.23g of sodium carbonate, 284.77g of ternary precursor, 83.42g of titanium dioxide, and 46.18g of calcium hydroxide and add them to a high-speed mixer. First, mix at a low speed of 300r / min for 10min, and then at a high speed of 700r / min for 20min. Place the fully mixed materials in a sagger, and use a high-temperature solid phase method to cut the materials in the sagger into pieces and place them in an oxygen atmosphere furnace for sintering. Oxygen is introduced, and the sintering temperature is set to 700℃, and the sintering time is 15h. After sintering, pour the materials into a crusher, sieve with a 300-mesh screen after crushing, and remove impurities with a permanent magnetic iron removal rod. Package and store for use to obtain the positive electrode material; the positive electrode material is tested by residual alkali titration, and the CO3 in the water is tested respectively. 2- OH - .
[0054] The molecular formula of the prepared positive electrode material is Na 0.95 Ni 0.25 Fe 0.30 Mn 0.30 Ti 0.10 Ca 0.05 O2.
[0055] The test results obtained in this embodiment are shown in Table 1.
[0056] Comparative Example 1
[0057] This comparative example provides a method for preparing a layered positive electrode active material for a low-residual alkali sodium ion battery. The specific process of the preparation method is as follows:
[0058] Weigh 215.73g of sodium carbonate, 284.12g of ternary precursor, and 83.42g of titanium dioxide into a high-speed mixer. Mix at 300r / min for 10min, and then at 700r / min for 20min. Place the fully mixed materials in a sagger, cut the materials in the sagger into pieces using a high-temperature solid phase method, and place them in an oxygen atmosphere furnace for sintering. Oxygen is introduced, and the sintering temperature is set to 500°C. The sintering time is 20h. After sintering, pour the materials into a crusher, sieve them with a 300-mesh screen after crushing, and remove impurities with a permanent magnetic iron removal rod. Package and store them for later use to obtain the positive electrode material. The positive electrode material is tested by residual alkali titration, and the CO3 in the water is tested respectively. 2- OH - .
[0059] The molecular formula of the prepared positive electrode material is Na 0.90 Ni 0.25 Fe 0.30 Mn 0.30 Ti 0.10 O2.
[0060] The test results obtained in this comparative example are shown in Table 1.
[0061] Comparative Example 2
[0062] This comparative example provides a method for preparing a layered positive electrode active material for a low-residual alkali sodium ion battery. The specific process of the preparation method is as follows:
[0063] Weigh 215.73g of sodium carbonate, 284.12g of ternary precursor, and 46.18g of calcium hydroxide and add them to a high-speed mixer. First, mix at a low speed of 300r / min for 10min, and then at a high speed of 700r / min for 20min. Place the fully mixed materials in a sagger, and use a high-temperature solid phase method to cut the materials in the sagger into pieces and place them in an oxygen atmosphere furnace for sintering, and introduce oxygen. The sintering temperature is set to 900℃, and the sintering time is 10h. After sintering, pour the materials into a crusher, sieve them with a 300-mesh screen after crushing, and remove impurities with a permanent magnetic iron removal rod. Package and store them for later use to obtain the positive electrode material; the positive electrode material is tested by residual alkali titration method, and the CO3 in the water is tested respectively. 2- OH - .
[0064] The molecular formula of the prepared positive electrode material is Na 0.90 Ni 0.25 Fe 0.30 Mn0.30 Ca 0.05 O2.
[0065] The test results obtained in this comparative example are shown in Table 1.
[0066] Comparative Example 3
[0067] This comparative example provides a method for preparing a layered positive electrode active material for a low-residual alkali sodium ion battery. The specific process of the preparation method is as follows:
[0068] Weigh 216.23g of sodium carbonate, 284.77g of ternary precursor, and 83.42g of titanium dioxide into a high-speed mixer. First, mix at a low speed of 300r / min for 10min, and then at a high speed of 700r / min for 20min. Place the fully mixed materials in a sagger, and use a high-temperature solid phase method to cut the materials in the sagger into pieces and place them in an oxygen atmosphere furnace for sintering. Oxygen is introduced, and the sintering temperature is set to 700℃ for 15h. After sintering, pour the materials into a crusher, sieve with a 300-mesh screen after crushing, and remove impurities with a permanent magnetic iron removal rod. Package and store for use to obtain the positive electrode material; the positive electrode material is tested by residual alkali titration, and the CO3 in the water is tested respectively. 2- OH - .
[0069] The molecular formula of the prepared positive electrode material is Na 0.95 Ni 0.25 Fe 0.30 Mn 0.30 Ti 0.10 O2.
[0070] The test results obtained in this comparative example are shown in Table 1.
[0071] Comparative Example 4
[0072] This comparative example provides a method for preparing a layered positive electrode active material for a low-residual alkali sodium ion battery. The specific process of the preparation method is as follows:
[0073] Weigh 216.23g of sodium carbonate, 284.77g of ternary precursor, and 46.18g of calcium hydroxide and add them to a high-speed mixer. First, mix at a low speed of 300r / min for 10min, and then at a high speed of 700r / min for 20min. Place the fully mixed materials in a sagger, and use a high-temperature solid phase method to cut the materials in the sagger into pieces and place them in an oxygen atmosphere furnace for sintering. Oxygen is introduced, and the sintering temperature is set to 700℃ and the sintering time is 15h. After sintering, pour the materials into a crusher, sieve them with a 300-mesh screen after crushing, and remove impurities with a permanent magnetic iron removal rod. Package and store them for later use to obtain the positive electrode material; the positive electrode material is tested by residual alkali titration, and the CO3 in the water is tested respectively.2- OH - .
[0074] The molecular formula of the prepared positive electrode material is Na 0.95 Ni 0.25 Fe 0.30 Mn 0.30 Ca 0.05 O2.
[0075] The test results obtained in this comparative example are shown in Table 1.
[0076] Comparative Example 5
[0077] This comparative example provides a method for preparing a layered positive electrode active material for a low-residual alkali sodium ion battery. The specific process of the preparation method is as follows:
[0078] Weigh 215.73g of sodium carbonate and 284.12g of ternary precursor, add them to a high-speed mixer, mix at a low speed of 300r / min for 10min, and then at a high speed of 700r / min for 20min. Place the fully mixed materials in a sagger, use a high-temperature solid phase method, cut the materials in the sagger into pieces, place them in an oxygen atmosphere furnace for sintering, and introduce oxygen. The sintering temperature is set to 700℃, and the sintering time is 15h. After sintering, pour the materials into a crusher, sieve them with a 300-mesh screen after crushing, and remove impurities with a permanent magnetic iron removal rod. Package and store them for later use to obtain the positive electrode material; the positive electrode material is tested by residual alkali titration, and the CO3 in the water is tested respectively. 2- OH - .
[0079] The test results obtained in this comparative example are shown in Table 1.
[0080] Table 1 Test results of residual alkali titration method for positive electrode materials prepared in Example 1 and Comparative Examples 1-5
[0081]
[0082] It can be seen from the data in Table 1 that compared with Comparative Example 5, the pH and CO3 content in water of Example 1 are significantly higher than those of Comparative Example 5. 2- With OH - The contents are all reduced, indicating that the present invention has the effect of reducing residual alkali.
[0083] In addition, in Example 1, the titanium source and calcium source were added simultaneously, and the pH and CO3 in the water 2- With OH - The contents are lower than those of comparative examples 1-4, indicating that in the present application, the simultaneous addition of the titanium source and the calcium source can effectively protect the positive electrode material while lowering the pH of the material and inhibiting the side reaction between the material and the electrolyte.
[0084] The present invention provides a layered positive electrode active material for a sodium ion battery with low residual alkali and a preparation method thereof, wherein a high-valent Ti is doped into the layered sodium battery material by high-temperature sintering. 4+ and Ca 2+ , increase Na + The degree of burning into the material's crystal lattice reduces the residual sodium on the material's surface.
[0085] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0086] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments, and the above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, and these changes and improvements all fall within the scope of the present invention to be protected.
Claims
1. A layered positive electrode active material for a sodium ion battery with low residual alkali, characterized in that: The molecular formula of the layered positive electrode active material is Na x Ni 0.25 Fe 0.30 Mn 0.30 Ti 0.10 Ca 0.05 O2; Among them, 0.7 <x<1。 2. A method for preparing a layered positive electrode active material for a sodium ion battery with low residual alkali according to claim 1, characterized in that: The method comprises the following steps: S1: adding a sodium source, a ternary precursor, a titanium source and a calcium source into a high-speed mixer for mixing and stirring to prepare a mixed material; S2: using a ball mill to ball mill the mixed material, pouring the ball-milled mixed material into a sagger, moving it into an atmosphere furnace, sintering it in an oxygen atmosphere, cooling it after sintering, and preparing a sintered product; S3: pour the sintered product into a crusher for crushing, sieve it after crushing, use a permanent magnetic iron removal rod to remove impurities from the sieved sintered product, and crush it with a jet mill to obtain a layered positive electrode active material.
3. The method for preparing a layered positive electrode active material for a sodium ion battery with low residual alkali according to claim 2, characterized in that: In step S1, the specific process of the mixing and stirring treatment is: adding the sodium source, the ternary precursor, the titanium source and the calcium source into a high-speed mixer, first mixing and stirring at a speed of 300 r / min for 10 minutes, and then mixing and stirring at a speed of 700 r / min for 20 minutes to prepare a mixed material.
4. The method for preparing a layered positive electrode active material for a sodium ion battery with low residual alkali according to claim 2, characterized in that: In step S1, the molar ratio of the sodium source, the ternary precursor, the titanium source and the calcium source is (0.6-1.0): (0.6-2.0): (0.1-1.0): (0.10-1.0).
5. The method for preparing a layered positive electrode active material for a sodium ion battery with low residual alkali according to claim 2, characterized in that: The sodium source includes any one of sodium carbonate, sodium nitrate, sodium bicarbonate, sodium oxalate or sodium acetate, or a combination of at least two thereof.
6. The method for preparing a layered positive electrode active material for a sodium ion battery with low residual alkali according to claim 2, characterized in that: The ternary precursor is a nickel-iron-manganese ternary precursor of model LPXS-NFM-1201 produced by Lepu.
7. The method for preparing a layered positive electrode active material for a sodium ion battery with low residual alkali according to claim 2, characterized in that: The titanium source includes any one of titanium oxide, titanium hydroxide or titanium carbonate, or a combination of at least two of them.
8. The method for preparing a layered positive electrode active material for a sodium ion battery with low residual alkali according to claim 2, characterized in that: The calcium source includes any one of calcium carbonate, calcium hydroxide, calcium bicarbonate or calcium oxide, or a combination of at least two thereof.
9. The method for preparing a layered positive electrode active material for a sodium ion battery with low residual alkali according to claim 2, characterized in that: In step S2, during the sintering process, the sintering temperature is 500-900°C and the sintering time is 10-20h.
10. The method for preparing a layered positive electrode active material for a sodium ion battery with low residual alkali according to claim 2, characterized in that: In step S3, the sieve aperture is not less than 300 meshes.
Citation Information
Patent Citations
Layered sodium ion positive electrode material and preparation method thereof
CN118047424A
Double-site metal ion doped nickel iron sodium manganate positive electrode material and preparation method thereof, positive electrode plate and sodium ion battery
CN118315567A
Positive electrode material and sodium ion battery
WO2024131048A1