High-durability and high-activity core-shell structure Pt and C catalyst and preparation method thereof

The preparation of core-shell structures Pt and C catalysts through high-voltage electrospinning technology has solved the problems of few active sites and low durability of platinum carbon catalysts in the prior art, achieved high durability and high activity of the catalyst, and extended the fuel cell service life.

CN118919741APending Publication Date: 2024-11-08ANHUI TOMORROW HYDROGEN ENERGY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411018903.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

There are few active sites of platinum carbon catalysts in existing proton exchange membrane fuel cells, resulting in low catalytic activity and agglomeration and migration of platinum particles during long-term operation, reducing catalyst activity, damaging proton membranes, and affecting battery performance and durability.

Method used

The core-shell structure Pt and C catalysts were prepared by high-pressure electrospinning technology. The outer core and inner core precursor solutions were uniformly mixed by ultrasonic and magnetic stirring, and the outer core and inner core precursor solutions were sintered at high temperature and three-stage sintered in a hydrogen atmosphere to form uniformly embedded platinum particles, which improved The durability of the carbon support and the catalyst slurry is formed by perfluorosulfonic acid resin and isopropanol, sprayed onto the proton exchange membrane.

Benefits of technology

It improves the durability and active sites of the catalyst, reduces the agglomeration and migration of platinum particles, enhances electrochemical activity, extends the service life of the battery, and avoids the influence of oxygen impurities through hydrogen protection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118919741A_ABST
    Figure CN118919741A_ABST
Patent Text Reader

Abstract

The invention discloses a core-shell structure Pt and C catalyst with high durability and high activity and a preparation method thereof, and relates to the field of fuel cells. Comprising the following steps: preparing chemicals PAN, N, N-dimethylformamide and chloroplatinic acid, mixing N, N-dimethylformamide, PAN and chloroplatinic acid powder, and uniformly mixing by ultrasonic and magnetic stirring to obtain an outer core precursor solution; meanwhile, preparing a PMMA (Polymethyl Methacrylate) solution, and uniformly mixing by ultrasonic and magnetic stirring to serve as a core precursor solution; and respectively transferring the solutions into an injector, spinning by using a high-voltage electrostatic spinning machine, and collecting the nanofiber membrane by using an aluminum foil. According to the invention, platinum can be uniformly embedded into the carbon nanofibers, the occurrence of platinum particle aggregation and migration in the chemical reaction process is reduced, the Oersted curing phenomenon is weakened, meanwhile, through three-stage high-temperature sintering, the reaction in each stage can be fully carried out, and the carbon carrier is more resistant to carbon oxidation, so that the catalyst shows excellent durability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of fuel cells, and in particular to a highly durable and highly active core-shell structured Pt, C catalyst and a preparation method thereof. Background Art

[0002] Proton exchange membrane fuel cell (PEMFC) is an advanced energy conversion technology that can directly convert chemical energy into electrical energy without going through the traditional combustion process. This type of battery has high-efficiency energy conversion, zero emissions, and can be quickly started at relatively low temperatures, so it has broad application prospects in many fields. In proton exchange membrane fuel cells, the membrane electrode assembly (MEA) plays a key role, which directly affects the performance of the fuel cell. MEA includes a proton exchange membrane, anode and cathode catalyst layers, and gas diffusion layers located on the anode and cathode respectively. These components work together to affect the overall function of the membrane electrode.

[0003] The catalytic layer in the membrane electrode is generally composed of a catalyst and a resin, in which the catalyst plays the main electrocatalytic role, promoting the electrochemical reaction of hydrogen (at the anode) and oxygen (at the cathode). Platinum-carbon catalyst is a common type of catalyst, and the activity and durability of the catalyst play an important role in the performance and durability of the entire fuel cell. In practical applications, the utilization rate of platinum on carbon carriers is very limited, and the electrochemical phenomenon exhibited is a small number of active sites, resulting in a small electrochemical active area and low catalytic activity; at the same time, due to long-term changes in operating conditions, platinum particles agglomerate and migrate, reducing the original catalytic activity of the catalyst, and may also damage the proton membrane due to overheating of the local catalyst reaction, resulting in membrane electrode failure.

[0004] To this end, the present invention proposes a highly durable and highly active core-shell structured Pt, C catalyst and a preparation method thereof, aiming to solve the above-mentioned problems existing in the prior art. Summary of the invention

[0005] The purpose of the present invention is to solve the shortcomings of the prior art and to propose a highly durable and highly active core-shell structured Pt, C catalyst and a preparation method thereof.

[0006] In order to achieve the above object, the present invention adopts the following technical solutions:

[0007] A method for preparing a highly durable and highly active core-shell structured Pt, C catalyst comprises the following steps:

[0008] S1: Prepare chemical reagents PAN, N,N-dimethylformamide and chloroplatinic acid, mix N,N-dimethylformamide, PAN and chloroplatinic acid powder, and mix them evenly by ultrasonic + magnetic stirring to use as outer core precursor solution; at the same time, prepare PMMA solution, and mix them evenly by ultrasonic + magnetic stirring to use as inner core precursor solution;

[0009] S2: The solutions were transferred into syringes and spun using a high-voltage electrospinning machine, and the nanofiber membranes were collected using aluminum foil;

[0010] S3: The collected nanofiber membranes are placed in an ark and loaded into a closed tubular high-temperature sintering furnace for sintering, and hydrogen is continuously introduced during the sintering process;

[0011] S4: Grinding the sintered sample into powder, adding the ground sample into a perfluorosulfonic acid resin solution, water and isopropanol to form an ink-like slurry, and then dispersing it at high speed to make it a uniformly dispersed catalyst slurry;

[0012] S5: The catalyst slurry is sprayed on both sides of the proton exchange membrane, and then the gas diffusion layer is placed on both sides, and a single cell is prepared using a graphite single serpentine electrode plate.

[0013] Preferably: the PAN content of the PMMA solution in step S1 is 25%.

[0014] Preferably: in the step S2, the voltage difference between the positive and negative electrodes of the high-voltage electrospinning machine is 20 kV, the outer core flow rate is 1.0 mL / h, the inner core solution flow rate is 0.2-0.6 mL / h, and the receiving distance is 15 cm.

[0015] Preferably, in step S3, the sintering is performed in three stages, which are:

[0016] S31: In the first stage, the temperature is raised from room temperature to 270 degrees Celsius and kept for 1 hour;

[0017] S32: The second stage is from 270 degrees Celsius to 400 degrees Celsius, and the temperature is kept for 1 hour;

[0018] S33: The third stage is to increase the temperature from 400°C to 1000°C, keep it at that temperature for 1 hour and then cool it naturally.

[0019] Preferably: in the step S3, hydrogen is introduced from the air inlet at the top of the sintering furnace, and an exhaust port is arranged at the bottom of the sintering furnace, and opening valves are installed on the outside of the air inlet and the exhaust port, and the opening degree of the opening valve located at the air inlet is larger than the opening degree of the opening valve located at the exhaust port.

[0020] Preferably: in the step S4, the Nafion content of the perfluorosulfonic acid resin solution is 5%; the high-speed dispersion speed is 30 m / s, the dispersion time is 30 min, and the temperature of the slurry during dispersion is lower than 20 degrees Celsius.

[0021] Preferably: in the step S4, the solid content of the slurry is 2.7%, and the volume ratio of water to isopropanol is 1 / 5.

[0022] Preferably: in step S5, the thickness of the proton exchange membrane is 12 μm.

[0023] Preferably: in the step S5, the spraying temperature is 90 degrees Celsius and the spraying area is 5*5cm 2 .

[0024] Preferably: in step S5, the total CCM loading is 0.5 mg / cm 2 The loading ratio between the anode surface and the cathode surface is 1 / 4, and the thickness of the gas diffusion layer is 180 μm.

[0025] A highly durable and highly active core-shell structure Pt, C catalyst comprising PAN, N,N-dimethylformamide, chloroplatinic acid, perfluorosulfonic acid resin solution, water and isopropanol

[0026] The beneficial effects of the present invention are:

[0027] 1. The present invention can evenly embed platinum into carbon nanofibers, reduce the occurrence of platinum particle agglomeration and migration during the chemical reaction, weaken the Oersted ripening phenomenon, and at the same time, after three-stage high-temperature sintering, each stage of the reaction can be fully carried out, the carbon carrier is more resistant to carbon oxidation, and the catalyst exhibits excellent durability.

[0028] 2. The platinum particles deposited on the carbon nanofibers of the present invention are exposed on both the inner shell and the outer shell, and the active sites are increased, thereby effectively improving the catalyst activity.

[0029] 3. The present invention adopts hydrogen atmosphere protection during the sintering process, thereby preventing the influence of other impurity gases such as oxygen on the purity during sintering, and controls the introduction position, discharge position and opening of hydrogen, utilizing the characteristic that the relative molecular mass of hydrogen is smaller than that of air, thereby ensuring the sufficiency of air discharge in the sintering furnace and increasing the sintering effect. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 This is a flow chart of a method for preparing a highly durable and highly active core-shell structure Pt, C catalyst proposed by the present invention;

[0031] Figure 2A comparison diagram of polarization curves of Examples 1-3 and Comparative Example 1 of a method for preparing a highly durable and highly active core-shell structure Pt, C catalyst proposed by the present invention;

[0032] Figure 3 This is a TEM morphology comparison diagram of an embodiment and a comparative example of a preparation method for a highly durable and highly active core-shell structured Pt, C catalyst proposed by the present invention. DETAILED DESCRIPTION

[0033] The technical solution of the present invention is further described in detail below in conjunction with specific implementation methods.

[0034] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", and "set" should be understood in a broad sense, for example, they can be fixedly connected or set, or detachably connected or set, or integrally connected or set. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0035] (1) Prepare chemicals PAN, N,N-dimethylformamide (DMF) and chloroplatinic acid. Mix 10 mL DMF, 1 g PAN and 0.2 g chloroplatinic acid powder, and mix them evenly by ultrasonic + magnetic stirring to use as the outer core precursor solution; at the same time, prepare a 25% PAN PMMA solution, and mix them evenly by ultrasonic + magnetic stirring to use as the inner core precursor solution. (2) Transfer the solutions to syringes for spinning. Use a high-voltage electrospinning machine, a positive and negative voltage difference of 20 kV, an outer core flow rate of 1.0 mL / h, an inner core flow rate of 0.2 mL / h, a receiving distance of 15 cm, and use aluminum foil to collect the nanofiber membrane. (3) The collected nanofiber membrane is placed in an ark and loaded into a closed tubular high-temperature sintering furnace for sintering. In the first stage, the temperature is raised from room temperature to 270 ° C and kept for 1 hour. In the second stage, the temperature is raised from 270 ° C to 400 ° C and kept for 1 hour. In the third stage, the temperature is raised from 400 ° C to 1000 ° C, kept for 1 hour, and cooled naturally. Hydrogen is continuously introduced into the tubular high-temperature sintering furnace. (4) The sintered sample is ground into powder in a mortar to obtain catalyst sample 1. Weigh 0.5 g of catalyst sample 1, add 3.77 mL of perfluorosulfonic acid resin solution (Nafion content is 5%), add water and isopropanol to form an ink-like slurry, and disperse at a high speed of 30 m / s for 30 min under the condition that the slurry temperature is lower than 20°C to make it a uniformly dispersed catalyst slurry. The water / isopropanol volume ratio in the above slurry is 1 / 5, and the solid content is 2.7%. (5) The catalyst slurry is evenly sprayed on a 12um thick proton exchange membrane. The spraying temperature is 90°C, the spraying area is 5×5 cm2, the total CCM loading is 0.5 mg / cm2, the loading ratio of the anode surface to the cathode surface is 1 / 4, and a 180um thick gas diffusion layer is placed on both sides of the above CCM. A single cell is prepared using a graphite single serpentine electrode.

[0036] Embodiment 2:

[0037] (1) Prepare chemicals PAN, N,N-dimethylformamide (DMF) and chloroplatinic acid. Mix 10 mL DMF, 1 g PAN and 0.4 g chloroplatinic acid powder, and mix them evenly by ultrasonic + magnetic stirring to use as the outer core precursor solution; at the same time, prepare a 25% PAN PMMA solution, and mix them evenly by ultrasonic + magnetic stirring to use as the inner core precursor solution. (2) Transfer the solutions to syringes for spinning. Use a high-voltage electrospinning machine with a positive and negative voltage difference of 20 kV, an outer core solution flow rate of 1.0 mL / h, an inner core solution flow rate of 0.4 mL / h, and a receiving distance of 15 cm. Use aluminum foil to collect the nanofiber membrane. (3) The collected nanofiber membrane is placed in an ark and loaded into a closed tubular high-temperature sintering furnace for sintering. In the first stage, the temperature is raised from room temperature to 400 ° C, and the temperature is kept for 1 hour. In the second stage, the temperature is raised from 400 ° C to 1000 ° C, and the temperature is kept for 1 hour, and then cooled naturally. Hydrogen is continuously introduced into the tubular high-temperature sintering furnace. (4) The sintered sample was ground into powder in a mortar to obtain catalyst sample 2. 0.5 g of catalyst sample 2 was weighed, 3.77 mL of perfluorosulfonic acid resin solution (Nafion content was 5%) was added, water and isopropanol were added to form an ink-like slurry, and the slurry temperature was lower than 20°C and dispersed at a high speed of 30 m / s for 30 min to make it a uniformly dispersed catalyst slurry. The volume ratio of water to isopropanol in the above slurry was 1 / 5, and the solid content was 2.7%. (5) The catalyst slurry was evenly sprayed on a 12 um thick proton exchange membrane. The spraying temperature was 90°C, the spraying area was 5×5 cm2, the CCM loading was 0.5 mg / cm2, the loading ratio of the anode surface to the cathode surface was 1 / 4, a 180 um thick gas diffusion layer was placed on both sides of the above CCM, and a single cell was prepared using a graphite single serpentine electrode.

[0038] Embodiment 3:

[0039] (1) Prepare chemicals PAN, N,N-dimethylformamide (DMF) and chloroplatinic acid. Mix 10 mL DMF, 1 g PAN and 0.6 g chloroplatinic acid powder, and mix them evenly by ultrasonic + magnetic stirring to use as the outer core precursor solution; at the same time, prepare a 25% PAN PMMA solution, and mix them evenly by ultrasonic + magnetic stirring to use as the inner core precursor solution. (2) Transfer the solutions to syringes for spinning. Use a high-voltage electrospinning machine, a positive and negative voltage difference of 20 kV, an outer core solution flow rate of 1.0 mL / h, an inner core solution flow rate of 0.6 mL / h, a receiving distance of 15 cm, and use aluminum foil to collect the nanofiber membrane. (3) The collected nanofiber membrane is placed in an ark and placed in a closed tubular high-temperature sintering furnace for sintering, rising from room temperature to 1000 ° C, keeping the temperature for 1 hour, and cooling naturally. Hydrogen is continuously introduced into the tubular high-temperature sintering furnace. (4) The sintered sample was ground into powder in a mortar to obtain catalyst sample 3. 0.5 g of catalyst sample 3 was weighed, 3.77 mL of perfluorosulfonic acid resin solution (Nafion content was 5%) was added, water and isopropanol were added to form an ink-like slurry, and the slurry temperature was lower than 20°C and dispersed at a high speed of 30 m / s for 30 min to make it a uniformly dispersed catalyst slurry. The water / isopropanol volume ratio in the above slurry was 1 / 5, and the solid content was 2.7%. (5) The catalyst slurry was evenly sprayed on a 12 um thick proton exchange membrane. The spraying temperature was 90°C, the spraying area was 5×5 cm2, the CCM loading was 0.5 mg / cm2, the loading ratio between the anode surface and the cathode surface was 1 / 4, a 180 um thick gas diffusion layer was placed on both sides of the above CCM, and a single cell was prepared using a graphite single serpentine electrode.

[0040] Embodiment 4:

[0041] A highly durable and highly active core-shell structured Pt, C catalyst is prepared by any one of Examples 1-3.

[0042] Comparative Example 1:

[0043] (1) Weigh 0.5g of commercial carbon nanotube-loaded platinum catalyst (Pt / CNT) (mass percentage of platinum is 20%), add 3.77mL of perfluorosulfonic acid resin solution (Nafion content is 5%), add water and isopropanol to form an ink-like slurry, and disperse it at a high speed of 30m / s for 30min under the condition that the slurry temperature is lower than 20°C to make it a uniformly dispersed catalyst slurry. The volume ratio of water / isopropanol in the above slurry is 1 / 5, and the solid content is 2.7%. (5) The catalyst slurry is evenly sprayed on a 12um thick proton exchange membrane, the spraying temperature is 90°C, the spraying area is 5×5cm2, the CCM loading is 0.5mg / cm2, the loading ratio of the anode surface to the cathode surface is 1 / 4, a 180um thick gas diffusion layer is placed on both sides of the above CCM, and a single cell is prepared using a graphite single serpentine electrode.

[0044] Test method:

[0045] The electrical properties of the membrane electrode were tested using a fuel cell test system. The reactants used in the system were compressed air and high-purity hydrogen. The system was equipped with an external humidification system, and different gas humidification effects were obtained by controlling the humidifier temperature. Before the test, the MEA was activated first, the purpose of which was to make the proton exchange membrane and the Nafion resin contained in the catalyst layer contain sufficient water to ensure sufficient conductivity. After the working conditions were stable, the battery was controlled to have different discharge currents or voltages. After the test, the experimental data were exported. The single cell of the fuel cell consists of a membrane electrode, a plate, a sealing gasket and an end plate. The plate uses an airtight hard graphite plate with a size of 50×50×3mm, and the inner side is designed as a parallel single serpentine; the sealing gasket uses an ordinary plastic gasket; and a stainless steel plate is used as the end plate. The components are tightly assembled to reduce the internal resistance of the battery. The effective area of ​​the membrane electrode in the homemade single cell is 25cm2. After the membrane electrode with an effective area of ​​25cm2 was installed in the single experimental cell, the single cell performance test was carried out on the test bench. Polarization test: In the electrochemical performance test conditions of the membrane electrode, the humidity of hydrogen and oxygen is 50% RH, the hydrogen pressure and oxygen pressure are adjusted to 0.28MPa and 0.30MPa respectively, the single cell is connected to an external constant current and constant voltage power supply, the battery temperature rises to 80℃, and the voltage-current curve of the battery is measured. Durability test: The catalyst durability cycle test is carried out between the voltage value of 0.5-0.95V, nitrogen and hydrogen are introduced into the anode and cathode, the humidity is set to 50% RH, the test is carried out at a temperature of 80℃, and the anode and cathode back pressure is adjusted to 0.5MPa; the carbon carrier durability cycle test is carried out between the voltage value of 0.8-1.6V, nitrogen and hydrogen are introduced into the anode and cathode, the humidity is set to 50% RH, the test is carried out at a temperature of 80℃, and the anode and cathode back pressure is adjusted to 0.5MPa.

[0046] The above examples and comparative examples analyze the microscopic morphology, electrochemical properties, and durability data of the Pt / C catalyst. From the comparison of the polarization curves of the examples and comparative examples, it can be seen that the initial performance of the core-shell structure catalyst is higher than that of the commercial catalyst, because the carrier of the carbon nanofiber structure has a better activation polarization; when the current density increases, the example has a higher battery voltage, because the core-shell structure provides more active sites, which increases the active area and the battery performance, but the voltage value increase of Example 1 is higher than that of Examples 2 and 3, because Example 1 is sintered at high temperature in three stages, the chemical reaction is sufficient, and the performance is improved; from the comparison of the TEM images of the examples and comparative examples, it can be seen that the number of deposited platinum particles on the core-shell structure catalyst is more and more uniform, because the chloroplatinic acid in the spinning solution precursor is evenly mixed, and the chloroplatinic acid on each fiber in the hydrogen atmosphere has the same probability of being reduced, so the reduced platinum particles are more uniform.

[0047]

[0048] From the comparison in the above table, it can be seen that after durability, the particle size of the core-shell structure increases less and the carbon content loss is less. This is because the mosaic structure of the platinum particles effectively reduces the migration and agglomeration of the platinum particles, and the carbon carrier treated at high temperature is more resistant to carbon oxidation, reducing the carbon corrosion effect.

[0049] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A method for preparing a highly durable and highly active core-shell structure Pt, C catalyst, characterized in that: The following steps are involved: S1: Prepare chemical reagents PAN, N,N-dimethylformamide and chloroplatinic acid, mix N,N-dimethylformamide, PAN and chloroplatinic acid powder, and mix them evenly by ultrasonic + magnetic stirring to use as outer core precursor solution; at the same time, prepare PMMA solution, and mix them evenly by ultrasonic + magnetic stirring to use as inner core precursor solution; S2: The solutions were transferred into syringes and spun using a high-voltage electrospinning machine, and the nanofiber membranes were collected using aluminum foil; S3: The collected nanofiber membranes are placed in an ark and loaded into a closed tubular high-temperature sintering furnace for sintering, and hydrogen is continuously introduced during the sintering process; S4: Grinding the sintered sample into powder, adding the ground sample into a perfluorosulfonic acid resin solution, water and isopropanol to form an ink-like slurry, and then dispersing it at high speed to make it a uniformly dispersed catalyst slurry; S5: The catalyst slurry is sprayed on both sides of the proton exchange membrane, and then the gas diffusion layer is placed on both sides, and a single cell is prepared using a graphite single serpentine electrode plate.

2. The method for preparing a highly durable and highly active core-shell structure Pt, C catalyst according to claim 1, characterized in that: The PAN content of the PMMA solution in step S1 is 25%.

3. The method for preparing a highly durable and highly active core-shell structure Pt, C catalyst according to claim 1, characterized in that: In the step S2, the voltage difference between the positive and negative electrodes of the high-voltage electrospinning machine is 20 kV, the outer core flow rate is 1.0 mL / h, the inner core solution flow rate is 0.2-0.6 mL / h, and the receiving distance is 15 cm.

4. The method for preparing a highly durable and highly active core-shell structure Pt, C catalyst according to claim 1, characterized in that: In the step S3, the sintering is carried out in three stages, which are: S31: In the first stage, the temperature is raised from room temperature to 270 degrees Celsius and kept for 1 hour; S32: The second stage is from 270 degrees Celsius to 400 degrees Celsius, and the temperature is kept for 1 hour; S33: The third stage is to increase the temperature from 400°C to 1000°C, keep it at that temperature for 1 hour and then cool it naturally.

5. The method for preparing a highly durable and highly active core-shell structure Pt, C catalyst according to claim 1, characterized in that: In the step S3, hydrogen is introduced from the air inlet at the top of the sintering furnace, and an exhaust port is arranged at the bottom of the sintering furnace, and opening valves are installed on the outsides of the air inlet and the exhaust port, and the opening degree of the opening valve at the air inlet is larger than that of the opening valve at the exhaust port.

6. The method for preparing a highly durable and highly active core-shell structure Pt, C catalyst according to claim 1, characterized in that: In the step S4, the Nafion content of the perfluorosulfonic acid resin solution is 5%; the high-speed dispersion speed is 30 m / s, the dispersion time is 30 min, and the temperature of the slurry during dispersion is lower than 20 degrees Celsius.

7. The method for preparing a highly durable and highly active core-shell structure Pt, C catalyst according to claim 1, characterized in that: In the step S4, the solid content of the slurry is 2.7%, and the volume ratio of water to isopropanol is 1 / 5.

8. The method for preparing a highly durable and highly active core-shell structure Pt, C catalyst according to claim 1, characterized in that: In the step S5, the thickness of the proton exchange membrane is 12 μm.

9. The method for preparing a highly durable and highly active core-shell structure Pt, C catalyst according to claim 1, characterized in that: In step S5, the spraying temperature is 90 degrees Celsius and the spraying area is 5*5cm 2 In step S5, the total CCM loading is 0.5 mg / cm 2 The loading ratio between the anode surface and the cathode surface is 1 / 4, and the thickness of the gas diffusion layer is 180 μm.

10. A highly durable and highly active core-shell structure Pt, C catalyst, prepared by the method for preparing a highly durable and highly active core-shell structure Pt, C catalyst according to any one of claims 1 to 9, characterized in that: Includes PAN, N,N-dimethylformamide, chloroplatinic acid, perfluorosulfonic acid resin solution, water and isopropyl alcohol.