Fuel cell modified phenolic resin dipping slurry, preparation method thereof and bipolar plate

Through the impregnation and hot pressing process of boric acid-modified phenolic resin and hydrophobic resin combined with nano-level conductive fillers, the embrittlement problem of fuel cell bipolar plates in high temperature environments is solved, which significantly improves the conductivity and mechanical strength and improves the overall performance. Performance and stability.

CN118919752APending Publication Date: 2024-11-08QINGDAO DUKE NEW MATERIAL CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410948229.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing fuel cell bipolar plates are brittled in high temperature environments, making it difficult to meet the requirements of high conductivity and excellent mechanical properties, and the heat resistance and cost problems of the modifier have not been completely solved.

Method used

Boric acid modified phenolic resin is used, and hydrophobic resin and nano-scale conductive filler are added to prepare bipolar plates through impregnation and hot pressing processes to improve conductivity, mechanical strength and thermal stability and form a tight structure.

Benefits of technology

It significantly improves conductivity, heat resistance and mechanical strength, improves the overall performance of fuel cells, including open circuit voltage and power density, and has good stability and reusability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004946331620000131
    Figure BDA0004946331620000131
Patent Text Reader

Abstract

The invention discloses fuel cell modified phenolic resin dipping slurry, a preparation method thereof and a bipolar plate, and relates to the technical field of fuel cells. On the basis of phenolic resin preparation, a modifier is added, carbon fibers are used as a conductive filler, mixing and stirring are performed to prepare impregnation slurry, and the method comprises the following steps: (1) preparing modified phenolic resin; (2) mixing and dissolving the modified phenolic resin and hydrophobic resin; and (3) mixing with a nanoscale conductive filler to form dipping slurry. The conductivity, the heat resistance and the mechanical strength can be remarkably improved, so that the overall performance of the fuel cell is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of fuel cells, and in particular to a fuel cell modified phenolic resin impregnation slurry, a preparation method thereof, and a bipolar plate. Background Art

[0002] In fuel cell technology, bipolar plates are key components that are responsible for transmitting reaction gases and providing electron transfer channels. Bipolar plates are divided into a microporous layer and a substrate layer. The substrate layer needs to have a uniform void structure, low resistivity, sufficient mechanical strength, suitable hydrophilicity / hydrophobicity, good thermal conductivity, and excellent chemical stability. Phenolic resin, as a cheap thermosetting plastic with good mechanical properties, can improve the comprehensive performance of bipolar plates after impregnation. However, pure phenolic resin is easily brittle at high temperatures, which limits its application in high temperature environments and is difficult to meet the requirements of high conductivity and excellent mechanical properties of bipolar plates. Therefore, how to improve the performance of phenolic resin to meet the requirements of fuel cell bipolar plates has become the focus of current research in the field of fuel cells.

[0003] Chinese patent CN106567283B modifies phenolic resin with polyvinyl butyral (PVB), which improves certain flexibility and strength, but the production cost of PVB itself is relatively high, the thermal stability is reduced, the residual carbon rate is not high, and the porosity is significantly reduced.

[0004] Chinese patent CN112430297A uses propylene oxide-inorganic acid as a modifier. Although it improves flexibility to a certain extent and improves strength and conductivity, it obviously lacks heat resistance, increases brittleness, and has poor impact resistance.

[0005] Chinese patent CN201910757768.6 describes the use of a variety of raw materials (nanocellulose, carbon fiber) to prepare bipolar plates, which are then impregnated with phenolic resin modified with carbon nanotubes and boric acid-cardanol. The bipolar plates prepared by this process have low resistivity and high tensile strength, but reduced porosity.

[0006] Therefore, it is of great significance to develop a bipolar plate with high conductivity, high strength, high porosity, corrosion resistance and smooth surface.

[0007] Although boric acid has been used as a modifier to modify phenolic resin, it does not focus on the key performance of bipolar plates in fuel cells, and there is still a problem that mechanical properties and conductive properties cannot be taken into account at the same time. Summary of the invention

[0008] In view of the problems existing in the prior art, the present invention discloses a fuel cell modified phenolic resin impregnation slurry and a preparation method thereof and a bipolar plate. On the basis of boric acid modified phenolic resin, thermal stability and mechanical strength are improved, hydrophobic resin is mixed to improve drainage, conductive filler is added to improve conductivity, nanocellulose is added to improve strength, and a compact structure is formed. It has excellent conductivity and strength, and the formula is flexible and the operation is simple. Therefore, the present invention has key application value.

[0009] The present invention relates to the following technical solutions:

[0010] A method for preparing a fuel cell modified phenolic resin impregnation slurry comprises the following steps:

[0011] (1) mixing m-diphenol and formaldehyde for reaction at a certain temperature, adding a catalyst, and mechanically stirring to obtain a phenolic resin;

[0012] (2) reacting boric acid and phenolic resin under heating and stirring;

[0013] (3) removing water by vacuum distillation to obtain a thermosetting boron-modified phenolic resin;

[0014] (4) dissolving the obtained thermosetting boron-modified phenolic resin and the hydrophobic resin in an organic solution to obtain a mixed solution A;

[0015] (5) adding the nano-scale conductive filler into the mixed solution A and mechanically stirring to obtain an impregnation slurry B;

[0016] (6) impregnating the bipolar plate precursor once;

[0017] (7) hot pressing after the primary impregnation to obtain the bipolar plate base paper, and drying;

[0018] (8) The dried bipolar plate base paper is impregnated for a second time and subjected to carbonization and graphitization treatment under a protective gas to obtain a bipolar plate sample.

[0019] Furthermore, the content of m-diphenol is 56-68 parts, and the content of formaldehyde is 24-30 parts.

[0020] Furthermore, the catalyst is an alkaline catalyst, which is sodium hydroxide, and the number of parts is 3-5 parts.

[0021] Furthermore, the reaction temperature is 65-70° C., the addition reaction time is 1-2 h, and after obtaining the reaction product, the temperature is continued to rise to 85-100° C., and the polycondensation reaction time is 0.5-1 h.

[0022] Furthermore, the mechanical stirring speed is 220-250 r / min, and the stirring reaction time is 2-3 h.

[0023] Furthermore, the boric acid is 5-11 parts.

[0024] Furthermore, the heating temperature is 110-120° C., the stirring speed is 260-310 r / min, and the reaction time is 50-60 min.

[0025] Furthermore, the reduced pressure distillation time is 40 to 50 minutes.

[0026] Furthermore, the hydrophobic resin is one of acrylic resin, epoxy resin, polytetrafluoroethylene and polydimethylsiloxane.

[0027] Furthermore, the organic solvent is one of methanol, anhydrous ethanol or acetone.

[0028] Furthermore, the nano-scale conductive filler is one of carbon fiber, carbon black, carbon nanotube, and graphene, the concentration of the nano-scale conductive filler solution is 3-5%, and the solvent is one of the above-mentioned ones.

[0029] Furthermore, the mechanical stirring speed is 700-900 r / min, the stirring time is 20-30 min, and the concentration of the obtained mixed impregnation slurry B is 60-70%.

[0030] Furthermore, the immersion time is 10 to 20 minutes, the hot pressing temperature is 180 to 200° C., the hot pressing time is 30 to 40 minutes, and the hot pressing pressure is 3 to 5 MPa.

[0031] Furthermore, the impregnation amount is 2.5 to 3 in terms of the mass ratio of the bipolar plate to the mixed solution.

[0032] Furthermore, the protective gas may be one of nitrogen, argon and helium.

[0033] Furthermore, the carbonization temperature is 900-1100° C., the carbonization heating rate is 10° C. / min, the carbonization time is 1.5-2.5 h, and the nitrogen flow rate is 5-10 ml / min.

[0034] Furthermore, the graphitization temperature of the bipolar plate is 2400° C. to 2700° C., the graphitization heating rate is 5 to 10° C. / min, and the graphitization treatment time is 1 to 2 hours.

[0035] The beneficial effects of the present invention are:

[0036] 1. The fuel cell impregnation resin of the present invention can significantly improve the electrical conductivity, heat resistance and mechanical strength. Compared with the case where the impregnation slurry of the present invention is not used, the electrical conductivity of the impregnation slurry of the present invention is increased by about 30%, the heat resistance is increased by about 20%, and the mechanical strength is increased by about 15%;

[0037] 2. The overall performance of the fuel cell has been significantly improved, including but not limited to open circuit voltage, power density and other indicators have been significantly improved;

[0038] 3. The impregnation solution of the present invention also has good stability and reusability, and can meet the needs of large-scale production and application. DETAILED DESCRIPTION

[0039] In order to make the purpose, technical solutions and advantages of the embodiments of the present application clearer, this section will elaborate on the technical solutions in the embodiments. It should be emphasized that the described content is only a part of the many embodiments of the present application, not all. Based on the embodiments disclosed in the present application, all other embodiments that can be derived by those skilled in the art without any creative work are also included in the protection scope of the present application.

[0040] This embodiment provides a method for preparing a fuel cell modified phenolic resin impregnation slurry, comprising the following steps:

[0041] (1) mixing the dissolved phenol with excess formaldehyde at a certain temperature, adding a catalyst, and mechanically stirring to obtain a phenolic resin;

[0042] (2) reacting boric acid and phenolic resin under heating and stirring;

[0043] (3) removing water by vacuum distillation to obtain a thermosetting boron-modified phenolic resin;

[0044] (4) and dissolved in an organic solution with a hydrophobic resin to obtain a mixed solution A;

[0045] (5) adding the nano-scale conductive filler into the mixed solution A and mechanically stirring to obtain an impregnation slurry B;

[0046] (6) impregnating the bipolar plate precursor once;

[0047] (7) hot pressing after the primary impregnation to obtain the bipolar plate base paper, and drying;

[0048] (8) The dried bipolar plate base paper is impregnated for a second time and subjected to carbonization and graphitization treatment under a protective gas to obtain a bipolar plate sample.

[0049] In another specific embodiment of the present invention, in step (1), the raw materials involved in the preparation are calculated by mass, the m-diphenol is 56-68 parts, the formaldehyde is 24-30 parts, the catalyst is an alkaline catalyst, which is sodium hydroxide, and the mass is 3-5 parts. The reaction temperature is 65-70°C, the addition reaction time is 1-2h, and after obtaining the reaction product, the temperature is continued to rise to 85°C-100°C, the condensation reaction time is 0.5-1h, the mechanical stirring speed is 220-250r / min, and the stirring reaction time is 2-3h.

[0050] In another specific embodiment of the present invention, in step (2), the amount of boric acid involved is 5-11 parts, the heating temperature is 110-120° C., the stirring speed is 260-310 r / min, and the reaction time is 50-60 min.

[0051] In another specific embodiment of the present invention, the reduced pressure distillation time in step (3) is 40 to 50 minutes.

[0052] In another specific embodiment of the present invention, in step (4), the hydrophobic resin is one of acrylic resin, epoxy resin, polytetrafluoroethylene, and polydimethylsiloxane, and the organic solvent is one of methanol, anhydrous ethanol, or acetone.

[0053] According to the preparation method of claim 1, in step (5), the nano-scale conductive filler is one of carbon fiber, carbon black, carbon nanotube, and graphene. The concentration of the nano-scale conductive filler solution is 3-5%, the solvent is one of the above, the mechanical stirring speed is 700-900 r / min, and the stirring time is 20-30 min. The concentration of the obtained mixed impregnation slurry B is 60-70%

[0054] In another specific embodiment of the present invention, in step (6), the immersion time is 10 to 20 minutes, the hot pressing temperature is 180 to 200° C., the hot pressing time is 30 to 40 minutes, the hot pressing pressure is 3 to 5 MPa, and the immersion amount is 2.5 to 3 in terms of the mass ratio of the bipolar plate to the mixed solution.

[0055] In another specific embodiment of the present invention, the drying in step (7) can be carried out in an oven, the drying temperature is controlled at 60 to 80° C., and the drying time is 15 to 25 minutes.

[0056] In another specific embodiment of the present invention, the protective gas involved in step (8) may be one of nitrogen, argon, and helium, the carbonization temperature is 900-1100°C, the carbonization heating rate is 10°C / min, the carbonization time is 1.5-2.5h, the nitrogen flow rate is 5-10ml / min, the graphitization temperature is 2400°C-2700°C, the graphitization heating rate is 5-10°C / min, and the graphitization time is 1-2h.

[0057] In another specific embodiment of the present invention, the impregnation slurry is obtained by the above preparation method.

[0058] In another specific embodiment of the present invention, a bipolar plate is prepared by the above-mentioned impregnation slurry.

[0059] Embodiment 1:

[0060] (1) Take 56 parts of m-diphenol and 24 parts of formaldehyde, add 2 parts of sodium hydroxide catalyst, stir at 220 r / min, add reaction at 65°C for 1 h, continue to heat to 85°C, and polycondensation reaction for 0.5 h;

[0061] (2) Take 5 parts of boric acid, heat at 110°C, rotate at 260 r / min, and react for 50 min;

[0062] (3) The vacuum distillation time is 45 min;

[0063] (4) taking a hydrophobic resin of acrylic resin and a phenolic resin in a mass ratio of 2:3, dissolving them in anhydrous ethanol to obtain a phenolic resin mixed solution A;

[0064] (5) Select carbon fiber conductive filler, the carbon fiber concentration is 3%, the mechanical stirring speed is 750r / min, the stirring time is 20r / min, and the concentration of the obtained mixed impregnation slurry B is 60%;

[0065] (6) The immersion time is 15 min, the hot pressing temperature is 200 °C, the hot pressing time is 40 min, the hot pressing pressure is 5 MPa, and the immersion volume is 1:3 in terms of the mass ratio of the bipolar plate to the mixed solution;

[0066] (7) Drying temperature is 80°C and drying time is 15 min;

[0067] (8) The protective gas was nitrogen, the carbonization temperature was 1100 °C, the heating rate was 10 °C / min, the carbonization time was 1.5 h, the nitrogen flow rate was 10 ml / min, and the graphitization time was 1 h.

[0068] Embodiment 2:

[0069] (1) 60 parts of m-diphenol, 26 parts of formaldehyde, 3 parts of sodium hydroxide catalyst, stirring speed of 240 r / min, addition reaction temperature of 70°C, addition reaction temperature of 1.5h, continue to rise to 90°C, polycondensation reaction time of 1h;

[0070] (2) Take 8 parts of boric acid, heat at 120°C, rotate at 300 r / min, and react for 55 min;

[0071] (3) The vacuum distillation time is 45 min;

[0072] (4) taking a hydrophobic resin of acrylic resin and a phenolic resin in a ratio of 2:3, dissolving them in anhydrous ethanol to obtain a phenolic resin mixed solution A;

[0073] (5) Select carbon fiber conductive filler, the concentration of carbon fiber solution is 4%, the mechanical stirring speed is 800r / min, the stirring time is 25min, and the concentration of the obtained mixed impregnation slurry B is 65%;

[0074] (6) The impregnation and hot pressing process is the same;

[0075] (7) The drying process conditions are the same;

[0076] (8) The carbonization and graphitization process is the same.

[0077] Embodiment 3:

[0078] (1) 68 parts of m-diphenol, 29 parts of formaldehyde, 4 parts of sodium hydroxide catalyst, stirring speed of 240 r / min, addition reaction temperature of 80°C, addition reaction temperature of 1.5h, continue to rise to 90°C, polycondensation reaction time of 1h;

[0079] (2) Take 11 parts of boric acid, heat at 120°C, rotate at 300 r / min, and react for 55 min;

[0080] (3) The vacuum distillation time is 45 min;

[0081] (4) taking a hydrophobic resin of acrylic resin and a phenolic resin in a ratio of 2:3, dissolving them in anhydrous ethanol to obtain a phenolic resin mixed solution A;

[0082] (5) Select carbon fiber conductive filler, the concentration of carbon fiber solution is 5%, the mechanical stirring speed is 900r / min, the stirring time is 25min, and the concentration of the obtained mixed impregnation slurry B is 70%;

[0083] (6) The impregnation and hot pressing process is the same;

[0084] (7) The drying process conditions are the same;

[0085] (8) The carbonization and graphitization process is the same.

[0086] Embodiment 4:

[0087] (1) Take 56 parts of m-diphenol and 24 parts of formaldehyde, add 3 parts of sodium hydroxide catalyst, stir at 220 r / min, add reaction temperature at 65°C, add reaction temperature for 1 h, continue to heat to 85°C, polycondensation reaction time for 0.5 h;

[0088] (2) Take 8 parts of boric acid, heat at 110°C, rotate at 260 r / min, and react for 50 min;

[0089] (3) The vacuum distillation time is 45 min;

[0090] (4) taking a hydrophobic resin of acrylic resin and a phenolic resin in a mass ratio of 2:3, dissolving them in anhydrous ethanol to obtain a phenolic resin mixed solution A;

[0091] (5) Select carbon fiber conductive filler, the carbon fiber concentration is 3%, the mechanical stirring speed is 750r / min, the stirring time is 20r / min, and the concentration of the obtained mixed impregnation slurry B is 60%;

[0092] (6) The impregnation and hot pressing process is the same;

[0093] (7) The drying process conditions are the same;

[0094] (8) The carbonization and graphitization process is the same.

[0095] Embodiment 5:

[0096] (1) 60 parts of m-diphenol, 26 parts of formaldehyde, 4 parts of sodium hydroxide catalyst, stirring speed of 240 r / min, addition reaction temperature of 70°C, addition reaction temperature of 1.5h, continue to rise to 90°C, polycondensation reaction time of 1h;

[0097] (2) Boric acid is taken in an amount of 7 parts, the heating temperature is 120°C, the rotation speed is 300 r / min, and the reaction time is 55 min;

[0098] (3) The vacuum distillation time is 45 min;

[0099] (4) taking a hydrophobic resin of acrylic resin and a phenolic resin in a ratio of 2:3, dissolving them in anhydrous ethanol to obtain a phenolic resin mixed solution A;

[0100] (5) Select carbon fiber conductive filler, the concentration of carbon fiber solution is 4%, the mechanical stirring speed is 800r / min, the stirring time is 25min, and the concentration of the obtained mixed impregnation slurry B is 65%;

[0101] (6) The impregnation and hot pressing process is the same;

[0102] (7) The drying process conditions are the same;

[0103] (8) The carbonization and graphitization process is the same.

[0104] Embodiment 6:

[0105] (1) 68 parts of m-diphenol, 29 parts of formaldehyde, 3 parts of sodium hydroxide catalyst, stirring speed of 240 r / min, addition reaction temperature of 80°C, addition reaction temperature of 1.5h, continue to rise to 90°C, polycondensation reaction time of 1h;

[0106] (2) Boric acid is taken in an amount of 7 parts, the heating temperature is 120°C, the rotation speed is 300 r / min, and the reaction time is 55 min;

[0107] (3) The vacuum distillation time is 45 min;

[0108] (4) taking a hydrophobic resin of acrylic resin and a phenolic resin in a ratio of 2:3, dissolving them in anhydrous ethanol to obtain a phenolic resin mixed solution A;

[0109] (5) Select carbon black conductive filler, the concentration of carbon black solution is 5%, the mechanical stirring speed is 900r / min, the stirring time is 25min, and the concentration of the obtained mixed impregnation slurry B is 70%;

[0110] (6) The impregnation and hot pressing process is the same;

[0111] (7) The drying process conditions are the same;

[0112] (8) The carbonization and graphitization process is the same.

[0113] Embodiment 7:

[0114] (1) 60 parts of m-diphenol, 26 parts of formaldehyde, 3 parts of sodium hydroxide catalyst, stirring speed of 240 r / min, addition reaction temperature of 70°C, addition reaction temperature of 1.5h, continue to rise to 90°C, polycondensation reaction time of 1h;

[0115] (2) Take 8 parts of boric acid, heat at 120°C, rotate at 300 r / min, and react for 55 min;

[0116] (3) The vacuum distillation time is 45 min;

[0117] (4) taking a hydrophobic resin of acrylic resin and a phenolic resin in a ratio of 2:3, dissolving them in anhydrous ethanol to obtain a phenolic resin mixed solution A;

[0118] (5) Select carbon black conductive filler, the concentration of carbon black solution is 4%, the mechanical stirring speed is 800r / min, the stirring time is 25min, and the concentration of the obtained mixed impregnation slurry B is 65%;

[0119] (6) The impregnation and hot pressing process is the same;

[0120] (7) The drying process conditions are the same;

[0121] (8) The carbonization and graphitization process is the same.

[0122] Embodiment 8:

[0123] (1) Take 56 parts of m-diphenol and 24 parts of formaldehyde, add 2 parts of sodium hydroxide catalyst, stir at 220 r / min, add reaction at 65°C for 1 h, continue to heat to 85°C, and polycondensation reaction for 0.5 h;

[0124] (2) Take 8 parts of propylene oxide-boric acid modifier, the heating temperature is 110°C, the speed is 260r / min, and the reaction time is 2h;

[0125] (3) The vacuum distillation time is 45 min;

[0126] (4) taking a hydrophobic resin of acrylic resin and a phenolic resin in a mass ratio of 2:3, dissolving them in anhydrous ethanol to obtain a phenolic resin mixed solution A;

[0127] (5) Select carbon fiber conductive filler, the carbon fiber concentration is 3%, the mechanical stirring speed is 750r / min, the stirring time is 20r / min, and the concentration of the obtained mixed impregnation slurry B is 60%;

[0128] (6) The impregnation and hot pressing process is the same;

[0129] (7) The drying process conditions are the same;

[0130] (8) The carbonization and graphitization process is the same.

[0131] Embodiment 9:

[0132] (1) Take 56 parts of m-diphenol and 24 parts of formaldehyde, add 4 parts of sodium hydroxide catalyst, stir at 220 r / min, add reaction temperature at 65°C, add reaction temperature for 1 h, continue to heat to 85°C, polycondensation reaction time for 0.5 h;

[0133] (2) 8 parts of polyvinyl butyral (PVB) were taken, the heating temperature was 110°C, the rotation speed was 260 r / min, and the reaction time was 2 h;

[0134] (3) The vacuum distillation time is 45 min;

[0135] (4) taking a hydrophobic resin of acrylic resin and a phenolic resin in a mass ratio of 2:3, dissolving them in anhydrous ethanol to obtain a phenolic resin mixed solution A;

[0136] (5) Carbon fiber conductive filler was selected, the carbon fiber concentration was 3%, the mechanical stirring speed was 750 r / min, the stirring time was 20 r / min, and the concentration of the obtained mixed impregnation slurry B was 60%.

[0137] (6) The impregnation and hot pressing process is the same;

[0138] (7) The drying process conditions are the same;

[0139] (8) The carbonization and graphitization process is the same.

[0140] Comparative Example 1:

[0141] The phenolic resins in Comparative Example 1 and Example 1 are prepared differently, in that no modifier is added to Comparative Example 1.

[0142] (1) 60 parts of m-diphenol, 26 parts of formaldehyde, 3 parts of sodium hydroxide catalyst, stirring speed of 240 r / min, addition reaction temperature of 70°C, addition reaction temperature of 1.5h, continue to raise the temperature to 90°C, polycondensation reaction time of 1.5h;

[0143] (2) The vacuum distillation time is 45 min;

[0144] (3) taking a hydrophobic resin such as an acrylic resin and a phenolic resin in a ratio of 2:3, dissolving them in anhydrous ethanol to obtain a phenolic resin mixed solution A;

[0145] (4) Select carbon fiber conductive filler, the concentration of carbon fiber solution is 4%, the mechanical stirring speed is 800r / min, the stirring time is 25min, and the concentration of the obtained mixed impregnation slurry B is 65%;

[0146] (5) The impregnation and hot pressing process is the same;

[0147] (6) The drying process conditions are the same;

[0148] (7) The carbonization and graphitization process is the same.

[0149] Comparative Example 2:

[0150] The modified phenolic resin in Comparative Example 2 is different from that in Example 1 in that no conductive filler is added.

[0151] (1) 60 parts of m-diphenol, 26 parts of formaldehyde, 3 parts of sodium hydroxide catalyst, stirring speed of 240 r / min, addition reaction temperature of 70°C, addition reaction temperature of 1.5h, continue to rise to 90°C, polycondensation reaction time of 1h;

[0152] (2) Take 8 parts of boric acid, heat at 120°C, rotate at 300 r / min, and react for 55 min;

[0153] (3) The vacuum distillation time is 45 min;

[0154] (4) taking a hydrophobic resin of acrylic resin and a phenolic resin in a ratio of 2:3, dissolving them in anhydrous ethanol to obtain a phenolic resin mixed solution A;

[0155] (5) The mechanical stirring speed is 800 r / min, the stirring time is 25 min, and the concentration of the obtained mixed impregnation slurry B is 65%;

[0156] (6) The impregnation and hot pressing process is the same;

[0157] (7) The drying process conditions are the same;

[0158] (8) The carbonization and graphitization process is the same.

[0159] The bipolar plate samples of Examples 1-9 were obtained through the above operations, and performance characterization tests were performed on the samples.

[0160] Test method:

[0161] Resistivity: The resistivity of the bipolar plate is tested using a four-probe tester using a four-probe measurement method.

[0162] Tensile strength: The tensile properties of carbon paper were tested using a tensile testing machine.

[0163] Bending strength: The three-point bending method was used with a universal material testing machine to test the bending strength of the bipolar plate.

[0164] Porosity: The porosity of the bipolar plates was measured using a Gold Spectroscopy porosimeter F-Sorb 3400.

[0165] Air permeability: The air permeability of the bipolar plate was tested using a Gurley air permeability meter.

[0166] Contact angle: The Young-Laplace equation was used for fitting, and the bipolar plate contact angle was tested using the SINDIN-static water contact angle meter.

[0167] Carbon residue rate: Determined according to GB / T17144 standard, using micro-method automatic carbon residue tester to test carbon residue rate.

[0168] The fuel cell bipolar plates prepared by using the embodiments 1-9 and comparative examples 1-2 of the present invention were tested, and the test results are shown in Table 1:

[0169]

[0170] Table 1

[0171] Effect description:

[0172] From Table 1, it can be seen that the fuel cell impregnation resin of the present invention can significantly improve the electrical conductivity, heat resistance and mechanical strength. Specifically, compared with the case where the impregnation slurry of the present invention is not used, the electrical conductivity of the impregnation slurry of the present invention is improved by about 30%, the heat resistance is improved by about 20%, and the mechanical strength is improved by about 15%. The improvement of these properties has significantly improved the overall performance of the fuel cell, including but not limited to the open circuit voltage, power density and other indicators have been significantly improved. In addition, the impregnation solution of the present invention also has good stability and reusability, and can meet the needs of large-scale production and application.

[0173] In summary, the method for preparing a fuel cell modified phenolic resin impregnation slurry of the present invention not only solves the problem of insufficient performance in the prior art, but also provides new technical means and application prospects for the further development of fuel cells.

[0174] The specific settings are based on actual process requirements and are not specifically limited in this application.

[0175] The relational terms such as "first" and "second" used in this application are only used to distinguish different entities or operations, and do not represent that there must be an actual association or a specific order between them. In addition, the words such as "including", "comprising" and their variants express an inclusive concept, which means that the described methods, devices, etc. are not limited to the components that have been clearly listed, and they may also include other components that have not been clearly pointed out, as well as those inherent elements that are closely related to and indispensable to the method or device itself. This inclusiveness is obvious without setting additional restrictions. When a certain content is described as "including one...", it does not mean that other identical contents may be excluded in the content. The above content is only a specific embodiment of this application, which is intended to help professionals understand or implement the content described in the present invention. Without violating the core ideas and boundaries of this application, the basic principles disclosed by it can be fully applied to other various implementation methods. Therefore, the scope of protection of the present invention is by no means limited to the specific examples shown in this article. Therefore, this application should not be limited to the embodiments described herein, but covers the widest range compatible with the principles and new features applied herein.

Claims

1. A method for preparing a mixed impregnation slurry of a fuel cell modified phenolic resin, comprising the following steps: (1) mixing dissolved meta-diphenol and formaldehyde for reaction at a certain temperature, adding a catalyst, and mechanically stirring to obtain a phenolic resin; (2) reacting boric acid and phenolic resin under heating and stirring; (3) removing water by vacuum distillation to obtain a thermosetting boron-modified phenolic resin; (4) dissolving the obtained thermosetting boron-modified phenolic resin and the hydrophobic resin in an organic solution to obtain a mixed solution A; (5) adding the nano-scale conductive filler into the mixed solution A and mechanically stirring to obtain an impregnation slurry B; (6) impregnating the bipolar plate precursor once; (7) After the first impregnation, hot pressing is performed to obtain a bipolar plate base paper, and drying; (8) The dried bipolar plate base paper is impregnated for a second time and subjected to carbonization and graphitization treatment under protective gas to obtain a bipolar plate sample.

2. The method for preparing a fuel cell modified phenolic resin mixed impregnation slurry according to claim 1, characterized in that: In step (1), the raw materials involved in the preparation are calculated by weight: the m-diphenol is 56-68 parts, the formaldehyde is 24-30 parts, the catalyst is an alkaline catalyst, which is sodium hydroxide, and the weight is 3-5 parts. The reaction temperature is 65-70°C, the addition reaction time is 1-2h, and after obtaining the reaction product, the temperature is continued to rise to 85°C-100°C, the condensation reaction time is 0.5-1h, the mechanical stirring speed is 220-250r / min, and the stirring reaction time is 2-3h.

3. The method for preparing a fuel cell modified phenolic resin mixed impregnation slurry according to claim 1, characterized in that: In step (2), the amount of boric acid involved is 5-11 parts, the heating and stirring temperature is 110-120° C., the stirring speed is 260-310 r / min, the reaction time is 50-60 min, and in step (3), the reduced pressure distillation time is 40-50 min.

4. The method for preparing a fuel cell modified phenolic resin mixed impregnation slurry according to claim 1, characterized in that: In step (4), the hydrophobic resin is one of acrylic resin, epoxy resin, polytetrafluoroethylene, and polydimethylsiloxane, and the organic solvent is one of methanol, anhydrous ethanol, or acetone.

5. The method for preparing a fuel cell modified phenolic resin mixed impregnation slurry according to claim 1, characterized in that: In step (5), the nano-scale conductive filler is one of carbon fiber, carbon black, carbon nanotube, and graphene, the concentration of the nano-scale conductive filler solution is 3-5%, the solvent is one of the above-mentioned ones, the mechanical stirring speed is 700-900 r / min, the stirring time is 20-30 min, and the concentration of the obtained mixed impregnation slurry B is 60-70%.

6. The method for preparing a fuel cell modified phenolic resin mixed impregnation slurry according to claim 1, characterized in that: In step (6), the immersion time is 10 to 20 minutes, the hot pressing temperature is 180 to 200° C., the hot pressing time is 30 to 40 minutes, the hot pressing pressure is 3 to 5 MPa, and the immersion amount is 2.5 to 3 in terms of the mass ratio of the bipolar plate to the mixed solution.

7. The method for preparing a fuel cell modified phenolic resin mixed impregnation slurry according to claim 1, characterized in that: The drying process in step (7) can be carried out in an oven, with the drying temperature controlled at 60 to 80° C. and the drying time being 15 to 25 minutes.

8. The method for preparing a fuel cell modified phenolic resin mixed impregnation slurry according to claim 1, characterized in that: In step (8), the protective gas involved can be one of nitrogen, argon, and helium. The carbonization temperature is 900-1100°C, the carbonization heating rate is 10°C / min, the carbonization time is 1.5-2.5h, the nitrogen flow rate is 5-10ml / min, the graphitization treatment bipolar plate temperature is 2400°C-2700°C, the graphitization heating rate is 5-10°C / min, and the graphitization treatment time is 1-2h.

9. An impregnation slurry, characterized in that: Obtained by the preparation method described in claims 1 to 4.

10. A bipolar plate, characterized in that: Prepared from the impregnation slurry according to any one of claims 6 to 8.

Citation Information

Cited By

  • Flexible graphite bipolar plate as well as preparation method and application thereof

    CN120999031A