Zinc-air battery electrolyte containing nicotinamide solid co-solvent
By using nicotinamide as a solid cosolvent in zinc-air batteries, the problems of oxygen reduction and oxidation reaction kinetics and volatilization of electrolyte in zinc-air batteries are solved, and the electrochemical performance and cycle life of the battery are improved.
Patent Information
- Application Number
- CN202410957341.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-11-08
AI Technical Summary
Zinc-air batteries face the problems of oxygen reduction and oxidation reaction kinetics of the positive electrode of the air, parasitic reaction between the negative electrode of the zinc and the electrolyte in an alkaline environment, and shortening of the cycle life caused by the volatility of the electrolyte.
Niacinamide is used as the solid cosolvent of zinc-air battery electrolyte, and through strong non-covalent bond interactions with water and zinc ions, the solvation structure of the electrolyte is coordinated, thereby improving the electrolyte/air positive electrode interface reaction kinetics and electrolyte/ The interface stability of zinc negative electrode reduces side reactions and moisture volatility.
It significantly improves the electrochemical performance of zinc-air batteries, increases the discharge specific capacity and cycle reversibility, and extends the cycle life of the battery.
Smart Images

Figure CN118919957A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of zinc-air batteries, and in particular to a zinc-air battery electrolyte containing nicotinamide. Background Art
[0002] Rechargeable zinc-air batteries (RZABs) are promising candidates for applications in the energy storage field due to their high theoretical energy density (≈1370 Wh kg -1 , oxygen-free) and excellent rate performance have attracted people's attention. - ), designed an internal Helmholtz layer with water-poor and zinc-rich characteristics, thus realizing a zinc-air battery based on a highly reversible two-electron reaction. Although this design enables highly reversible cathode reactions in zinc-air batteries, it faces many challenges. 1) The slow ORR and OER at the air cathode limit the kinetics of zinc-air batteries; 2) The neutral electrolyte has a higher H + activity, which makes it easier to induce parasitic reactions between the zinc negative electrode and the electrolyte; 3) Since zinc-air batteries are used directly in an open atmospheric environment, the water in the electrolyte is easily volatilized, resulting in a shortened battery cycle life.
[0003] Nicotinamide is often used as an active ingredient in human skin care products. It contains an amide group, which is a typical hydrogen bond donor and has strong hydrogen bond interactions with water molecules. In addition, as a typical Lewis base, niacinamide can react with Lewis acids (such as Zn 2+ The two interactions can synergistically regulate the electrolyte solvation structure, improve the ORR / OER reaction kinetics at the electrolyte / air cathode interface and the electrolyte / zinc anode interface stability, and reduce electrolyte volatilization, thereby improving the battery's overall cycle performance and discharge capacity. Summary of the invention
[0004] The invention provides a zinc-air battery electrolyte containing nicotinamide. When applied to a zinc-air battery, the electrolyte prepared by the invention uses nicotinamide as a solid co-solvent. The unique molecular structure of nicotinamide has strong non-covalent bond interactions with water and zinc ions, which can effectively alleviate dendrite growth, reduce the occurrence of side reactions, and improve the reaction kinetics of the battery, thereby greatly improving the electrochemical performance of the zinc-air battery.
[0005] The present invention firstly provides the application of nicotinamide as a solid co-solvent for zinc-air battery electrolyte.
[0006] Another object of the present invention is to provide the use of nicotinamide in preparing zinc-air battery electrolyte.
[0007] The third object of the present invention is to provide a battery electrolyte comprising a zinc salt, a solvent and a solid co-solvent.
[0008] The battery electrolyte is composed of a solvent, a zinc salt and a solid co-solvent.
[0009] In the above-mentioned battery electrolyte, the zinc salt is at least one of ZnSO4, ZnCl2, Zn(Ac)2 and Zn(OTf)2;
[0010] The solvent is water;
[0011] The solid co-solvent is nicotinamide.
[0012] In the above-mentioned battery electrolyte, the zinc salt concentration is 0.001 to 5 mol / L; specifically, it can be 0.05 to 3 mol / L; more specifically, it can be 1 mol / L;
[0013] The concentration of the solid co-solvent is 0.001 to 5 mol / L; specifically, it can be 0.01 to 3 mol / L; more specifically, it can be 0.5 to 3 mol / L.
[0014] The present invention also provides a method for preparing the above battery electrolyte, comprising the following steps:
[0015] The zinc salt is dissolved in the solvent, and then the solid co-solvent is added, fully stirred, and allowed to stand for 3 to 4 days to obtain the battery electrolyte.
[0016] The application of the above battery electrolyte in the preparation of zinc-air batteries also falls within the protection scope of the present invention.
[0017] The present invention further provides a zinc-air battery, the electrolyte of which is the above-mentioned battery electrolyte.
[0018] The positive active electrode material of the zinc-air battery is at least one of nitrogen-doped graphene, multi-walled carbon nanotubes, Ketjen black, Super P, carbocarbon, ruthenium dioxide, cobalt tetraoxide / nickel foam and nickel / nickel oxide.
[0019] The beneficial effects of the present invention are as follows:
[0020] The preparation method of a zinc-air battery electrolyte containing nicotinamide provided by the present invention is simple and easy. Thanks to the unique properties of the nicotinamide solid co-solvent, the growth of zinc dendrites and the occurrence of hydrogen evolution side reactions can be effectively alleviated, the electrolyte components can be protected, and the electrochemical performance of the zinc-air battery can be greatly improved, such as increasing the discharge specific capacity and improving the cycle reversibility of the battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 This is a schematic diagram of the molecular structure of nicotinamide in Example 1 of the present invention;
[0022] Figure 2 This is the first week full discharge performance diagram in Comparative Example 1;
[0023] Figure 3 This is the first cycle full discharge performance diagram in Example 1;
[0024] Figure 4 Schematic diagram of the cycle performance of the zinc-air battery of Comparative Example 1;
[0025] Figure 5 Schematic diagram of the cycle performance of the zinc-air battery in Example 1. DETAILED DESCRIPTION
[0026] The present invention is further described in detail below in conjunction with specific embodiments. The given examples are only for illustrating the present invention, but not for limiting the scope of the present invention.
[0027] The experimental methods in the following examples are all conventional methods unless otherwise specified.
[0028] Unless otherwise specified, the materials and reagents used in the following examples can be obtained from commercial sources.
[0029] In the following embodiments:
[0030] (1) Full discharge performance test: The instrument model used is: Land, Wuhan, test parameters: current density 0.4 mA cm -2 .
[0031] (2) Cyclic performance test: The instrument model used is: Land, Wuhan, test parameters: current density 0.4 mA cm -2 .
[0032] (3) Assembly of battery mold:
[0033] The assembly mold is Changsha Spring Zinc-Air Test Device (OMS-G1), and the assembly order is zinc foil, electrolyte, and positive electrode.
[0034] Preparation of the positive electrode: 0.9312 g of cobalt nitrate hexahydrate, 0.2368 g of ammonium fluoride, and 0.9616 g of urea were dissolved in 80 mL of water, and the nickel foam was placed in a hydrothermal kettle and added with the above solution, and hydrothermal was performed at 105°C for 5 hours. After hydrothermal, the nickel foam was washed with deionized water, dried, and calcined in a muffle furnace at 350°C for 2 hours to obtain the positive electrode.
[0035] Assemble the battery by assembling the mold, zinc foil, electrolyte, positive electrode and mold in sequence to obtain a battery.
[0036] Comparative Example 1
[0037] Preparation of electrolyte: At room temperature, weigh 3.6353 g Zn(OTf)2 and dissolve it in 10 mL deionized water. Stir well and let stand for 3 days to obtain zinc-air electrolyte.
[0038] The battery mold was assembled by the above method. The active electrode material used in this embodiment was Co3O4, and the electrolyte was the zinc-air electrolyte prepared in this comparative example.
[0039] Full discharge performance test: Test results are as follows Figure 2 As shown, the discharge capacity is 12.88 mAh.
[0040] Cycle performance test: Test results are as follows Figure 4 As shown, the cycle time is 67h.
[0041] Example 1
[0042] Preparation of electrolyte: At room temperature, weigh 3.6353 g Zn(OTf)2 and dissolve it in 10 mL deionized water. Then take 1.2212 g nicotinamide and add it to the above electrolyte. Stir well and let it stand for 3 days to obtain zinc-air electrolyte.
[0043] The battery mold was assembled by the above method. The active electrode material used in this embodiment was Co3O4, and the electrolyte was the zinc-air electrolyte prepared in this comparative example.
[0044] Full discharge performance test: Test results are as follows Figure 3 As shown, the discharge capacity is 48.32 mAh. It can be seen that the addition of astaxanthin effectively inhibits side reactions, reduces the attack of active oxygen groups, and improves the discharge specific capacity.
[0045] Cycle performance test: Test results are as follows Figure 5 As shown, the cycle time is 200h.
[0046] Example 2
[0047] Preparation of electrolyte: At room temperature, weigh 3.6353 g Zn(OTf)2 and dissolve it in 10 mL deionized water. Then take 2.4425 g nicotinamide and add it to the above electrolyte. Stir well and let it stand for 3 days to obtain zinc-air electrolyte.
[0048] The battery mold was assembled by the above method. The active electrode material used in this embodiment was Co3O4, and the electrolyte was the zinc-air electrolyte prepared in this comparative example.
[0049] Cycle performance test: cycle time is 180h.
[0050] Example 3
[0051] Preparation of electrolyte: At room temperature, weigh 3.6353 g Zn(OTf)2 and dissolve it in 10 mL deionized water. Then take 3.6637 g nicotinamide and add it to the above electrolyte. Stir well and let it stand for 3 days to obtain zinc-air electrolyte.
[0052] The battery mold was assembled by the above method. The active electrode material used in this embodiment was Co3O4, and the electrolyte was the zinc-air electrolyte prepared in this comparative example.
[0053] Cycle performance test: cycle time is 120h.
Claims
1. Use of nicotinamide as a solid co-solvent for zinc-air battery electrolyte, and / or Application of nicotinamide in preparing zinc-air battery electrolyte, including solvent, zinc salt and solid co-solvent.
2. The zinc-air battery electrolyte according to claim 1, characterized in that: The electrolyte consists of a solvent, a zinc salt and a solid co-solvent.
3. The zinc-air battery electrolyte according to claim 1, characterized in that: The zinc salt is at least one of ZnSO4, ZnCl2, Zn(Ac)2 and Zn(OTf)2, The solvent for dissolving the zinc salt is water, The solid co-solvent is nicotinamide.
4. The zinc-air battery electrolyte according to claim 1, characterized in that: The concentration of the zinc salt is 0.001 to 5 mol / L, specifically 1 mol / L, and the concentration of the solid co-solvent is 0.001 to 5 mol / L; specifically 1 to 3 mol / L.
5. The method for preparing a zinc-air battery electrolyte according to claim 1, wherein: The following steps are involved: The zinc salt is dissolved in the solvent, and then the solid co-solvent is added, fully stirred, and allowed to stand for 3 to 4 days to obtain the battery electrolyte.
6. Use of the battery electrolyte as claimed in claim 1 in the preparation of a zinc-air battery.
7. A zinc-air battery, wherein the electrolyte used is the zinc-air battery electrolyte as claimed in claim 1.
8. A zinc-air battery, wherein the positive active electrode material is at least one of nitrogen-doped graphene, multi-walled carbon nanotubes, Ketjen black, Super P, carbocarbon, ruthenium dioxide, cobalt tetroxide / nickel foam and nickel / nickel oxide.
Citation Information
Patent Citations
Electrolyte additives for zinc metal electrodes
CN110770949A
Multi-functional lithium air battery electrolyte additive
CN113363577A
Battery having zinc plated copper electrode and method of making the same
US11769869B1
Cited By
Nicotinamide-containing aqueous zinc ion battery electrolyte, battery and preparation method