Battery, pole piece, conductive material and preparation method thereof

By using specific chemical formula powder materials to coat the positive and negative electrode active materials, the unpredictable performance problems caused by environmental impact of lithium powder materials in new energy batteries are solved, and the performance of the electrode sheet and the stability and safety of the battery are improved. sex.

CN118919719AInactive Publication Date: 2024-11-08SHENZHEN BTR NEW ENERGY TECH RES INST CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410874576.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-28
Publication Date
2024-11-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

When existing lithium-containing powder materials are used as positive and negative electrode coating materials in new energy batteries, they are easily affected by the environment, resulting in unpredictable powder performance and electrochemical performance, affecting the stability and application effect of the battery.

Method used

The chemical formula of the powder material is LiaMbNcRdPeTfOg, and a spherical conductive material is prepared through specific element combinations and process processing, and used to coat the positive electrode active material and the negative electrode active material to improve the performance of the electrode sheet.

Benefits of technology

Through the coating treatment, the compaction density and electrochemical performance of the electrode sheet are significantly improved, the cycle retention rate and volume energy density of the battery are enhanced, the volume expansion after high-temperature storage is reduced, and the safety performance is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118919719A_ABST
    Figure CN118919719A_ABST
Patent Text Reader

Abstract

The invention discloses a battery, a pole piece, a conductive material and a preparation method of the conductive material. Wherein the conductive material is a powder material, and the chemical formula of the powder material is Li M N < c > R < d > P < e > T < f > O < g >; the primary particles and / or the secondary particles of the powder material are / is spheroid; the spheroid is provided with a first short shaft, a second short shaft and a long shaft; the long shaft is perpendicular to the plane where the first short shaft and the second short shaft are located. The sizes of the spheroid on the first short axis, the second short axis and the long axis are x, y and z respectively, z / x is larger than or equal to 1 and smaller than 2, and z / y is larger than or equal to 1 and smaller than 2. The battery, the pole piece, the conductive material and the preparation method thereof have the beneficial effects that the performance of the pole piece can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of new energy technology, and in particular to a battery, electrode, conductive material and its preparation method. Background Technology

[0002] In the related technologies of new energy batteries, lithium-containing powder materials are used to coat the positive and negative electrode active materials; commonly used lithium-containing powder materials include LATP, LLZO, LLZTO, etc.

[0003] However, these lithium-containing powder materials, when used as coating materials for positive and negative electrodes, can have unpredictable effects on their performance and electrochemical performance after being applied to new energy batteries due to environmental influences during storage. Summary of the Invention

[0004] In view of this, this application provides a battery, an electrode, a conductive material, and a method for preparing the same, aiming to improve the existing problems.

[0005] The embodiments of this application are implemented as follows: a conductive material includes a powder material, the chemical formula of which is Li. a M b N c R d P e T f O g ;

[0006] Wherein, M is selected from at least one of In, Sc, B, Ga, Nb, Y, Zr, Al, Ni, Co, Mn, Mg, Ca, Sr, Cu, Zn, Fe, Na, and K;

[0007] Wherein, N is selected from at least one of Ti, Zr, Hf, Si, Ge, and Sn;

[0008] Wherein, R is selected from at least one of Nb, Ti, Zr, Hf, As, Sb, Si, Ge, and Sn; R and N are not the same element;

[0009] Wherein, T is selected from at least one of S, Se, N, F, Cl, Br, and I;

[0010] The primary and / or secondary particles of the powder material are spheroids; each spheroid has a first minor axis, a second minor axis, and a major axis; the major axis is perpendicular to the plane containing the first and second minor axes; the dimensions of the spheroid along the first minor axis, the second minor axis, and the major axis are x, y, and z, respectively, where 1 ≤ z / x < 2, 1 ≤ z / y < 2; the value of the dimension z along the major axis of the spheroid is in the range of 0.014 μm ≤ z ≤ 0.5 μm.

[0011] Wherein, d / (b+c+d+e) is defined as the first metrological characteristic value A; and f / (f+g) is defined as the second metrological characteristic value B.

[0012] The range of the first measurement characteristic value A is 0.005 < A ≤ 0.6; the range of the second measurement characteristic value B is 0.001 < B ≤ 0.4.

[0013] Optionally, in some embodiments of this application, the spheroidal body has a dimensional range of 0.014 μm ≤ x ≤ 0.5 μm for the size x of the first minor axis.

[0014] Optionally, in some embodiments of this application, the spheroidal body has a dimensional value y of the second minor axis ranging from 0.014 μm to 0.5 μm.

[0015] Optionally, in some embodiments of this application, the range of the first measurement feature value A is 0.015≤A≤0.2; and the range of the second measurement feature value B is 0.005<B≤0.35.

[0016] Optionally, in some embodiments of this application, wherein the Li a M b N c R d P e T f O g In the given information, 1 < a ≤ 6, 0 < b < 1, 0 < c < 2, 0 < d < 3, 0 < e < 3, 0 < f < 8, and 0 < g < 12.

[0017] Accordingly, this application also provides a method for preparing a conductive material, comprising the following steps:

[0018] Step 1: Based on the chemical formula Li of the powder material a M b N c R d P e T f O g Provide the raw materials to be mixed, corresponding to each element;

[0019] Step 2: Mix the various raw materials to be mixed provided in Step 1 to obtain the precursor material;

[0020] Step 3: The precursor material obtained in Step 2 is subjected to heat treatment to obtain a heat-treated product;

[0021] Step 4: The heat-treated product obtained in Step 3 is crushed, ball-milled, dried, and sieved to obtain the powder material;

[0022] Wherein, M is selected from at least one of In, Sc, B, Ga, Nb, Y, Zr, Al, Ni, Co, Mn, Mg, Ca, Sr, Cu, Zn, Fe, Na, and K;

[0023] Wherein, N is selected from at least one of Ti, Zr, Hf, Si, Ge, and Sn;

[0024] Wherein, R is selected from at least one of Nb, Ti, Zr, Hf, As, Sb, Si, Ge, and Sn; R and N are not the same element;

[0025] Wherein, T is selected from at least one of S, Se, N, F, Cl, Br, and I;

[0026] The primary and / or secondary particles of the powder material are spheroids; each spheroid has a first minor axis, a second minor axis, and a major axis; the major axis is perpendicular to the plane containing the first and second minor axes; the dimensions of the spheroid along the first minor axis, the second minor axis, and the major axis are x, y, and z, respectively, where 1 ≤ z / x < 2, 1 ≤ z / y < 2; the value of the dimension z along the major axis of the spheroid is in the range of 0.014 μm ≤ z ≤ 0.5 μm.

[0027] Wherein, d / (b+c+d+e) is defined as the first metrological characteristic value A; and f / (f+g) is defined as the second metrological characteristic value B.

[0028] The range of the first measurement characteristic value A is 0.015 < A ≤ 0.6; the range of the second measurement characteristic value B is 0.005 < B ≤ 0.4.

[0029] Optionally, in some embodiments of this application, the preparation method further includes the following steps:

[0030] Step 5: Coat the positive electrode active material and / or negative electrode active material with the powder material.

[0031] Optionally, in some embodiments of this application, the positive electrode active material is selected from at least one of NCM, NCA, LNMO, LCO, LFP, and LFMP.

[0032] Optionally, in some embodiments of this application, the negative electrode active material is selected from at least one of graphite, silicon carbide, silicon oxide, nano-silicon, LTO, lithium metal, and lithium alloy.

[0033] Accordingly, embodiments of this application also provide an electrode sheet made of the aforementioned conductive material; and / or made of a conductive material prepared by the aforementioned preparation method.

[0034] Accordingly, embodiments of this application also provide a battery, including the aforementioned electrode.

[0035] The advantage of this application is that it provides a battery, electrode, conductive material, and preparation method thereof that can improve the performance of the electrode. Attached Figure Description

[0036] To more clearly illustrate the technical solutions in the embodiments of this application, the accompanying drawings used in the description of the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0037] Figure 1 This is a SEM image of a 30μm-micron-sized powder material provided in this application;

[0038] Figure 2 This is a SEM image of a 350nm nanoscale powder material provided in Example 1 of this application;

[0039] Figure 3 This is a SEM image of a 30nm-nanometer-scale powder material provided in this application;

[0040] Figure 4 This is a schematic diagram of the defined axes of a powder material provided in an embodiment of this application;

[0041] Figure 5 This is a schematic diagram of a preparation method provided in an embodiment of this application. Detailed Implementation

[0042] The technical solutions of the embodiments of this application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of this application, and not all embodiments. Based on the embodiments of this application, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this application. Furthermore, it should be understood that the specific embodiments described herein are only for illustration and explanation of this application and are not intended to limit this application.

[0043] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. The terminology used herein in the specification of this invention is for the purpose of describing particular embodiments only and is not intended to be limiting of the invention. The term "and / or" as used herein includes any and all combinations of one or more of the associated listed items.

[0044] In this application, unless otherwise stated, directional terms such as "upper" and "lower" generally refer to the upper and lower positions of the device in its actual use or operating state, specifically the drawing directions in the accompanying drawings; while "inner" and "outer" refer to the outline of the device. Furthermore, in the description of this application, the term "comprising" means "including but not limited to". The terms first, second, third, etc., are used merely as illustrative purposes and do not impose numerical requirements or establish a numerical order.

[0045] In this application, "and / or" describes the relationship between related objects, indicating that three relationships can exist. For example, A and / or B can represent: A existing alone, A and B existing simultaneously, or B existing alone. A and B can be singular or plural.

[0046] In this application, "at least one" means one or more, and "more than one" means two or more. "One or more", "at least one of the following", or similar expressions refer to any combination of these items, including any combination of single or multiple items. For example, "at least one of a, b, or c", or "at least one of a, b, and c", can both mean: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, and c can be single or multiple.

[0047] In this application, the term "on" forming another layer on a certain layer is a broad concept. It can mean that the formed other layer is adjacent to a certain layer, or it can mean that there are other spacer structures between the other layer and the certain layer. For example, when a second electrode is formed "on" a first charge carrier functional layer, the term "on" can mean that the formed second electrode is adjacent to the first charge carrier functional layer, or it can mean that there are other spacer structures between the second electrode and the first charge carrier functional layer, such as a light-emitting layer.

[0048] Various embodiments of this application may exist in the form of a range; it should be understood that the description in the form of a range is merely for convenience and brevity and should not be construed as a hard limitation on the scope of this application; therefore, it should be considered that the range description has specifically disclosed all possible sub-ranges and single numerical values ​​within that range. For example, it should be considered that the range description from 1 to 6 has specifically disclosed sub-ranges such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., and single numbers within the range, such as 1, 2, 3, 4, 5, and 6, regardless of the range. Furthermore, whenever a numerical range is referred to herein, it means including any referenced number (fraction or integer) within the referred range.

[0049] The technical solution of this application is as follows:

[0050] In a first aspect, embodiments of this application provide a conductive material, including: a powder material.

[0051] The chemical formula of the powder material is Li a M b N c R d P e T f O g ;

[0052] Wherein, M is selected from at least one of In, Sc, B, Ga, Nb, Y, Zr, Al, Ni, Co, Mn, Mg, Ca, Sr, Cu, Zn, Fe, Na, and K;

[0053] Wherein, N is selected from at least one of Ti, Zr, Hf, Si, Ge, and Sn;

[0054] R is selected from at least one of Nb, Ti, Zr, Hf, As, Sb, Si, Ge, and Sn; R and N are not the same element.

[0055] Wherein, T is selected from at least one of S, Se, N, F, Cl, Br, and I;

[0056] The primary and / or secondary particles of the powder material are spheroids; each spheroid has a first minor axis, a second minor axis, and a major axis; the major axis is perpendicular to the plane containing the first and second minor axes; the dimensions of the spheroid along the first minor axis, the second minor axis, and the major axis are x, y, and z, respectively, where 1 ≤ z / x < 2, 1 ≤ z / y < 2; the value of the dimension z along the major axis of the spheroid is in the range of 0.014 μm ≤ z ≤ 0.5 μm.

[0057] Wherein, d / (b+c+d+e) is defined as the first metrological characteristic value A; and f / (f+g) is defined as the second metrological characteristic value B.

[0058] The range of the first measurement characteristic value A is 0.005 < A ≤ 0.6; the range of the second measurement characteristic value B is 0.001 < B ≤ 0.4.

[0059] Optionally, in some embodiments of this application, the spheroidal body has a dimensional range of 0.014 μm ≤ x ≤ 0.5 μm for the size x of the first minor axis.

[0060] Optionally, in some embodiments of this application, the spheroidal body has a dimensional value y of the second minor axis ranging from 0.014 μm to 0.5 μm.

[0061] Optionally, in some embodiments of this application, the range of the first measurement feature value A is 0.015≤A≤0.2; and the range of the second measurement feature value B is 0.005<B≤0.35.

[0062] Optionally, in some embodiments of this application, wherein the Li a M b N c S d P e T f O g In the given information, 1 < a ≤ 6, 0 < b < 1, 0 < c < 2, 0 < d < 3, 0 < e < 3, 0 < f < 8, and 0 < g < 12.

[0063] Secondly, embodiments of this application also provide a method for preparing a conductive material, comprising the following steps:

[0064] S101: According to the chemical formula Li of the powder material a M b N c R d P e T f O g Provide the raw materials to be mixed, corresponding to each element.

[0065] S102: Mix the various raw materials to be mixed provided in step one to obtain a precursor material.

[0066] S103: The precursor material obtained in step two is subjected to heat treatment to obtain a heat-treated product.

[0067] S104: The heat-treated product obtained in step three is crushed, ball-milled, dried, and sieved to obtain the powder material.

[0068] S105: Use the powder material to coat the positive electrode active material and / or the negative electrode active material.

[0069] Wherein, M is selected from at least one of In, Sc, B, Ga, Nb, Y, Zr, Al, Ni, Co, Mn, Mg, Ca, Sr, Cu, Zn, Fe, Na, and K; N is selected from at least one of Ti, Zr, Hf, Si, Ge, and Sn; R is selected from at least one of Nb, Ti, Zr, Hf, As, Sb, Si, Ge, and Sn; R and N are not the same element; T is selected from at least one of S, Se, N, F, Cl, Br, and I.

[0070] Optionally, in some embodiments of this application, the positive electrode active material is selected from at least one of NCM, NCA, LNMO, LCO, LFP, and LFMP.

[0071] Optionally, in some embodiments of this application, the negative electrode active material is selected from at least one of graphite, silicon carbide, silicon oxide, nano-silicon, LTO, lithium metal, and lithium alloy.

[0072] Optionally, in some embodiments of this application, the raw materials in step S101 may be: Li2CO3, Al2O3, TiO2, SiO2, NH4H2PO4, or LiF. Li2CO3 needs to be prepared in 15wt% excess according to the stoichiometric formula.

[0073] Optionally, in some embodiments of this application, the specific method of step S102 is as follows:

[0074] The raw materials to be mixed are added to the dispersant in a certain order, and then thoroughly mixed by wet milling. After the wet milling is completed, the mixture is dried.

[0075] As an optional option, the dispersant used in wet milling is selected from one or more of ethanol, propanol, isopropanol, butanol, water, NMP, DMF and acetone.

[0076] Optionally, in some embodiments of this application, the mass percentage of the powder material relative to the positive electrode active material when coating the positive electrode active material ranges from 0.05 to 1% wt; the mass percentage of the powder material relative to the negative electrode active material when coating the negative electrode active material ranges from 0.05 to 3% wt.

[0077] Optionally, in some embodiments of this application, the specific method of step S105 is: mixing and sintering the powder material with the positive electrode active material or the negative electrode active material according to the mass ratio.

[0078] Optionally, in some embodiments of this application, the positive electrode active material is selected from NCM, NCA, LNMO, and LCO; and the powder material is sintered in an oxygen atmosphere when coating the positive electrode active material.

[0079] Optionally, in some embodiments of this application, when the positive electrode active material is selected from LFP and LFMP, the powder material is sintered in an inert atmosphere when coating the positive electrode active material.

[0080] Optionally, in some embodiments of this application, the sintering temperature of the powder material coating the positive electrode active material ranges from 300 to 1000°C; the sintering time ranges from 4 to 12 hours; and the temperature rise rate ranges from 1 to 10°C / min.

[0081] Optionally, in some embodiments of this application, when the negative electrode active material is graphite, silicon carbide, silicon oxide, nano-silicon, LTO, etc., the powder material is sintered in an inert atmosphere when coating the negative electrode active material.

[0082] Optionally, in some embodiments of this application, when the negative electrode active material is lithium metal and lithium alloy, a coating of the powder material is applied to their surface, and the coating thickness ranges from 0.05 to 5 μm.

[0083] As an optional option, the wet grinding reagent used for wet grinding is selected from one or more of ethanol, propanol, isopropanol, butanol, water, NMP, DMF and acetone.

[0084] Among the optional methods, wet milling mixing can include, but is not limited to, ball milling, sand milling, high-speed dispersion, liquid phase spraying, and electrospinning.

[0085] Among the optional options, the specific drying methods include, but are not limited to, oven drying, belt drying, microwave drying, rotary evaporator, freeze drying, centrifugal drying, and single cone drying.

[0086] Optionally, in some embodiments of this application, the temperature range of the heat treatment in step S103 is 300 to 1000°C.

[0087] Optionally, in some embodiments of this application, the heat treatment time in step S103 is in the range of 4 to 12 hours.

[0088] Optionally, in some embodiments of this application, the heating rate of the heat treatment in step S103 ranges from 1 to 10 °C / min.

[0089] Optionally, in some embodiments of this application, the equipment used for the crushing process in step S104 includes, but is not limited to, a jaw crusher, a ball mill, a sand mill, and an air crusher. Alternatively, two or more crushing processes can be performed.

[0090] Thirdly, embodiments of this application also provide an electrode sheet made of the aforementioned conductive material; and / or made of a conductive material prepared by the aforementioned preparation method.

[0091] Fourthly, embodiments of this application also provide a battery, including the aforementioned electrode.

[0092] The present application will be further described below with reference to specific embodiments thereof.

[0093] Example 1

[0094] 1) A spherical Li with a particle size of 350 nm was prepared by VC mixing, sintering, and ball milling. 1.9 Al 0.4 Ti 1.6 Si 0.5 P 2. 5F 1.26 O 11.37 Lithium aluminum titanium phosphate solid electrolyte powder. Its specific preparation includes: using a molar ratio of Li, Al, Ti, Si, P, and F of 1.9:0.4:1.6:0.5:2.5:1.26, where A = 0.1 and B = 0.1. Li₂CO₃, Al₂O₃, TiO₂, SiO₂, NH₄H₂PO₄, and LiF as raw materials, with Li₂CO₃ in excess at 15 wt%, and the precursor powders are thoroughly mixed. Then, the mixture is heated at 900℃ for 12 h at a heating rate of 3℃ / min to obtain LATSPF powder. Further wet ball milling and sand milling are performed, followed by drying and sieving to obtain 350 nm spherical powder, denoted as SY-1.

[0095] 2) Select 2.5μm LFMP powder, SY-1, Al2O3 and ZrO2, mix them thoroughly at 98.5%, 0.6%, 0.5% and 0.4% respectively, and heat treat them at 600℃ for 4h under nitrogen atmosphere to obtain composite LFMP material, denoted as SY-C1.

[0096] 3) The above SY-1 and SY-C1 powders were placed in a vacuum oven at 200℃ for 20 hours to remove water. Morphology (statistical z / x, z / y), XRD, ionic conductivity, water absorption, specific surface area, and particle strength were tested. A positive electrode was prepared according to a ratio of SY-C1:conductive agent:binder = 96%:2%:2%, and the contact angle and electrode compaction density were tested. Together with Li metal, a Li||LFMP button cell was assembled, and the initial cycle efficiency, cycle capacity and retention rate at 1C current rate, and capacity and retention rate at high temperature were tested. Graphite, acetylene black, CMC, and SBR were weighed in a ratio of 95:2.5:1.5:1 to prepare an aqueous slurry, which was then coated with copper foil to prepare the negative electrode. Boehmite-coated PP separator, coated positive electrode, boehmite-coated PP separator, and graphite negative electrode were selected and assembled into a 2Ah AG||LFMP soft-pack battery of model 554065 by winding. The volumetric energy density, capacity retention after 500 cycles at 45℃, storage at 55℃ for 7 days, hot box at 150℃ for 30 minutes, and needle penetration safety performance were tested.

[0097] Example 2

[0098] 1) A spherical Li with a particle size of 350 nm was prepared by VC mixing, sintering, and ball milling. 1.9 Al 0.4 Ti 1.6 Si 0.5 P 2. 5F 1.26 O 11.37 Lithium aluminum titanium phosphate solid electrolyte powder. Its specific preparation includes: using a molar ratio of Li, Al, Ti, Si, P, and F of 1.9:0.4:1.6:0.5:2.5:1.26, where A = 0.1 and B = 0.1. Li₂CO₃, Al₂O₃, TiO₂, SiO₂, NH₄H₂PO₄, and LiF as raw materials, with Li₂CO₃ in excess at 15 wt%, and the precursor powders are thoroughly mixed. Then, the mixture is heated at 900℃ for 12 h at a heating rate of 3℃ / min to obtain LATSPF powder. Further wet ball milling and sand milling are performed, followed by drying and sieving to obtain 350 nm spherical powder, denoted as SY-2.

[0099] 2) Select 2.0μm SiC powder, SY-2, Al2O3 and LiF, mix them thoroughly at 98.5%, 0.6%, 0.4% and 0.5% respectively, and heat treat them at 600℃ for 4h under nitrogen atmosphere to obtain composite SiC material, denoted as SY-A2.

[0100] 3) The SY-2 and SY-A2 powders were placed in a vacuum oven at 200℃ for 20 hours to remove water. Morphology (statistical z / x, z / y), XRD, ionic conductivity, water absorption, specific surface area, and particle strength were tested. A negative electrode was prepared by weighing SY-A2 + graphite (SYA2 / graphite = 1 / 5), acetylene black, CMC, and SBR in a ratio of 95:2.5:1.5:1. The contact angle and electrode compaction density were tested. Together with Li metal, a Li||AG button cell was assembled. The initial cycle efficiency, cycle capacity and retention rate at 1C current rate, and capacity and retention rate at high temperature were tested. An NMP-based slurry was prepared by weighing NCM95:conductive agent:binder in a ratio of 96%:2%:2%, coated with aluminum foil, and used to prepare the positive electrode. Boehm-coated PP separator, positive electrode, boehm-coated PP separator, and graphite-SiC negative electrode were selected and assembled into a 2Ah AG||NCM95 soft-pack battery of model 554065 by winding. The volumetric energy density, capacity retention after 500 cycles at 45℃, storage at 55℃ for 7 days, hot box at 150℃ for 30 minutes, and needle penetration safety performance were tested.

[0101] Example 3

[0102] 1) A spherical Li with a particle size of 350 nm was prepared by VC mixing, sintering, and ball milling.1.9 Al 0.4 Ti 1.6 Si 0.5 P 2. 5F 1.26 O 11.37 Lithium aluminum titanium phosphate solid electrolyte powder. Its specific preparation includes: using a molar ratio of Li, Al, Ti, Si, P, and F of 1.9:0.4:1.6:0.5:2.5:1.26, where A = 0.1 and B = 0.1. Li₂CO₃, Al₂O₃, TiO₂, SiO₂, NH₄H₂PO₄, and LiF as raw materials, with Li₂CO₃ in excess at 15 wt%, and the precursor powders are thoroughly mixed. Then, the mixture is heated at 900℃ for 12 h at a heating rate of 3℃ / min to obtain LATSPF powder. Further wet ball milling and sand milling are performed, followed by drying and sieving to obtain 350 nm spherical powder, denoted as SY-3.

[0103] 2) Select 10μm LCO powder, SY-3, Al2O3 and ZrO2, mix them thoroughly at 98.5%, 0.6%, 0.5% and 0.4% respectively, and heat treat them at 600℃ for 4h in an oxygen atmosphere to obtain composite LCO material, denoted as SY-C3.

[0104] 3) The above SY-3 and SY-C3 powders were placed in a vacuum oven at 200℃ for 20 hours to remove water. Morphology (statistical z / x, z / y), XRD, ionic conductivity, water absorption, specific surface area, and particle strength were tested. A positive electrode was prepared according to a ratio of SY-C3:conductive agent:binder = 96%:2%:2%, and the contact angle and electrode compaction density were tested. Together with Li metal, a Li||LCO button cell was assembled, and the initial cycle efficiency, cycle capacity and retention rate at 1C current rate, and capacity and retention rate at high temperature were tested. Graphite, acetylene black, CMC, and SBR were weighed in a ratio of 95:2.5:1.5:1 to prepare an aqueous slurry, which was then coated with copper foil to prepare the negative electrode. Boehmite-coated PP separator, coated positive electrode, boehmite-coated PP separator, and graphite negative electrode were selected and assembled into a 2Ah AG||LCO pouch battery of model 554065 by winding. The volumetric energy density, capacity retention after 500 cycles at 45℃, storage at 55℃ for 7 days, hot box at 150℃ for 30 minutes, and needle penetration safety performance were tested.

[0105] Example 4

[0106] 1) A spherical Li with a particle size of 350 nm was prepared by VC mixing, sintering, and ball milling. 1.9 Al 0.4 Ti 1.6 Si 0.5 P 2. 5F 1.26O 11.37 Lithium aluminum titanium phosphate solid electrolyte powder. Its specific preparation includes: using a molar ratio of Li, Al, Ti, Si, P, and F of 1.9:0.4:1.6:0.5:2.5:1.26, where A = 0.1 and B = 0.1. LiOH (or Li₂CO₃), Al₂O₃, TiO₂, SiO₂, NH₄H₂PO₄, and LiF as raw materials, with LiOH (or Li₂CO₃) in excess at 15 wt%, and the precursor powders are thoroughly mixed. Then, the mixture is heated at 900℃ for 12 h at a heating rate of 3℃ / min to obtain LATSPF powder. Further wet ball milling and sand milling are performed, followed by drying and sieving to obtain 350 nm spherical powder, denoted as SY-4.

[0107] 2) Select 12.5μm NCM95 powder, SY-4, Al2O3 and ZrO2, mix them thoroughly at 98.5%, 0.6%, 0.5% and 0.4% respectively, and heat treat them at 600℃ for 4h in an oxygen atmosphere to obtain composite NCM95 material, denoted as SY-C4.

[0108] 3) The above SY-4 and SY-C4 powders were placed in a vacuum oven at 200℃ for 20 hours to remove water. Morphology (statistical z / x, z / y), XRD, ionic conductivity, water absorption, specific surface area, and particle strength were tested. A positive electrode was prepared according to a ratio of SY-C4:conductive agent:binder = 96%:2%:2%, and the contact angle and electrode compaction density were tested. Together with Li metal, a Li||NCM95 coin cell was assembled, and the initial cycle efficiency, cycle capacity and retention rate at 1C current rate, and capacity and retention rate at high temperature were tested. Graphite, acetylene black, CMC, and SBR were weighed in a ratio of 95:2.5:1.5:1 to prepare an aqueous slurry, which was then coated with copper foil to prepare the negative electrode. Boehmite-coated PP separator, coated positive electrode, boehmite-coated PP separator, and graphite negative electrode were selected and assembled into a 2Ah AG||NCM95 soft-pack battery of model 554065 by winding. The volumetric energy density, capacity retention after 500 cycles at 45℃, storage at 55℃ for 7 days, hot box at 150℃ for 30 minutes, and needle penetration safety performance were tested.

[0109] Example 5

[0110] 1) A spherical Li with a particle size of 200 nm was prepared by VC mixing, sintering, and ball milling. 1.9 Al 0.4 Ti 1.6 Si 0.5 P 2. 5F 1.26 O 11.37Lithium aluminum titanium phosphate solid electrolyte powder. Its specific preparation includes: using a molar ratio of Li, Al, Ti, Si, P, and F of 1.9:0.4:1.6:0.5:2.5:1.26, where A = 0.1 and B = 0.1. LiOH (or Li₂CO₃), Al₂O₃, TiO₂, SiO₂, NH₄H₂PO₄, and LiF as raw materials, with LiOH (or Li₂CO₃) in excess at 15 wt%, and the precursor powders are thoroughly mixed. Then, the mixture is heated at 900℃ for 12 h at a heating rate of 3℃ / min to obtain LATSPF powder. Further wet ball milling and sand milling are performed, followed by drying and sieving to obtain 200 nm spherical powder, denoted as SY-5.

[0111] 2) Select 10μm NCM95 powder, SY-5, Al2O3 and ZrO2, mix them thoroughly at 98.5%, 0.6%, 0.5% and 0.4% respectively, and heat treat them at 600℃ for 4h in an oxygen atmosphere to obtain composite LCO material, denoted as SY-C5.

[0112] 3) The above SY-5 and SY-C5 powders were placed in a vacuum oven at 200℃ for 20 hours to remove water. Morphology (statistical z / x, z / y), XRD, ionic conductivity, water absorption, specific surface area, and particle strength were tested. A positive electrode was prepared according to a ratio of SY-C5:conductive agent:binder = 96%:2%:2%, and the contact angle and electrode compaction density were tested. Together with Li metal, a Li||NCM95 coin cell was assembled, and the initial cycle efficiency, cycle capacity and retention rate at 1C current rate, and capacity and retention rate at high temperature were tested. Graphite, acetylene black, CMC, and SBR were weighed in a ratio of 95:2.5:1.5:1 to prepare an aqueous slurry, which was then coated with copper foil to prepare the negative electrode. Boehmite-coated PP separator, coated positive electrode, boehmite-coated PP separator, and graphite negative electrode were selected and assembled into a 2Ah AG||NCM95 soft-pack battery of model 554065 by winding. The volumetric energy density, capacity retention after 500 cycles at 45℃, storage at 55℃ for 7 days, hot box at 150℃ for 30 minutes, and needle penetration safety performance were tested.

[0113] Example 6

[0114] 1) A spherical Li with a particle size of 600 nm was prepared by VC mixing, sintering, and ball milling. 1.9 Al 0.4 Ti 1.6 Si 0.5 P 2. 5F 1.26 O 11.37Lithium aluminum titanium phosphate solid electrolyte powder. Its specific preparation includes: using a molar ratio of Li, Al, Ti, Si, P, and F of 1.9:0.4:1.6:0.5:2.5:1.26, where A = 0.1 and B = 0.1. Li₂CO₃, Al₂O₃, TiO₂, SiO₂, NH₄H₂PO₄, and LiF as raw materials, with Li₂CO₃ in excess at 15 wt%, and the precursor powders are thoroughly mixed. Then, the mixture is heated at 900℃ for 12 h at a heating rate of 3℃ / min to obtain LATSPF powder. Further wet ball milling and sand milling are performed, followed by drying and sieving to obtain 600 nm spherical powder, designated SY-6.

[0115] 2) Select 10μm NCM95 powder, SY-6, Al2O3 and ZrO2, mix them thoroughly at 98.5%, 0.6%, 0.5% and 0.4% respectively, and heat treat them at 600℃ for 4h in an oxygen atmosphere to obtain composite LCO material, denoted as SY-C6.

[0116] 3) The above SY-6 and SY-C6 powders were placed in a vacuum oven at 200℃ for 20 hours to remove water. Morphology (statistical z / x, z / y), XRD, ionic conductivity, water absorption, specific surface area, and particle strength were tested. A positive electrode was prepared according to the ratio of SY-C5:conductive agent:binder = 96%:2%:2%, and the contact angle and electrode compaction density were tested. Together with Li metal, a Li||NCM95 coin cell was assembled, and the initial cycle efficiency, cycle capacity and retention rate at 1C current rate, and capacity and retention rate at high temperature were tested. Graphite, acetylene black, CMC, and SBR were weighed in a ratio of 95:2.5:1.5:1 to prepare an aqueous slurry, which was then coated with copper foil to prepare the negative electrode. Boehmite-coated PP separator, coated positive electrode, boehmite-coated PP separator, and graphite negative electrode were selected and assembled into a 2Ah AG||NCM95 soft-pack battery of model 554065 by winding. The volumetric energy density, capacity retention after 500 cycles at 45℃, storage at 55℃ for 7 days, hot box at 150℃ for 30 minutes, and needle penetration safety performance were tested.

[0117] Example 7

[0118] 1) A spherical Li with a particle size of 1000 nm was prepared by VC mixing, sintering, and ball milling. 1.9 Al 0.4 Ti 1.6 Si 0.5 P 2. 5F 1.26 O 11.37Lithium aluminum titanium phosphate solid electrolyte powder. Its specific preparation includes: using a molar ratio of Li, Al, Ti, Si, P, and F of 1.9:0.4:1.6:0.5:2.5:1.26, where A = 0.1 and B = 0.1. Li₂CO₃, Al₂O₃, TiO₂, SiO₂, NH₄H₂PO₄, and LiF as raw materials, with Li₂CO₃ in excess at 15 wt%, and the precursor powders are thoroughly mixed. Then, the mixture is heated at 900℃ for 12 h at a heating rate of 3℃ / min to obtain LATSPF powder. Further wet ball milling and sand milling are performed, followed by drying and sieving to obtain 1000 nm spherical powder, designated SY-7.

[0119] 2) Select 10μm NCM95 powder, SY-7, Al2O3 and ZrO2, mix them thoroughly at 98.5%, 0.6%, 0.5% and 0.4% respectively, and heat treat them at 600℃ for 4h in an oxygen atmosphere to obtain composite LCO material, denoted as SY-C7.

[0120] 3) The above SY-7 and SY-C7 powders were placed in a vacuum oven at 200℃ for 20 hours to remove water. Morphology (statistical z / x, z / y), XRD, ionic conductivity, water absorption, specific surface area, and particle strength were tested. Positive electrode sheets were prepared according to a ratio of SY-C7:conductive agent:binder = 96%:2%:2%, and the contact angle and electrode compaction density were tested. Together with Li metal, they were assembled into Li||NCM95 button cells. The initial cycle efficiency, cycle capacity and retention rate at 1C current rate, and capacity and retention rate at high temperature were tested. Graphite, acetylene black, CMC, and SBR were weighed in a ratio of 95:2.5:1.5:1 to prepare an aqueous slurry, which was then coated with copper foil to prepare the negative electrode sheet. Boehmite-coated PP separator, coated positive electrode, boehmite-coated PP separator, and graphite negative electrode were selected and assembled into a 2Ah AG||NCM95 soft-pack battery of model 554065 by winding. The volumetric energy density, capacity retention after 500 cycles at 45℃, storage at 55℃ for 7 days, hot box at 150℃ for 30 minutes, and needle penetration safety performance were tested.

[0121] Comparative Example 1

[0122] Same as Example 1, except that the LATP composition is Li 1.4 Al 0.4 Ti 1.6 P3O 12 , where A = 0, B = 0.

[0123] Comparative Example 2

[0124] Same as Example 2, except that the LATP composition is Li 1.4 Al 0.4 Ti 1.6P3O 12 , where A = 0, B = 0.

[0125] Comparative Example 3

[0126] Same as Example 3, except that the LATP composition is Li 1.4 Al 0.4 Ti 1.6 P3O 12 , where A = 0, B = 0.

[0127] Comparative Example 4

[0128] Same as Example 4, except that the LATP composition is Li 1.4 Al 0.4 Ti 1.6 P3O 12 , where A = 0, B = 0.

[0129] Comparative Example 5

[0130] Same as Example 5, except that the LATP composition is Li 1.4 Al 0.4 Ti 1.6 P3O 12 , where A = 0, B = 0.

[0131] Comparative Example 6

[0132] Same as Example 6, except that the LATP composition is Li 1.4 Al 0.4 Ti 1.6 P3O 12 , where A = 0, B = 0.

[0133] Comparative Example 7

[0134] Same as Example 7, except that the LATP composition is Li 1.4 Al 0.4 Ti 1.6 P3O 12 , where A = 0, B = 0.

[0135] Comparative Example 8

[0136] Same as Example 8, except that the LATP composition is Li 1.4 Al 0.4 Ti 1.6 P3O 12 , where A = 0, B = 0.

[0137] Comparative Example 9

[0138] Same as Example 9, but without LATP coating, the positive electrode is the LFMP reference sample, where A=0 and B=0.

[0139] Comparative Example 10

[0140] Same as Example 10, but without LATP coating, the negative electrode is a graphite-SiC reference sample, where A=0 and B=0.

[0141] Comparative Example 11

[0142] Same as Example 11, but without LATP coating, with NCM95 as the positive electrode, where A=0 and B=0.

[0143] The specific testing methods are as follows:

[0144] Physical and chemical property testing

[0145] Moisture content testing: GB / T 24533-2019 Karl Fischer method. The powder was dried at 200℃ for 24 hours, then placed in an environment at 25℃ and 60% humidity for different time periods to test moisture content. Moisture testing was performed in a drying chamber with a dew point below -35℃.

[0146] Lithium-ion conductivity detection: The AC impedance of the solid electrolyte sheet was measured using an electrochemical workstation, and the lithium-ion conductivity was calculated using a formula. The detection frequency was 1,000,000-0.01 Hz, the amplitude was 5 mA, and each sample was measured in triplicate. Sample preparation: 0.5 g of dry LATP powder was pressed into a sheet at 300 MPa for 1 min under a 15 mm diameter mold, maintaining a sheet thickness of 1-2 mm. The sheet was then heat-treated at 850℃ for 10 h, cooled to room temperature, and vacuum-sealed for storage, achieving a density >90%. The LATP sheet was uniformly gold-plated on both sides, and then the AC impedance spectrum was measured on an EC-Lab. A Swagelok mold (with Teflon insulation on the inner wall) was selected, and the two ends of the LATP sheet were connected with stainless steel sheets. The torque wrench was set to a pressure of 5 mN. The lithium-ion conductivity was calculated using the formula δ = l / (RS), where l and S are the sheet thickness and surface area, respectively, R is the measured AC impedance value, and δ is the lithium-ion conductivity.

[0147] Powder conductivity testing: GB / T30835-2014 "Carbon composite lithium iron phosphate cathode material for lithium-ion batteries". Four-probe testing principle: applied pressure range 10-200 MPa, pressure interval 10 MPa, holding pressure for 10 s, pressure released to 3 MPa, holding pressure for 10 s;

[0148] Phase detection: JY / T 0587-2020 General rules for polycrystalline X-ray diffraction methods.

[0149] Morphology inspection: JY / T 0584-2020 General Rules for Analysis Methods of Scanning Electron Microscopy.

[0150] Laser particle size distribution: Prepare a 10% solids-content aqueous solution, sonicate for 5 minutes, and measure the particle size using a Malvern 3000 laser. Select a refractive index of 2.42 and an absorbance of 1. Water is used as the dispersant, with a refractive index of 1.33.

[0151] Specific surface area testing: GB / T 19587-2017.

[0152] Contact angle testing: A contact angle meter is used to test the wettability of electrolyte, electrode slurry, diaphragm, and electrode sheet. Contact angle testing involves dropping electrolyte or water onto the surface of a solid electrolyte sheet / diaphragm / positive / negative electrode sheet using a contact angle meter, measuring the distance and height between the two ends of the droplet, and calculating the contact angle. The smaller the contact angle value, the better the hydrophilicity of the diaphragm.

[0153] Compacted density testing: GB / T 24533-2019 and GBT30835-2014 "Carbon composite lithium iron phosphate cathode material for lithium-ion batteries".

[0154] Electrochemical performance testing

[0155] Coin cell preparation and testing: GB / T 24533-2019. Ternary materials NCM95, Super P, and PVDF were weighed in a 96:2:2 ratio, dispersed in NMP slurry, and then coated onto a 16μm thick Al foil. The mixture was then vacuum-dried at 100℃ for 12 hours to serve as the positive electrode. CR232 coin cells were assembled using the above positive electrode, a boehmite-coated PP separator (coating thickness 2μm, separator thickness 9μm), and a Li metal negative electrode. The diameters of the positive and negative electrodes were 15mm, the separator diameter was 20mm, and the electrolyte was 1.2M LiPF6-EC / DEC / EMC + 1.5% VC + 1.5% FEC + 2.5% PS. 1C constant current charge-discharge testing was performed. The constant current charge-discharge voltage range was 2.5V-4.3V, and the current was 1C. If the positive electrode was AG and the negative electrode was Li, the corresponding constant current charge-discharge voltage range was 0.01V-1.5V.

[0156] Preparation and Testing of Pouch Cells: NCM95, Super P, and PVDF were weighed in a ratio of 96:2:2, dispersed in NMP slurry, and then coated on a 16-μm-thick Al foil, followed by vacuum drying at 80 °C for 12 h to obtain the positive electrode sheet. Graphite, acetylene black, CMC, and SBR were weighed in a ratio of 95:2.5:1.5:1, dispersed into an aqueous slurry, and then coated on a 10-μm-thick copper foil, followed by vacuum drying at 100 °C for 12 h to obtain the negative electrode sheet. A 2-Ah pouch cell was assembled using the above positive electrode sheet, a PP separator coated with boehmite (coating thickness 2 μm, separator 9 μm), and the negative electrode sheet. The electrolyte was a 1.2-M LiPF6-EC / DEC / EMC + 1.5% VC + 1.5% FEC + 2.5% PS battery, and 1C constant current charge-discharge testing was performed. The constant current charge-discharge voltage range was 2.5 V - 4.3 V, and the current was 1C. For all-solid-state batteries, the positive electrode sheet and the negative electrode were directly hot-pressed at a hot-pressing temperature of 300 °C, a pressure of 300 MPa for 20 s, and then encapsulated in an aluminum-plastic film to prepare a 2-Ah all-solid-state pouch cell. The constant current charge-discharge voltage range was 2.5 V - 4.3 V, and the current was 0.2C.

[0157] Battery Safety Performance Testing:

[0158] High-Temperature Thermal Storage Retention Rate and Recovery Rate: GB / T 31484-2015. For the fully charged battery, 1C full charge was performed, and it was stored at 55 °C for 7 days, cooled to 25 °C, and left standing for 4 h. The capacity retention rate and recovery rate were measured separately.

[0159] Hot Box Testing: GB / T 36276-2023 "Lithium-Ion Batteries for Electric Energy Storage". One 2-Ah pouch cell was placed in a high-temperature oven with protective measures, and a temperature-programmed treatment from 45 °C to 200 °C was carried out at a heating rate of 5 °C / min, and held at each 5 °C for 30 min for hot box safety testing to observe whether the battery caught fire, smoked, or exploded. There were 6 parallel samples in each group. <00004�2>Pin Prick Test: GB 31241-2014, GB / T 31485-2015, GB 38031-2020. A 2-Ah small pouch cell was selected, fully charged, and a high-temperature-resistant steel needle with a diameter of 5 - 8 mm was vertically penetrated through the battery electrode plate at a speed of (25 ± 5) mm / s. The steel needle was left in the battery for 1 hour, and it was considered qualified if there was no fire or explosion. It was required to have fire extinguishing facilities and an open environment around, and the operators should have professional capabilities and protective measures. There were 8 parallel samples in each group.

[0161] The test results are shown in Tables 1 to 4.

[0162] Table 1 shows the data of moisture detection of powder materials in different examples and comparative examples over time when placed in the same air environment.

[0163] Table 2 shows the physicochemical properties of the powder materials in different embodiments and comparative examples.

[0164] Table 3 shows the coin cell cycle performance test data of the powder materials used in different embodiments and comparative examples after they were used to construct coin cells.

[0165] Table 4 shows the safety performance test data of the powder materials used in different embodiments and comparative examples to construct pouch batteries.

[0166] Table 1

[0167] Table 2

[0168]

[0169] Table 3

[0170]

[0171] Table 4

[0172]

[0173] According to the experimental data, the technical solution of this application coats the positive and negative electrode active materials with 0.6% wt. spherical LMNSPTO material, which results in a higher compaction density of the positive and negative electrode sheets. Finally, the soft-pack battery achieves a larger volumetric energy density of 682 Wh / kg, which is more than 5% better.

[0174] Table 1 shows the moisture changes of LMNSPTO materials with different particle sizes and micron-sized NCM95 (polycrystalline NCM, 95% Ni, 1% Co, 4% Mn) cathode active materials after being exposed to air for different periods. The moisture content of both NCM95 and LMNSPTO materials increased over time. The increase was more pronounced in conventional LATP materials (Comparative Examples 1-7), significantly higher than that of the cathode powder, possibly due to the smaller size of LATP particles and the higher hygroscopicity of their phosphate ions. In contrast, the spherical LATP materials (Examples 1-7) exhibited reduced water absorption due to their lower specific surface area. Furthermore, the water absorption decreased somewhat with increasing LATP particle size, likely due to their even smaller specific surface area.

[0175] Table 2 shows the physicochemical properties of LMNSPTO materials and composite positive and negative electrode active materials and electrodes, as well as Examples 1-7 and Comparative Examples 1-11. When A = 0.1 and B = 0.1, the LMNSPTO material exhibits good sphericity, Z / X and Z / Y ratios are close to 1, and it demonstrates high phase purity and lithium-ion conductivity. Figure 1 and Figure 2The particle size of LATP spherical particles is controllable, ranging from approximately 20 nm to 30 μm. As the particle size of LATP powder increases, the specific surface area of ​​spherical LATP materials gradually decreases from 28.42 m² / g to 3.79 m² / g, while the specific surface area of ​​non-spherical LATP gradually decreases from 66.54 m² / g to 5.18 m² / g. After LMNSPTO coating the positive and negative electrodes, the specific surface area of ​​the composite materials in Examples 1-7 is somewhat lower than that of the composite materials in Comparative Examples 1-7. Simultaneously, the compaction density of the electrode sheets formed by coating non-spherical LMNSPTO decreases to some extent, while the compaction density of the electrode sheets formed by coating spherical LMNSPTO increases slightly. After LMNSPTO coating the positive and negative electrodes, the particle strength of the composite positive and negative electrode powder increases to some extent, while the increase is relatively smaller for spherical LMNSPTO. This indicates that LATP coating increases the material's hardness, making rolling more difficult. Under pressure, spherical LMNSPTO exhibits some elasticity, facilitating the translation of rolled particles to fill the positive electrode gaps. Non-spherical particles, being harder and unable to translate, may puncture the aluminum foil, causing the rolled electrode to become brittle and break. LMNSPTO coating improves the hydrophobic and electrophilic properties of the electrolyte, with a more significant improvement observed in positive and negative electrode sheets coated with spherical LMNSPTO material.

[0176] Table 3 shows the electrochemical properties of coin cells with LMNSPTO-coated positive and negative electrode active materials of different particle sizes. When A = 0.1 and B = 0.1, the sphericity of the LMNSPTO material is good, and Z / X and Z / Y are close to 1. After coating with LATP, the coin cell test results show a significant improvement in initial efficiency, initial capacity, and 1C cycle retention. In particular, the addition of spherical LATP material significantly improves the low-temperature cycling performance compared to Comparative Examples 8-11 (reference samples). A comparison of Examples 1-7 and Comparative Examples 1-7 shows that the excellent cycling performance may be due to the lower specific surface area and better hydrophobic-liquid properties of the spherical material, while its volume expansion after high-temperature storage is also greatly reduced. In particular, Example 2, after coating with silicon-carbon material, shows a significant improvement in initial efficiency, initial discharge capacity, and capacity retention (Comparative Examples 2 and 9).

[0177] Table 4 shows the electrochemical properties of pouch cells with LMNSPTO-coated positive and negative electrode active materials of different particle sizes. When A = 0.1 and B = 0.1, the sphericity of the LMNSPTO material is good, and Z / X and Z / Y are close to 1. Specifically, when A = 0.1 and B = 0.1, the pouch cell prepared with LMNSPTO material achieves higher capacity retention and recovery rates at 55℃ and less volume expansion, and its 150℃-30min hot box pass rate is also high. As shown in Example 2 and Comparative Example 9, the expansion rate is significantly reduced after coating the silicon-carbon anode. The volumetric energy density of the pouch cell increases by 5% after coating with spherical LMNSPTO, which may be attributed to its higher compaction density.

[0178] In summary, a spherical LMNSPTO with a particle size D50 range of 1.0≤Z / X≤1.2, 1.0≤Z / Y≤1.2, and Z≤1.2μm, and a coating amount of 0.6%, after coating the positive and negative electrodes, the electrode compaction density is improved to a certain extent. The resulting 2Ah soft-pack battery achieves a high cycle retention rate and volumetric energy density, with the highest volumetric energy density reaching 682.59Wh / kg, which is more than 5% higher than that of the uncoated battery.

[0179] The battery, electrode, conductive material and its preparation method provided in the embodiments of this application have been described in detail above. Specific examples have been used to illustrate the principles and implementation methods of this application. The description of the above embodiments is only for the purpose of helping to understand the method and core ideas of this application. At the same time, for those skilled in the art, there will be changes in the specific implementation methods and application scope based on the ideas of this application. Therefore, the content of this specification should not be construed as a limitation of this application.

Claims

1. A conductive material, characterized in that: The conductive material includes a powder material, the chemical formula of the powder material is Li a M b N c R d P e T f O g ; Wherein, M is selected from at least one of In, Sc, B, Ga, Nb, Y, Zr, Al, Ni, Co, Mn, Mg, Ca, Sr, Cu, Zn, Fe, Na, and K; Wherein, N is selected from at least one of Ti, Zr, Hf, Si, Ge, and Sn; Wherein, R is selected from at least one of Nb, Ti, Zr, Hf, As, Sb, Si, Ge, and Sn; R and N are selected from different elements; Wherein, T is selected from at least one of S, Se, N, F, Cl, Br, and I; The primary particles and / or secondary particles of the powder material are spheroids; the spheroids have a first short axis, a second short axis and a long axis; the long axis is perpendicular to the plane where the first short axis and the second short axis are located; the dimensions of the spheroids on the first short axis, the second short axis and the long axis are x, y, and z respectively, wherein 1≤z / x<2, 1≤z / y<2; the dimension z of the spheroids on the long axis ranges from 0.014μm≤z≤0.5μm, Wherein, d / (b+c+d+e) is defined as the first metrological characteristic value A; f / (f+g) is defined as the second metrological characteristic value B; The value range of the first metrological characteristic value A is 0.005<A≤0.6; the value range of the second metrological characteristic value B is 0.001<B≤0.

4.

2. The conductive material according to claim 1, wherein: The dimension x of the spheroid at the first minor axis ranges from 0.014 μm ≤ x ≤ 0.5 μm.

3. The conductive material according to claim 1, wherein: The value range of the dimension y of the spheroid at the second minor axis is 0.014 μm≤y≤0.5 μm.

4. The conductive material according to claim 1, wherein: The value range of the first metrological characteristic value A is 0.015≤A≤0.2; the value range of the second metrological characteristic value B is 0.005<B≤0.

35.

5. The conductive material according to claim 1, wherein: in, The Li a M b N c S d P e T f O g where 1 < a ≤ 6, 0 < b < 1, 0 < c < 2, 0 < d < 3, 0 < e < 3, 0 < f < 8, 0 < g < 12.

6. A method for preparing a conductive material, characterized in that: The preparation method comprises the following steps: Step 1: According to the chemical formula of the powder material Li a M b N c R d P e T f O g Providing raw materials to be mixed corresponding to each element; Step 2: Mixing the multiple raw materials to be mixed provided in step 1 to obtain a precursor material; Step 3: heat-treating the precursor material obtained in step 2 to obtain a heat-treated product; Step 4: crushing, ball milling, drying and sieving the heat-treated product obtained in step 3 to obtain the powder material; Step 5: using the powder material to coat the positive electrode active material and / or the negative electrode active material; Wherein, M is selected from at least one of In, Sc, B, Ga, Nb, Y, Zr, Al, Ni, Co, Mn, Mg, Ca, Sr, Cu, Zn, Fe, Na, and K; Wherein, N is selected from at least one of Ti, Zr, Hf, Si, Ge, and Sn; Wherein, R is selected from at least one of Nb, Ti, Zr, Hf, As, Sb, Si, Ge, and Sn; Wherein, T is selected from at least one of S, Se, N, F, Cl, Br, and I; The primary particles and / or secondary particles of the powder material are spheroids; the spheroids have a first short axis, a second short axis and a long axis; the long axis is perpendicular to the plane where the first short axis and the second short axis are located; the dimensions of the spheroids on the first short axis, the second short axis and the long axis are x, y, and z respectively, wherein 1≤z / x<2, 1≤z / y<2; the dimension z of the spheroids on the long axis ranges from 0.014μm≤z≤0.5μm, Wherein, d / (b+c+d+e) is defined as the first metrological characteristic value A; f / (f+g) is defined as the second metrological characteristic value B; The value range of the first metrological characteristic value A is 0.005<A≤0.6; the value range of the second metrological characteristic value B is 0.001<B≤0.

4.

7. The preparation method according to claim 6, characterized in that: in, The positive electrode active material is selected from at least one of NCM, NCA, LNMO, LCO, LFP, and LFMP.

8. The preparation method according to claim 6, characterized in that: in, The negative electrode active material is selected from at least one of graphite, silicon carbon, silicon oxygen, nano silicon, LTO, lithium metal, and lithium alloy.

9. A pole piece, characterized in that: Made of the conductive material described in any one of claims 1 to 5; and / or made of the conductive material prepared by the preparation method described in any one of claims 6 to 8.

10. A battery, characterized in that: Including the pole piece as claimed in claim 9.

Citation Information

Patent Citations

  • NASICON type solid lithium-ion electrolyte and preparation method thereof

    CN101894972A

  • In-situ composite lithium battery negative electrode material and preparation method and application thereof

    CN110034280A

  • Rechargeable high-safety lithium battery

    CN117039114A

  • Solid Electrolyte Sensor for Oxygen Concentration in Gas Environments

    RU2012152300A

  • Nasicon-type solid electrolyte, positive electrode material coated with same, and preparation methods therefor

    WO2023056748A1