Outer packaging material for all-solid-state battery, method for producing same, and all-solid-state battery
By setting a barrier layer protective film in the outer packaging material of the all-solid battery and controlling the hydrogen sulfide transmission amount of the hot-welded resin layer, the problems of peeling off the solid electrolyte and active material layer and accumulation of hydrogen sulfide gas are solved, and the high voltage of the battery is achieved Improved stability and safety.
Patent Information
- Application Number
- CN202410988324.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2019-01-23
- Filing Date
- 2020-01-23
- Publication Date
- 2024-11-08
AI Technical Summary
In the high-voltage state, a full-solid battery is prone to peel off between the solid electrolyte and the negative electrode active material layer or the positive electrode active material layer, and the sulfide-based inorganic solid electrolyte produces toxic hydrogen sulfide gas when reacting with water, which poses a safety hazard.
An outer packaging material consisting of a base material layer, a barrier layer and a hot-weld resin layer is used, and a barrier layer protective film is provided on the surface of the barrier layer to ensure that the hydrogen sulfide transmission amount of the hot-weld resin layer reaches 1.0×10-8cc·mm /cm2·sec·cmHg or more to suppress deterioration of the barrier layer and discharge of hydrogen sulfide generated inside.
It effectively suppresses the deterioration of the barrier layer of the outer packaging material, prevents the accumulation of hydrogen sulfide, and improves the safety and performance stability of all-solid batteries.
Smart Images

Figure CN118919964A_ABST
Abstract
Description
[0001] This case is filed on January 23, 2020 、Application No. 202080010355.2(PCT / JP2020 / 002424) 、The name of the invention is Outer packaging material for all-solid-state battery, method for producing the same, and all-solid-state battery Divisional application. Technical Field
[0002] The present invention relates to an outer packaging material for an all-solid battery, a method for producing the same, and an all-solid battery. Background Art
[0003] All-solid batteries in which the electrolyte is a solid electrolyte are known. Since no organic solvent is used in the battery, the all-solid battery has the advantages of high safety and a wide operating temperature range.
[0004] On the other hand, it is known that in all-solid-state batteries, due to the expansion and contraction of the negative electrode or positive electrode during charge and discharge, separation between the solid electrolyte and the negative electrode active material layer or the positive electrode active material layer is likely to occur, and battery degradation is likely to occur.
[0005] As a method of suppressing the peeling between the solid electrolyte and the negative electrode active material layer or the positive electrode active material layer, a technique of restricting the all-solid battery in a state of high pressure pressing is known. For example, Patent Document 1 discloses a method for manufacturing a battery, which includes: a lamination process of making a laminate having a positive electrode collector, a positive electrode layer, an electrolyte layer, a negative electrode layer and a negative electrode collector in sequence; a pressurizing process of pressurizing the laminate obtained in the lamination process in the lamination direction; and a restricting process of restricting the laminate in a state where the laminate is pressurized in the lamination direction at a pressure of 0.1 MPa or more and 100 MPa or less for a prescribed time after the pressurizing process.
[0006] In addition, it is known that sulfide-based inorganic solid electrolytes have high ion conductivity among inorganic solid electrolytes. However, as described in Patent Document 2, for example, sulfide-based inorganic solid electrolytes contain sulfur compounds that may produce toxic hydrogen sulfide once reacting with water. Therefore, in the event of damage to the all-solid-state battery, there is a risk of reacting with moisture in the air to produce hydrogen sulfide gas.
[0007] Prior art literature
[0008] Patent Literature
[0009] Patent Document 1: Japanese Patent Application Publication No. 2012-142228
[0010] Patent Document 2: Japanese Patent Application Publication No. 2008-103288 Summary of the invention
[0011] Problems to be solved by the invention
[0012] In the use environment of all-solid-state batteries, in order to inhibit the peeling between the solid electrolyte and the negative electrode active material layer or the positive electrode active material layer, it is expected to continuously confine the solid electrolyte and the negative electrode active material layer and the positive electrode active material layer by performing high-pressure pressing on the all-solid-state battery from the outside of the outer packaging material.
[0013] On the other hand, in recent years, with the high performance of electric vehicles, hybrid electric vehicles, personal computers, cameras, mobile phones, etc., all-solid batteries require a variety of shapes, and require thinning and lightweight. However, in the prior art, the metal outer packaging materials often used in batteries have the disadvantages of being difficult to follow the diversification of shapes and having a limit to lightweight. Therefore, as an outer packaging material that is easy to process into various shapes and can achieve thinning and lightweight, a film-like outer packaging material having a base material / metal foil layer / thermofusible resin layer laminated in sequence is proposed.
[0014] In such a film-like outer packaging material, a space for accommodating battery elements is usually designed by molding into a bag shape or using a mold, and battery elements such as electrodes and solid electrolytes are arranged in the space, and the heat-fusible resin layers are heat-fused to each other, thereby obtaining an all-solid-state battery in which the battery elements are accommodated on the inner side of the outer packaging material.
[0015] By applying a film-like outer casing material to an outer casing material of an all-solid-state battery, it is expected that electric vehicles, hybrid electric vehicles, and the like can be reduced in weight.
[0016] However, when the solid electrolyte and the negative electrode active material layer or the positive electrode active material layer are continuously restricted at high pressure from the outside of the outer packaging material of the all-solid battery, the heat-fusible resin layer of the outer packaging material is strongly pressed against the battery element, and the thickness of the heat-fusible resin layer (inner layer) of the outer packaging material becomes thinner, which may cause the barrier layer stacked by the outer packaging material to contact the solid electrolyte. In particular, the inventors of the present invention conducted research and found that when the barrier layer of the outer packaging material is in contact with the solid electrolyte containing the sulfide solid electrolyte material, when electricity is passed between them, an alloy is generated on the surface of the barrier layer, and the barrier layer deteriorates. Once the barrier layer of the outer packaging material deteriorates, the barrier property of the outer packaging material to the battery element will be reduced.
[0017] In addition, Patent Document 2 proposes the following technology: in an all-solid-state battery using a sulfide-based inorganic solid electrolyte, in order to cope with the generation of hydrogen sulfide gas when the all-solid-state battery is damaged, the outer casing of the all-solid-state battery is further covered with an adsorbent and / or a material containing an alkaline substance.
[0018] However, when a film-like outer packaging material having a substrate / barrier layer / thermo-fusible resin layer laminated in sequence is used, not only the all-solid-state battery is damaged, but also a trace amount of water vapor may penetrate into the interior of the all-solid-state battery from the heat-fused portions of the heat-fused resin layers, and hydrogen sulfide may be generated inside the all-solid-state battery. Furthermore, the inventors of the present invention believe that if the hydrogen sulfide generated inside the all-solid-state battery is not retained inside the all-solid-state battery but is actively discharged, the internal pressure rise of the all-solid-state battery can be suppressed.
[0019] Under such circumstances, the main purpose of the present invention is to provide an outer packaging material for an all-solid-state battery, which is applied to an all-solid-state battery using a solid electrolyte containing a sulfide solid electrolyte material, and can effectively suppress the degradation of the barrier layer of the outer packaging material even when the all-solid-state battery is confined in a high-voltage state, and can discharge hydrogen sulfide generated inside the all-solid-state battery to the outside.
[0020] Methods for solving problems
[0021] The inventors of the present invention have conducted intensive research to solve the above-mentioned problems. As a result, it has been found that, in an outer packaging material for a solid-state battery composed of a laminated body having at least a base layer, a barrier layer, and a heat-fusible resin layer in order from the outside, by providing a barrier layer protective film on the surface of the barrier layer of the outer packaging material and setting the hydrogen sulfide permeation amount of the resin constituting the heat-fusible resin layer to a prescribed value or more, even when the solid-state battery is restrained in a high-pressure state, the degradation of the barrier layer of the outer packaging material can be effectively suppressed, and the hydrogen sulfide generated inside the solid-state battery can be discharged to the outside.
[0022] The present invention has been completed through further research based on these findings. That is, the present invention provides the following aspects.
[0023] An outer packaging material for an all-solid-state battery, for an all-solid-state battery containing a sulfide solid electrolyte material, the outer packaging material for an all-solid-state battery comprising, from the outside, at least a substrate layer, a barrier layer, a barrier layer protective film formed on the surface of the barrier layer, and a heat-fusible resin layer, wherein the hydrogen sulfide permeability of the resin constituting the heat-fusible resin layer is 1.0×10 -8 cc mm / cm 2 ·sec·cmHg or more.
[0024] Effects of the Invention
[0025] According to the present invention, it is possible to provide an outer packaging material for an all-solid-state battery, which is an outer packaging material for an all-solid-state battery using a solid electrolyte containing a sulfide solid electrolyte material, and can effectively suppress the degradation of the barrier layer of the outer packaging material even when the all-solid-state battery is confined in a high-voltage state, and can discharge hydrogen sulfide generated inside the all-solid-state battery to the outside. In addition, according to the present invention, it is also possible to provide a method for manufacturing an outer packaging material for an all-solid-state battery and an all-solid-state battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 This is a schematic diagram showing an example of the cross-sectional structure of an all-solid-state battery to which the all-solid-state battery casing material of the present invention is applied.
[0027] Figure 2 This is a schematic diagram showing an example of the cross-sectional structure of an all-solid-state battery to which the all-solid-state battery casing material of the present invention is applied.
[0028] Figure 3 This is a schematic plan view of an example of an all-solid-state battery to which the all-solid-state battery casing material of the present invention is applied.
[0029] Figure 4 It is a schematic cross-sectional view showing an example of the laminated structure of the all-solid-state battery packaging material of the present invention.
[0030] Figure 5 It is a schematic cross-sectional view showing an example of the laminated structure of the all-solid-state battery packaging material of the present invention.
[0031] Figure 6 It is a schematic cross-sectional view showing an example of the laminated structure of the all-solid-state battery packaging material of the present invention.
[0032] Figure 7 It is a schematic cross-sectional view showing an example of the laminated structure of the all-solid-state battery packaging material of the present invention.
[0033] Figure 8 This is a schematic diagram for explaining a method for measuring the hydrogen sulfide permeation amount of a resin constituting a thermally adhesive resin layer in Examples.
[0034] Description of Reference Numerals
[0035] 1: substrate layer; 2: adhesive layer; 3: barrier layer; 3a, 3b: barrier layer protective film; 4: heat-fusible resin layer; 5: adhesive layer; 10: outer packaging material for all-solid-state battery; 20: negative electrode layer; 21: negative electrode active material layer; 22: negative electrode collector; 30: positive electrode layer; 31: positive electrode active material layer; 32: positive electrode collector; 40: solid electrolyte layer; 50: single cell; 60: terminal; 70: all-solid-state battery. DETAILED DESCRIPTION
[0036] The all-solid-state battery outer packaging material of the present invention is composed of a laminate having at least a substrate layer, a barrier layer, a barrier layer protective film formed on the surface of the barrier layer, and a heat-fusible resin layer in order from the outside. The all-solid-state battery outer packaging material is used for an all-solid-state battery containing a sulfide solid electrolyte material. The all-solid-state battery outer packaging material is characterized in that the hydrogen sulfide permeation amount of the resin constituting the heat-fusible resin layer is 1.0×10 -8 cc mm / cm 2 ·sec·cmHg or more. The all-solid-state battery outer packaging material of the present invention has such a structure, and even when the all-solid-state battery is confined in a high-pressure state, it is possible to effectively suppress the degradation of the barrier layer of the outer packaging material and discharge hydrogen sulfide generated inside the all-solid-state battery to the outside.
[0037] The all-solid battery outer packaging material of the present invention is described in detail below. In this specification, the numerical range indicated by "to" means "above" or "below". For example, the expression of 2 to 15 mm means above 2 mm and below 15 mm.
[0038] 1. Laminated structure of outer packaging materials for all-solid-state batteries
[0039] For example Figure 4 to Figure 7 As shown, the outer packaging material 10 of the present invention is composed of a laminated body having at least a base layer 1, a barrier layer 3, a barrier layer protective film 3a formed on the surface of the barrier layer 3, and a heat-fusible resin layer 4 in this order. In the outer packaging material 10, the base layer 1 is the outer layer side, and the heat-fusible resin layer 4 is the inner layer side. When the all-solid battery is assembled using the outer packaging material 10 and the battery element, the peripheral portions are heat-fused in a state where the heat-fusible resin layers 4 of the outer packaging material 10 are facing each other, and the battery element is accommodated in the space formed thereby.
[0040] A barrier layer protective film 3a is provided on the surface of the barrier layer 3 on the side of the heat-fusible resin layer 4. The barrier layer protective film 3a contains chromium. Figures 4 to 7 A schematic diagram showing a case where the outer packaging material 10 of the present invention has a barrier layer protective film 3a on the surface of the barrier layer 3 on the side of the heat-fusible resin layer 4. Figures 5 to 7 Schematic diagram showing a case where the outer packaging material 10 has barrier layer protective films 3a and 3b on both sides of the barrier layer 3. In addition, as described later, in the outer packaging material 10, the barrier layer protective film 3a may be provided only on the surface of the barrier layer 3 on the side of the heat-fusible resin layer 4, or the barrier layer protective films 3a and 3b may be provided on both sides of the barrier layer 3.
[0041] like Figure 6 and Figure 7As shown in FIG. 1 , the all-solid-state battery outer packaging material 10 may have an adhesive layer 2 between the substrate layer 1 and the barrier layer 3 (in the case of a barrier layer protective film 3 b, between the substrate layer 1 and the barrier layer protective film 3 b) as needed to improve the adhesion between these layers. Figure 6 and Figure 7 As shown in FIG. 1 , an adhesive layer 5 may be provided between the barrier layer protective film 3a and the heat-fusible resin layer 4, in order to improve the adhesion between these layers. Figure 7 As shown, a surface coating layer 6 or the like may be provided on the outer side of the base material layer 1 (the side opposite to the thermally fusible resin layer 4 side) as necessary.
[0042] The details of each layer constituting the outer packaging material 10 are described in detail in the item “3. Each layer constituting the outer packaging material”.
[0043] The thickness of the laminate constituting the outer packaging material 10 for all-solid batteries is not particularly limited. From the perspective of reducing costs and improving energy density, it is preferably about 10000 μm or less, about 8000 μm or less, and about 5000 μm or less. From the perspective of maintaining the function of the outer packaging material 10 for all-solid batteries such as protecting battery elements, it is preferably about 100 μm or more, about 150 μm or more, and about 200 μm or more. Regarding the preferred range, for example, about 100 to 10000 μm, about 100 to 8000 μm, about 100 to 5000 μm, about 150 to 10000 μm, about 150 to 8000 μm, about 150 to 5000 μm, about 200 to 10000 μm, about 200 to 8000 μm, about 200 to 5000 μm, and about 100 to 500 μm is particularly preferred.
[0044] The details of each layer constituting the all-solid-state battery outer casing material 10 are described in detail in the section “3. Each layer forming the all-solid-state battery outer casing material”.
[0045] 2. All-solid-state batteries
[0046] Regarding the all-solid battery to which the all-solid battery outer packaging material 10 of the present invention is applied (hereinafter sometimes referred to as "outer packaging material 10"), there are no particular restrictions except that the solid electrolyte layer 40 contains a sulfide solid electrolyte material and a specific outer packaging material 10 is used. That is, as for the structure other than the solid electrolyte layer 40 and the outer packaging material 10 (electrodes, terminals, etc.), there are no particular restrictions as long as it is a structure suitable for an all-solid battery, and it can be a structure used in a known all-solid battery. Below, taking the all-solid battery 70 of the present invention as an example, the method of applying the all-solid battery outer packaging material 10 of the present invention to the all-solid battery is specifically described.
[0047] like Figures 1 to 3 As shown in the schematic diagram of , the all-solid battery 70 of the present invention is obtained by containing at least a battery element of a single cell 50 in a package formed by the outer packaging material 10 for the all-solid battery of the present invention, and the above-mentioned single cell 50 includes a positive electrode active material layer 31, a negative electrode active material layer 21, and a solid electrolyte layer 40 stacked between the positive electrode active material layer 31 and the negative electrode active material layer 21. More specifically, the positive electrode active material layer 31 is stacked on the positive electrode collector 32 to form the positive electrode layer 30, and the negative electrode active material layer 21 is stacked on the negative electrode collector 22 to form the negative electrode layer 20. The positive electrode collector 32 and the negative electrode collector 22 are respectively connected to the terminal 60 exposed to the outside and are electrically connected to the external environment. The solid electrolyte layer 40 is stacked between the positive electrode layer 30 and the negative electrode layer 20, and the positive electrode layer 30, the negative electrode layer 20 and the solid electrolyte layer 40 constitute the single cell 50. The battery element of the all-solid-state battery 70 may include only one unit cell 50 , or may include a plurality of unit cells 50 . Figure 1 70 including two single cells 50 as battery elements, Figure 2 A full solid-state battery 70 is shown in which three unit cells 50 are stacked to form a battery element.
[0048] In the all-solid battery 70, the battery element is covered in a manner that a flange portion (an area where the heat-fusible resin layers 4 are in contact with each other) is formed at the periphery of the battery element, while the terminals 60 connected to the positive electrode layer 30 and the negative electrode layer 20 are protruding outward, and the heat-fusible resin layers 4 of the flange portion are heat-sealed to each other to seal the battery element, thereby forming an all-solid battery using an outer packaging material for an all-solid battery. In the case where the battery element is accommodated in a packaging body formed by the outer packaging material 10 for an all-solid battery of the present invention, the packaging body is formed in a manner that the heat-fusible resin portion of the outer packaging material 10 for an all-solid battery of the present invention becomes the inner side (the surface in contact with the battery element).
[0049] As described above, there are no particular limitations on the all-solid battery to which the outer packaging material 10 of the present invention is applied, as long as the solid electrolyte contains a sulfide solid electrolyte material and a specific outer packaging material 10 is used, and the same applies to the all-solid battery 70 of the present invention. The following is an example of the materials and the like constituting the battery element of the all-solid battery to which the outer packaging material 10 of the present invention is applied.
[0050] As described above, in the battery element of the all-solid-state battery 70, at least the positive electrode layer 30, the negative electrode layer 20, and the solid electrolyte layer 40 constitute a single cell 50. The positive electrode layer 30 has a structure in which a positive electrode active material layer 31 is stacked on a positive electrode collector 32. The negative electrode layer 20 has a structure in which a negative electrode active material layer 21 is stacked on a negative electrode collector 22. Moreover, the positive electrode collector 32 and the negative electrode collector 22 are respectively connected to the terminal 60 exposed to the outside, and are electrically connected to the external environment.
[0051] [Positive Electrode Active Material Layer 31]
[0052] The positive electrode active material layer 31 is a layer containing at least a positive electrode active material. In addition to the positive electrode active material, the positive electrode active material layer 31 may contain a solid electrolyte material, a conductive material, a binder, etc. as necessary.
[0053] There are no particular restrictions on the positive electrode active material, and examples thereof include oxide active materials, sulfide active materials, and the like. In the case where the all-solid battery is an all-solid lithium battery, examples of the oxide active material used as the positive electrode active material include LiCoO2, LiMnO2, LiNiO2, LiVO2, LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2 and other rock salt layered active materials, LiMn2O4, Li(Ni 0.5 Mn 1.5 )O4 and other spinel active materials, LiFePO4, LiMnPO4 and other olivine active materials, Li2FeSiO4, Li2MnSiO4 and other Si-containing active materials, etc. In addition, as sulfide active materials used as positive electrode active materials of all-solid-state lithium batteries, for example, copper chevron, iron sulfide, cobalt sulfide, nickel sulfide, etc. can be listed.
[0054] The shape of the positive electrode active material is not particularly limited, and an example thereof may be a particle shape. The average particle size (D 50 ) is preferably about 0.1 to 50 μm, for example. The content of the positive electrode active material in the positive electrode active material layer 31 is preferably about 10 to 99 mass %, more preferably about 20 to 90 mass %.
[0055] The positive electrode active material layer 31 preferably further contains a solid electrolyte material. This can improve the ion conductivity in the positive electrode active material layer 31. The solid electrolyte material contained in the positive electrode active material layer 31 is the same as the solid electrolyte material exemplified in the solid electrolyte layer 40 described later. The content of the solid electrolyte material in the positive electrode active material layer is preferably about 1 to 90 mass %, more preferably about 10 to 80 mass %.
[0056] The positive electrode active material layer 31 may further contain a conductive material. By adding a conductive material, the electronic conductivity of the positive electrode active material layer can be improved. As the conductive material, for example, acetylene black, Ketjen black, carbon fiber, etc. can be listed. In addition, the positive electrode active material layer may further contain a binding material. As the binding material, for example, fluorine-containing binding materials such as polytetrafluoroethylene (PTFE) and polyvinylidene fluoride (PVDF) can be listed.
[0057] The thickness of the positive electrode active material layer 31 can be appropriately set according to the size of the all-solid-state battery, and is preferably about 0.1 to 1000 μm.
[0058] [Positive electrode current collector 32]
[0059] Examples of the material constituting the positive electrode current collector 32 include stainless steel (SUS), aluminum, nickel, iron, titanium, and carbon.
[0060] The thickness of the positive electrode current collector 32 can be appropriately set according to the size of the all-solid-state battery, and is preferably about 10 to 1000 μm.
[0061] [Negative Electrode Active Material Layer 21]
[0062] The negative electrode active material layer 21 is a layer containing at least a negative electrode active material. In addition to the negative electrode active material, the negative electrode active material layer 21 may contain a solid electrolyte material, a conductive material, a binder, etc. as necessary.
[0063] There are no particular restrictions on the negative electrode active material, and examples thereof include carbon active materials, metal active materials, oxide active materials, and the like. Examples of carbon active materials include graphites such as mesocarbon microbeads (MCMB) and highly oriented graphite (HOPG), and amorphous carbons such as hard carbon and soft carbon. Examples of metal active materials include In, Al, Si, and Sn. Examples of oxide active materials include Nb2O5, Li4Ti5O 12 , SiO, etc.
[0064] The shape of the negative electrode active material is not particularly limited, and examples thereof include particle shape and film shape. The average particle size (D 50) is preferably about 0.1 to 50 μm. The content of the negative electrode active material in the negative electrode active material layer 21 is, for example, about 10 to 99 mass %, more preferably about 20 to 90 mass %.
[0065] The negative electrode active material layer 21 preferably further contains a solid electrolyte material. This can improve the ion conductivity in the negative electrode active material layer 21. In addition, the solid electrolyte material contained in the negative electrode active material layer 21 is the same as the solid electrolyte material exemplified in the solid electrolyte layer 40 described later. The content of the solid electrolyte material in the negative electrode active material layer 21 is preferably about 1 to 90 mass %, more preferably about 10 to 80 mass %.
[0066] The negative electrode active material layer 21 may further contain a conductive material. In addition, the negative electrode active material layer 21 may further contain a binder. The conductive material and the binder are the same as those exemplified in the positive electrode active material layer 31 described above.
[0067] The thickness of the negative electrode active material layer 21 can be appropriately set depending on the size of the all-solid-state battery, and is preferably about 0.1 to 1000 μm.
[0068] [Negative Electrode Collector 22]
[0069] Examples of the material constituting the negative electrode current collector 22 include stainless steel (SUS), copper, nickel, and carbon.
[0070] The thickness of the negative electrode current collector 22 can be appropriately set according to the size of the all-solid battery, and is preferably about 10 to 1000 μm.
[0071] [Solid electrolyte layer 40]
[0072] The solid electrolyte layer 40 is a layer containing a sulfide solid electrolyte material.
[0073] Sulfide solid electrolyte materials are more preferred than oxide solid electrolyte materials because they have higher ion conductivity. When the all-solid battery outer packaging material 10 of the present invention is applied to an all-solid battery containing a sulfide solid electrolyte material, hydrogen sulfide generated inside the all-solid battery can be appropriately discharged.
[0074] In addition, specific examples of sulfide solid electrolyte materials include Li2S-P2S5, Li2S-P2S5-LiI, Li2S-P2S5-Li2O, Li2S-P2S5-Li2O-LiI, Li2S-SiS2, Li2S-SiS2-LiI, Li2S-SiS2-LiBr, Li2S-SiS2-LiCl, Li2S-SiS2-B2S3-LiI, Li2S-SiS2-P2S5-LiI, Li2S-B2S3, Li2S-P2S5-Z m S n (where m and n are positive numbers; Z is any one of Ge, Zn, and Ga), Li2S-GeS2, Li2S-SiS2-Li3PO4, Li2S-SiS2-Li x MO y (where x and y are positive numbers; M is any one of P, Si, Ge, B, Al, Ga, and In), etc. The above description of "Li2S-P2S5" refers to a sulfide solid electrolyte material made using a raw material composition containing Li2S and P2S5, and the same applies to other descriptions. In addition, the sulfide solid electrolyte material may be sulfide glass or crystallized sulfide glass.
[0075] The content of the solid electrolyte material in the solid electrolyte layer 40 is not particularly limited, but is preferably 60% by mass or more, more preferably 70% by mass or more, and further preferably 80% by mass or more. The solid electrolyte layer may contain a binder or may consist only of a solid electrolyte material.
[0076] The thickness of the solid electrolyte layer 40 can be appropriately set according to the size of the all-solid battery, and is preferably about 0.1 to 1000 μm, and more preferably about 0.1 to 300 μm.
[0077] The all-solid battery 70 of the present invention is suitable for use in an environment where it is restricted from the outside under high pressure. As the pressure for restricting the all-solid battery 70 from the outside, from the viewpoint of appropriately suppressing the peeling between the solid electrolyte and the negative electrode active material layer (and between the solid electrolyte and the positive electrode active material layer), preferably about 0.1MPa or more, more preferably 5MPa or more, further preferably about 1MPa or more, and preferably about 100MPa or less, more preferably about 30MPa or less. As a preferred range, about 0.1 to 100MPa, about 0.1 to 70MPa, about 5 to 100MPa, about 5 to 70MPa, about 10 to 100MPa, and about 1 to 30MPa can be listed. As a method for restricting the all-solid battery 70 from the outside under high pressure, a method of clamping the all-solid battery with a metal plate or the like, fixing it in a state of high pressure pressing (for example, fastening it with a vise or the like) can be listed.
[0078] Methods for restricting the all-solid battery 70 from the outside under high pressure include clamping the all-solid battery with metal plates, fixing it under high pressure pressing (for example, fastening it with a vise, etc.), and gas pressurization.
[0079] From the same viewpoint, the temperature when the all-solid battery 70 is restrained from the outside is preferably 20°C or higher, more preferably 40°C or higher, and preferably 200°C or lower, more preferably 150°C or lower. The preferred range is about 20 to 150°C.
[0080] The shape of the all-solid-state battery 70 of the present invention is not particularly limited. Figure 3 As shown in the schematic diagram, it is preferably rectangular when viewed from above. It is further preferred that the ratio of the length of the first side of the all-solid-state battery 70, which is rectangular when viewed from above, to the length of the second side in the direction perpendicular to the first side (the length of the first side: the length of the second side) is about 1:1 to 1:5. Among them, if the length of the second side is too long relative to the length of the first side, when the outer packaging material 10 is molded to form the molding portion M described later, the second side is difficult to fix to the mold, and there is a tendency for the R value (radius of curvature) of the ridge portion of the molding portion M along the second side (the first curved portion described later) to become too large.
[0081] like Figure 1 to Figure 3 As shown in the schematic diagram of the present invention, in the all-solid battery 70, the battery element is preferably housed in a molding portion M which is rectangular in shape when viewed from above, and the molding portion M is formed in such a way that the outer packaging material 10 protrudes from the thermally fusible resin layer 4 side toward the barrier layer 3 side. Figure 1 FIG. 7 shows a diagram in which a molded portion M is formed on one side of a solid-state battery 70. Figure 2 A diagram showing that the molded portion M is formed on both sides of the all-solid-state battery 70 .
[0082] In the present invention, when the all-solid-state battery 70 is viewed from the barrier layer 3 side, the two sides ( Figures 1 to 3 A straight line parallel to the two sides parallel to the y direction or the two sides parallel to the z direction) and passing through the middle of the two parallel sides (refer to Figure 3 In the cross section of the outer packaging material 10 in the thickness direction on the imaginary line Y in the y direction and the imaginary line Z in the z direction), the outer packaging material 10 has the first curved portion R1 (see Figure 2 R1z) and the second curved portion R2 (refer to Figure 2R2z), the R value (radius of curvature) of the first curved portion R1 is preferably greater than 1 mm. If the R value (radius of curvature) is greater than 1 mm, the force of stretching the outer packaging material 10 will not become too large at the corners (corners) of the rectangular molding portion M, and the generation of pinholes in the barrier layer 3 before reaching the specified molding depth can be suppressed. If the outer packaging material 10 is molded using a mold, the molding portion M having the first curved portion R1 and the second curved portion R2 is formed in a manner such that the outer packaging material 10 protrudes from the side of the thermally fusible resin layer 4 to the side of the barrier layer 3. In the molding portion M, the first curved portion R1 is located at a position protruding from the outside of the all-solid-state battery.
[0083] exist Figure 3 In the schematic diagram, the cross-sectional view on the dotted line Z is Figure 2 Corresponding to the schematic diagram of FIG. 1 , the molded portion M has a first curved portion R1z and a second curved portion R2z in sequence from the center portion to the end portion of the outer packaging material 10. Figure 3 In the schematic diagram, on the cross section on the dotted line Y, the molding portion M has a first bend R1y and a second bend R2y in sequence from the center to the end of the outer packaging material 10. Among them, the expression of the first bend R1z means the first bend in the z direction. Similarly, the expression of the second bend R2z means the second bend in the z direction, the expression of the first bend R1y means the first bend in the y direction, and the expression of the second bend R2y means the second bend in the y direction. Regarding the first bend R1y, as with the R value of the first bend R1 mentioned above, if the R value (radius of curvature) is greater than 1 mm, the force of stretching the outer packaging material 10 at the corner (corner) of the rectangular molding portion M will not become too large, and the generation of pinholes in the barrier layer 3 can be suppressed before the specified molding depth is reached, so the R value (radius of curvature) is preferably greater than 1 mm.
[0084] In the present invention, the R values (radii of curvature) of the first curved portion R1 and the second curved portion R2 are respectively the barrier layer 3 side of the outer packaging material 10 (i.e., the outer surface side of the outer packaging material 10, for example Figure 2 The R value (radius of curvature) of the surface (the area surrounded by the dotted line).
[0085] In the all-solid battery 70, in order to minimize the dead space inside the battery and increase the volume energy density, if the Figure 3 For explanation, it is preferred that the first side parallel to the y direction of the all-solid-state battery that is rectangular in shape when viewed from above is the short side, and the second side parallel to the z direction is the long side, and the R value (radius of curvature) of the first bend R1z of the all-solid-state battery that is rectangular in shape when viewed from above along the short side parallel to the y direction where the terminal is set is greater than the R value (radius of curvature) of the first bend R1y along the long side parallel to the z direction.
[0086] 3. Forming the layers of the outer packaging material for all-solid-state batteries
[0087] The outer packaging material 10 of the present invention is composed of a laminated body having at least a base layer 1, a barrier layer 3, a barrier layer protective film 3a formed on the surface of the barrier layer 3, and a heat-fusible resin layer 4 in this order from the outside. When the barrier layer protective film 3a is analyzed by time-of-flight secondary ion mass spectrometry, the PO3 - The peak intensity P PO3 Relative to CrPO4 - The peak intensity P CrPO4 Ratio P PO3 / CrPO4 The hydrogen sulfide permeation rate of the resin constituting the heat-adhesive resin layer 4 is within the range of 6 to 120. -8 cc mm / cm 2 ·sec·cmHg or more Hereinafter, each layer constituting the outer packaging material 10 of the present invention will be described in detail.
[0088] [Base material layer 1]
[0089] In the present invention, the base material layer 1 is a layer provided on the outside of the barrier layer 3 (on the outside of the barrier layer protective film 3b when there is a barrier layer protective film 3b) as needed in order to fulfill the function as a base material of the outer packaging material 10. The base material layer 1 is located on the outer layer side of the outer packaging material 10.
[0090] There is no particular limitation on the material forming the base layer 1 as long as it can function as a base material, that is, has at least insulating properties. The base layer 1 can be formed using, for example, a resin, and the resin may contain additives described below.
[0091] When the substrate layer 1 is formed of a resin, the substrate layer 1 may be, for example, a resin film formed of a resin, or may be formed by coating a resin. The resin film may be an unstretched film or a stretched film. As a stretched film, a uniaxially stretched film and a biaxially stretched film may be cited, preferably a biaxially stretched film. As a stretching method for forming a biaxially stretched film, for example, a sequential biaxial stretching method, an inflation method, a simultaneous biaxial stretching method, etc. may be cited. As a method for coating a resin, a roll coating method, a gravure coating method, an extrusion coating method, etc. may be cited.
[0092] Examples of the resin forming the substrate layer 1 include polyester, polyamide, polyolefin, epoxy resin, acrylic resin, fluororesin, polyurethane, silicone resin, phenolic resin and the like, or modified products of these resins. In addition, the resin forming the substrate layer 1 may be a copolymer of these resins, or a modified product of the copolymer. Furthermore, it may be a mixture of these resins.
[0093] As the resin forming the base material layer 1, polyester and polyamide are preferably used among them.
[0094] As polyester, specifically, polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polybutylene naphthalate, polyethylene isophthalate, copolyester, etc. can be cited. In addition, as copolyester, copolyester with ethylene terephthalate as the main body of repeating unit can be cited. Specifically, copolymer polyester with ethylene terephthalate as the main body of repeating unit and polymerized with ethylene isophthalate (hereinafter, abbreviated as polyethylene glycol (terephthalate / isophthalate)), polyethylene glycol (terephthalate / adipate), polyethylene glycol (terephthalate / sodium sulfoisophthalate), polyethylene glycol (terephthalate / sodium isophthalate), polyethylene glycol (terephthalate / phenyl diphthalate), polyethylene glycol (terephthalate / decane dicarboxylate), etc. can be cited. These polyesters may be used alone or in combination of two or more.
[0095] In addition, specific examples of polyamides include aliphatic polyamides such as nylon 6, nylon 66, nylon 610, nylon 12, nylon 46, and copolymers of nylon 6 and nylon 66; hexamethylenediamine-isophthalic acid-terephthalic acid copolymer polyamides such as nylon 6I, nylon 6T, nylon 6IT, and nylon 6I6T (I represents isophthalic acid and T represents terephthalic acid) containing structural units derived from terephthalic acid and / or isophthalic acid; and polyamides. Aromatic polyamides such as MXD6 (poly(m-xylylene adipamide)), alicyclic polyamides such as polyamide PACM6 (poly(bis(4-aminocyclohexyl)methane adipamide), polyamides obtained by copolymerizing lactam components or isocyanate components such as 4,4′-diphenylmethane-diisocyanate, polyesteramide copolymers or polyetheresteramide copolymers which are copolymers of copolyamide and polyester or polyalkylene ether glycol, and copolymers thereof. These polyamides may be used alone or in combination of two or more.
[0096] The substrate layer 1 preferably comprises at least one of a polyester film, a polyamide film and a polyolefin film, preferably comprises at least one of a stretched polyester film, a stretched polyamide film and a stretched polyolefin film, more preferably comprises at least one of a stretched polyethylene terephthalate film, a stretched polybutylene terephthalate film, a stretched nylon film and a stretched polypropylene film, and further preferably comprises at least one of a biaxially stretched polyethylene terephthalate film, a biaxially stretched polybutylene terephthalate film, a biaxially stretched nylon film and a biaxially stretched polypropylene film.
[0097] The substrate layer 1 may be a single layer or may be composed of two or more layers. When the substrate layer 1 is composed of two or more layers, the substrate layer 1 may be a laminated body formed by laminating resin films with an adhesive or the like, or a laminated body formed by co-extruding resins to form two or more layers of resin films. In addition, a laminated body formed by co-extruding resins to form two or more layers of resin films may be used directly as the substrate layer 1 in an unstretched state, or may be formed by uniaxial stretching or biaxial stretching. When the substrate layer 1 is a single layer, the substrate layer 1 is preferably composed of a single layer of a polyester resin.
[0098] In the substrate layer 1, as specific examples of a laminate of two or more layers of resin films, there can be cited a laminate of a polyester film and a nylon film, a laminate of two or more layers of nylon films, a laminate of two or more layers of polyester films, etc., preferably a laminate of a stretched nylon film and a stretched polyester film, a laminate of two or more layers of stretched nylon films, and a laminate of two or more layers of stretched polyester films. For example, when the substrate layer 1 is a laminate of two layers of resin films, preferably a laminate of a polyester resin film and a polyester resin film, a laminate of a polyamide resin film and a polyamide resin film, or a laminate of a polyester resin film and a polyamide resin film, more preferably a laminate of a polyethylene terephthalate film and a polyethylene terephthalate film, a laminate of a nylon film and a nylon film, or a laminate of a polyethylene terephthalate film and a nylon film.
[0099] In the case where the substrate layer 1 is a laminate of two or more layers of resin films, the two or more layers of resin films can be laminated via an adhesive. As for the preferred adhesive, the same substances as the adhesives exemplified in the adhesive layer 2 described later can be cited. In addition, there is no particular limitation on the method of laminating more than two layers of resin films, and a known method can be adopted, for example, dry lamination, sandwich lamination, extrusion lamination, thermal lamination, etc., preferably dry lamination. In the case of lamination by dry lamination, a polyurethane adhesive is preferably used as the adhesive. At this time, as the thickness of the adhesive, for example, about 2 to 5 μm can be cited. In addition, an anchor coating can also be formed and laminated on the resin film. The anchor coating can be a layer similar to the adhesive exemplified in the adhesive layer 2 described later. At this time, as the thickness of the anchor coating, for example, about 0.01 to 1.0 μm can be cited.
[0100] In addition, additives such as lubricants, flame retardants, antiblocking agents, antioxidants, light stabilizers, tackifiers, and antistatic agents may be present on at least one of the surface and the interior of the base layer 1. The additives may be used alone or in combination of two or more.
[0101] In the present invention, from the viewpoint of improving the formability of the outer packaging material 10, it is preferred that a lubricant is present on the surface of the substrate layer 1. As a lubricant, there is no particular limitation, and preferably an amide lubricant is cited. As a specific example of an amide lubricant, for example, saturated fatty acid amide, unsaturated fatty acid amide, substituted amide, hydroxymethyl amide, saturated fatty acid bisamide, unsaturated fatty acid bisamide, fatty acid ester amide, aromatic bisamide, etc. can be cited. As a specific example of saturated fatty acid amide, lauric acid amide, palmitic acid amide, stearic acid amide, behenic acid amide, hydroxystearic acid amide, etc. can be cited. As a specific example of unsaturated fatty acid amide, oleic acid amide, erucic acid amide, etc. can be cited. As a specific example of substituted amide, N-oleyl palmitic acid amide, N-stearyl stearic acid amide, N-stearyl oleic acid amide, N-oleyl stearic acid amide, N-stearyl erucic acid amide, etc. can be cited. In addition, as a specific example of hydroxymethyl amide, hydroxymethyl stearic acid amide, etc. can be cited. Specific examples of saturated fatty acid bisamides include methylene bisstearic acid amide, ethylene biscapric acid amide, ethylene bislauric acid amide, ethylene bisstearic acid amide, ethylene bishydroxystearic acid amide, ethylene bisbehenic acid amide, hexamethylene bisstearic acid amide, hexamethylene bisbehenic acid amide, hexamethylene hydroxystearic acid amide, N,N'-distearyl adipamide, N,N'-distearyl sebacic acid amide, etc. Specific examples of unsaturated fatty acid bisamides include ethylene bisoleic acid amide, ethylene biserucic acid amide, hexamethylene bisoleic acid amide, N,N'-dioleyl adipamide, N,N'-dioleyl sebacic acid amide, etc. Specific examples of fatty acid ester amides include stearic acid stearamidoethyl ester, etc. Specific examples of the aromatic bisamide include meta-xylylene bisstearic acid amide, meta-xylylene bishydroxystearic acid amide, N,N′-distearylisophthalic acid amide, etc. The lubricant may be used alone or in combination of two or more.
[0102] When a lubricant is present on the surface of the base material layer 1, the amount of the lubricant is not particularly limited, but preferably about 3 mg / m 2 More preferably 4 to 15 mg / m 2 About 5 to 14 mg / m 2 about.
[0103] The lubricant present on the surface of the base layer 1 may be a lubricant seeping out from the resin constituting the base layer 1 , or may be a lubricant applied on the surface of the base layer 1 .
[0104] The thickness of the substrate layer 1 is not particularly limited as long as it can function as a substrate, and can be, for example, about 3 to 50 μm, preferably about 10 to 35 μm. When the substrate layer 1 is a laminate of two or more layers of resin films, the thickness of the resin films constituting each layer is preferably about 2 to 25 μm.
[0105] [Adhesive layer 2]
[0106] In the outer packaging material 10, the adhesive layer 2 is a layer provided between the substrate layer 1 and the barrier layer 3 as necessary for the purpose of improving the adhesion between them (when there is a barrier layer protective film 3b, the adhesion between the substrate layer 1 and the barrier layer protective film 3b).
[0107] The adhesive layer 2 is formed of an adhesive capable of bonding the substrate layer 1 to the barrier layer 3 (or the barrier layer protective film 3b). The adhesive used to form the adhesive layer 2 is not limited, and may be any of a chemical reaction type, a solvent evaporation type, a hot melt type, a hot pressing type, and the like. In addition, it may be a two-component curing adhesive (two-component adhesive), a single-component curing adhesive (single-component adhesive), or a resin that is not accompanied by a curing reaction. In addition, the adhesive layer 2 may be a single layer or a multilayer.
[0108] As the adhesive component contained in the adhesive, specifically, polyesters such as polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polybutylene naphthalate, polyethylene isophthalate, and copolyesters can be listed; polyethers; polyurethanes; epoxy resins; phenolic resins; polyamides such as nylon 6, nylon 66, nylon 12, and copolyamides; polyolefin resins such as polyolefins, cyclic polyolefins, acid-modified polyolefins, and acid-modified cyclic polyolefins; polyvinyl acetate; cellulose; (meth) acrylic resins; polyimides; polycarbonates; amino resins such as urea resins and melamine resins; rubbers such as chloroprene rubber, nitrile rubber, and styrene-butadiene rubber; silicone resins, etc. These adhesive components can be used alone or in combination of two or more. Among these adhesive components, polyurethane adhesives are preferably listed. In addition, the resins that become these adhesive components can be used in combination with appropriate curing agents to improve the bonding strength. The curing agent is appropriately selected from polyisocyanates, polyfunctional epoxy resins, oxazoline group-containing polymers, polyamine resins, acid anhydrides, and the like, depending on the functional groups of the adhesive component.
[0109] As the polyurethane adhesive, for example, there can be mentioned a polyurethane adhesive comprising a main agent containing a polyol compound and a curing agent containing an isocyanate compound. Preferably, there is mentioned a two-component curing type polyurethane adhesive using a polyol such as polyester polyol, polyether polyol and acrylic polyol as a main agent and an aromatic or aliphatic polyisocyanate as a curing agent. In addition, as the polyol compound, it is preferable to use a polyester polyol having a hydroxyl group in the side chain in addition to the hydroxyl group at the end of the repeating unit.
[0110] In addition, the adhesive layer 2 allows the addition of other components as long as it does not hinder adhesion, and can contain a colorant or a thermoplastic elastomer, a tackifier, a filler, etc. By including a colorant in the adhesive layer 2, the outer packaging material 10 can be colored. As the colorant, known colorants such as pigments and dyes can be used. In addition, the colorant can be used only one kind, or two or more kinds can be mixed and used.
[0111] The type of pigment is not particularly limited as long as it does not impair the adhesiveness of the adhesive layer 2. Examples of organic pigments include azo pigments, phthalocyanine pigments, quinacridone pigments, anthraquinone pigments, dioxazine pigments, indigo thioindigo pigments, perindolyl pigments, isoindoline pigments, and benzimidazolone pigments. Examples of inorganic pigments include carbon black pigments, titanium oxide pigments, cadmium pigments, lead pigments, chromium oxide pigments, and iron pigments. In addition, examples of fine powder of mica and fish scale foil pigments include the like.
[0112] Among the colorants, carbon black is preferred in order to make the outer packaging material 10 appear black, for example.
[0113] The average particle size of the pigment is not particularly limited, and may be, for example, about 0.05 to 5 μm, preferably about 0.08 to 2 μm. The average particle size of the pigment is a median particle size measured by a laser diffraction / scattering particle size distribution measuring device.
[0114] The content of the pigment in the adhesive layer 2 is not particularly limited as long as the packaging material 10 is colored, and is, for example, about 5 to 60% by mass, preferably 10 to 40% by mass.
[0115] The thickness of the adhesive layer 2 is not particularly limited as long as the substrate layer 1 and the barrier layer 3 can be bonded together. For example, the thickness may be about 1 μm or more and about 2 μm or more. In addition, the thickness may be about 10 μm or less and about 5 μm or less. The preferred range may be about 1 to 10 μm, about 1 to 5 μm, about 2 to 10 μm, and about 2 to 5 μm.
[0116] [Coloring Layer]
[0117] The colored layer is a layer (not shown) provided between the substrate layer 1 and the barrier layer 3 (or barrier layer protective film 3b) as required. In the case of having an adhesive layer 2, a colored layer may be provided between the substrate layer 1 and the adhesive layer 2, or between the adhesive layer 2 and the barrier layer 3 (or barrier layer protective film 3b). In addition, a colored layer may be provided outside the substrate layer 1. By providing a colored layer, the outer packaging material 10 can be colored.
[0118] The coloring layer can be formed, for example, by applying ink containing a colorant to the surface of the base layer 1 or the surface of the barrier layer 3 (in the case of a barrier layer protective film 3b, the surface of the barrier layer protective film 3b). As the colorant, a known colorant such as a pigment or a dye can be used. In addition, a single colorant may be used, or two or more colorants may be mixed and used.
[0119] Specific examples of the colorant contained in the colored layer include the same colorants as exemplified in the section [Adhesive layer 2].
[0120] [Barrier layer 3]
[0121] In the outer packaging material 10 , the barrier layer 3 is a layer that at least suppresses the intrusion of moisture.
[0122] As the barrier layer 3, for example, metal foil, vapor-deposited film, resin layer, etc. having barrier properties can be listed. As the vapor-deposited film, metal vapor-deposited film, inorganic oxide vapor-deposited film, carbon-containing inorganic oxide vapor-deposited film, etc. can be listed. As the resin layer, polyvinylidene chloride, polymers with chlorotrifluoroethylene (CTFE) as the main component, polymers with tetrafluoroethylene (TFE) as the main component, polymers with fluoroalkyl groups, and polymers with fluoroalkyl units as the main component, etc., fluororesins, ethylene-vinyl alcohol copolymers, etc. can be listed. In addition, as the barrier layer 3, resin films provided with at least one layer of these vapor-deposited films and resin layers can also be listed. The barrier layer 3 can be provided with multiple layers. The barrier layer 3 preferably includes a layer composed of a metal material. As the metal material constituting the barrier layer 3, specifically aluminum alloy, stainless steel, titanium steel, steel plate, etc. can be listed. When used in the form of metal foil, it preferably includes at least one of aluminum alloy foil and stainless steel foil.
[0123] From the viewpoint of improving the formability of the outer packaging material 10, the aluminum alloy foil is preferably a soft aluminum alloy foil composed of an annealed aluminum alloy, etc., and from the viewpoint of further improving the formability, an aluminum alloy foil containing iron is preferred. In the aluminum alloy foil containing iron (100% by mass), the content of iron is preferably 0.1 to 9.0% by mass, and more preferably 0.5 to 2.0% by mass. When the content of iron is 0.1% by mass or more, an outer packaging material with better formability can be obtained. When the content of iron is 9.0% by mass or less, an outer packaging material with better flexibility can be obtained. As a soft aluminum alloy foil, for example, an aluminum alloy foil having a composition specified in JIS H4160: 1994A8021H-O, JIS H4160: 1994A8079H-O, JIS H4000: 2014A8021P-O, or JIS H4000: 2014A8079P-O can be cited. In addition, silicon, magnesium, copper, manganese, etc. may be added as needed. Softening may be performed by annealing treatment or the like.
[0124] In addition, examples of stainless steel foil include austenitic, ferritic, austenitic-ferritic, martensitic, and precipitation hardened stainless steel foils. In order to provide an outer packaging material 10 having excellent formability, the stainless steel foil is preferably made of austenitic stainless steel.
[0125] Specific examples of the austenitic stainless steel constituting the stainless steel foil include SUS304, SUS301, and SUS316L. Among them, SUS304 is particularly preferred.
[0126] Regarding the thickness of the barrier layer 3, in the case of a metal foil, as long as it can function as a barrier layer that at least inhibits the intrusion of water, for example, about 9 to 200 μm can be cited. The thickness of the barrier layer 3 is preferably about 85 μm or less, more preferably about 50 μm or less, further preferably about 40 μm or less, and particularly preferably about 35 μm or less. In addition, it is preferably about 10 μm or more, further preferably about 20 μm or more, and more preferably about 25 μm or more. As a preferred range of the thickness, about 10 to 85 μm, about 10 to 50 μm, about 10 to 40 μm, about 10 to 35 μm, about 20 to 85 μm, about 20 to 50 μm, about 20 to 40 μm, about 20 to 35 μm, about 25 to 85 μm, about 25 to 50 μm, about 25 to 40 μm, and about 25 to 35 μm. When the barrier layer 3 is composed of an aluminum alloy foil, the above range is particularly preferred, and about 25 to 85 μm and about 25 to 50 μm are particularly preferred. In addition, in particular, when the barrier layer 3 is composed of a stainless steel foil, the thickness of the stainless steel foil is preferably about 60 μm or less, more preferably about 50 μm or less, further preferably about 40 μm or less, further preferably about 30 μm or less, and particularly preferably about 25 μm or less. In addition, about 10 μm or more is preferably cited, and about 15 μm or more is more preferably cited. As a preferred range of thickness, about 10 to 60 μm, about 10 to 50 μm, about 10 to 40 μm, about 10 to 30 μm, about 10 to 25 μm, about 15 to 60 μm, about 15 to 50 μm, about 15 to 40 μm, about 15 to 30 μm, and about 15 to 25 μm can be cited.
[0127] [Barrier layer protective films 3a, 3b]
[0128] In the outer packaging material 10, the barrier layer protective film 3a is provided on the surface of the barrier layer 3 on the side of the heat-fusible resin layer 4. In the outer packaging material 10, the barrier layer protective film 3a may be provided only on the surface of the barrier layer 3 on the side of the heat-fusible resin layer 4, or the barrier layer protective films 3a and 3b may be provided on both surfaces of the barrier layer 3, respectively.
[0129] In the outer packaging material 10 of the present invention, when the barrier layer protective film 3a is analyzed using time-of-flight secondary ion mass spectrometry, the PO3 - The peak intensity P PO3 Relative to CrPO4 - The peak intensity P CrPO4 Ratio P PO3 / CrPO4 It is preferably in the range of 6 to 120.
[0130] As described above, in an all-solid-state battery, in order to suppress the peeling between the solid electrolyte and the negative electrode active material layer or the positive electrode active material layer, it is expected that the all-solid-state battery can be continuously restrained by high pressure pressing from the outside of the outer packaging material even when in use. However, when the solid electrolyte and the negative electrode active material layer or the positive electrode active material layer are continuously restrained in a high pressure state from the outside of the outer packaging material of the all-solid-state battery, the heat-fusible resin layer of the outer packaging material is pressed forcefully toward the battery element, and the thickness of the heat-fusible resin layer (inner layer) of the outer packaging material becomes thinner, which may cause the barrier layer laminated by the outer packaging material to contact the solid electrolyte. In particular, when the barrier layer of the outer packaging material is in contact with the solid electrolyte containing the sulfide solid electrolyte material, when electricity is passed between them, an alloy is generated on the surface of the barrier layer, and there is a problem of barrier layer degradation. In contrast, in the outer packaging material 10 of the present invention, by providing a barrier layer protective film 3a on the surface of the barrier layer 3 of the outer packaging material 10, the all-solid-state battery 70 is restrained in a high-voltage state, thereby, even when electricity is passed between the barrier layer 3 and the solid electrolyte layer 40 in a state where the solid electrolyte containing the sulfide solid electrolyte material penetrates the heat-fusible resin layer 4 and the adhesive layer 5, etc., it is not easy to form an alloy on the surface of the barrier layer 3, and the degradation of the barrier layer 3 is effectively suppressed. In particular, the peak intensity of the barrier layer protective film 3a is higher than P PO3 / CrPO4 When the ratio is within the range of 6 to 120, the generation of alloys on the surface of the barrier layer 3 can be more effectively suppressed, and the degradation of the barrier layer 3 can be more effectively suppressed.
[0131] In the present invention, as derived from PO3 - The peak intensity P PO3 Relative to CrPO4 - The peak intensity P CrPO4 Ratio P PO3 / CrPO4 The lower limit is preferably about 10 or more, the upper limit is preferably about 115 or less, more preferably about 110 or less, and further preferably about 50 or less. PO3 / CrPO4 The preferred range of may be about 6 to 120, about 6 to 115, about 6 to 110, about 6 to 50, about 10 to 120, about 10 to 115, about 10 to 110, about 10 to 50, among which about 10 to 50 is more preferred, and about 25 to 30 is further particularly preferred.
[0132] In addition, in the present invention, when the barrier layer protective film 3a is analyzed using time-of-flight secondary ion mass spectrometry, the PO2 - The peak intensity P PO2 Relative to CrPO4 - The peak intensity P CrPO4 Ratio P PO2 / CrPO4 It is preferably in the range of 7-70.
[0133] From PO2 - The peak intensity P PO2 Relative to CrPO4 - The peak intensity P CrPO4 Ratio P PO2 / CrPO4 It is preferably in the range of 7 to 70. From the viewpoint of more effectively suppressing the degradation of the barrier layer 3, the ratio P PO2 / CrPO4 The lower limit is preferably about 10 or more, the upper limit is preferably about 65 or less, and more preferably about 50 or less. PO2 / CrPO4 The preferred range of may be about 7 to 70, about 7 to 65, about 7 to 50, about 10 to 70, about 10 to 65, about 10 to 50, among which about 10 to 50 is more preferred, and about 15 to 20 is further particularly preferred.
[0134] In the present invention, when barrier layer 3 has barrier layer protective films 3a and 3b on both sides, it is preferred that the peak intensity ratio P of either barrier layer protective films 3a and 3b is PO3 / CrPO4 Within the above range, and for P PO2 / CrPO4 It is also preferably within the above range.
[0135] The method of analyzing the barrier layer protection films 3 a and 3 b using time-of-flight secondary ion mass spectrometry can be specifically performed using a time-of-flight secondary ion mass spectrometer under the following measurement conditions.
[0136] (Measurement conditions)
[0137] Primary ions: Doubly charged ions of bismuth cluster (Bi3 ++ )
[0138] Primary ion acceleration voltage: 30kV
[0139] Mass range (m / z): 0~1500
[0140] Measuring range: 100μm×100μm
[0141] Scan number: 16 scan / cycle
[0142] Number of pixels (1 side): 256 pixels
[0143] Etching ions: Ar gas cluster ion beam (Ar-GCIB)
[0144] Etching ion acceleration voltage: 5.0kV
[0145] In addition, the presence of chromium in the barrier layer protective film can be confirmed using X-ray photoelectron spectroscopy. Specifically, first, in the outer packaging material, the layers (adhesive layer, hot-melt resin layer, adhesive layer, etc.) laminated on the barrier layer are physically peeled off. Next, the barrier layer is placed in an electric furnace and the organic components present on the surface of the barrier layer are removed at about 300°C for about 30 minutes. Then, using X-ray photoelectron spectroscopy of the surface of the barrier layer, it is confirmed that chromium is contained.
[0146] The barrier layer protection films 3 a and 3 b can be formed by subjecting the surface of the barrier layer 3 to a chemical conversion treatment using a treatment solution containing a chromium compound such as chromium oxide.
[0147] As a chemical conversion treatment using a treatment solution containing a chromium compound, for example, the following method can be cited: a treatment solution in which a chromium compound such as chromium oxide is dispersed in phosphoric acid and / or its salt is applied to the surface of the barrier layer 3, and a sintering treatment is performed, thereby forming a barrier layer protective film on the surface of the barrier layer 3.
[0148] The peak intensity ratio P of barrier layer protective films 3a and 3b PO3 / CrPO4 And the above peak intensity ratio P PO2 / CrPO4 The barrier layer protective films 3a and 3b can be adjusted by, for example, the composition of the treatment solution for forming the barrier layer protective films 3a and 3b, the temperature and time of the sintering treatment after the treatment, and other production conditions.
[0149] The ratio of the chromium compound to phosphoric acid and / or its salt in the treatment solution containing the chromium compound is not particularly limited. PO3 / CrPO4 And the above peak intensity ratio P PO2 / CrPO4 From the viewpoint of setting the above ranges, the ratio of phosphoric acid and / or its salt to 100 parts by mass of the chromium compound is preferably about 30 to 120 parts by mass, more preferably about 40 to 110 parts by mass. As phosphoric acid and its salt, for example, condensed phosphoric acid and its salt may be used.
[0150] In addition, the treatment solution containing the chromium compound may further contain an anionic polymer and a crosslinking agent for crosslinking the anionic polymer. As the anionic polymer, poly(meth)acrylic acid or its salt, a copolymer with (meth)acrylic acid or its salt as the main component, etc. may be cited. In addition, as the crosslinking agent, a compound having any functional group among isocyanate group, glycidyl group, carboxyl group, oxazoline group, or a silane coupling agent may be cited. The anionic polymer and the crosslinking agent may be one kind, or two or more kinds, respectively.
[0151] In addition, from the viewpoint of effectively suppressing the degradation of the barrier layer 3, the treatment liquid containing the chromium compound preferably contains an aminophenol polymer. In the treatment liquid containing the chromium compound, the content of the aminophenol polymer is preferably about 100 to 400 parts by mass, and more preferably about 200 to 300 parts by mass, relative to 100 parts by mass of the chromium compound. In addition, the weight average molecular weight of the aminophenol polymer is preferably about 5000 to 20000. The weight average molecular weight of the aminophenol polymer is a value measured by gel permeation chromatography (GPC) under the condition of using polystyrene as a standard sample.
[0152] The solvent of the treatment liquid containing a chromium compound is not particularly limited as long as it is a solvent that can disperse the components contained in the treatment liquid and evaporate by subsequent heating, but water is preferred.
[0153] The solid content concentration of the chromium compound contained in the treatment solution for forming the barrier layer protective films 3a and 3b is not particularly limited, and can be obtained by adjusting the peak intensity ratio P PO3 / CrPO4 And the above peak intensity ratio P PO2 / CrPO4 From the viewpoint of effectively suppressing the degradation of the barrier layer 3 by setting the above-mentioned predetermined ranges, for example, about 1 to 15 mass %, preferably about 7.0 to 12.0 mass %, more preferably about 8.0 to 11.0 mass %, and further preferably about 9.0 to 10.0 mass % can be cited.
[0154] The thickness of the barrier layer protective films 3a and 3b is not particularly limited, but is preferably about 1 nm to 10 μm, more preferably about 1 to 100 nm, and further preferably about 1 to 50 nm from the viewpoint of effectively suppressing the degradation of the barrier layer 3. The thickness of the barrier layer protective film can be measured by observation using a transmission electron microscope, or by a combination of observation using a transmission electron microscope and energy dispersive X-ray spectroscopy or electron beam energy loss spectroscopy.
[0155] From the same point of view, as the barrier layer 3, every 1m 2 The amount of the barrier layer protective films 3a and 3b on the surface is preferably about 1 to 500 mg, more preferably about 1 to 100 mg, and further preferably about 1 to 50 mg.
[0156] Examples of a method for applying the treatment liquid containing a chromium compound to the surface of the barrier layer include a bar coating method, a roll coating method, a gravure coating method, and a dipping method.
[0157] From the above peak intensity ratio P PO3 / CrPO4 And the above peak intensity ratio P PO2 / CrPO4From the viewpoint of effectively suppressing the degradation of the barrier layer 3 by setting the above-specified ranges, the heating temperature when the barrier layer protective film is prepared as the sintering treatment liquid is preferably about 170 to 250° C., more preferably about 180 to 230° C., and further preferably about 190 to 220° C. From the same viewpoint, the sintering time is preferably about 2 to 10 seconds, and more preferably about 3 to 6 seconds.
[0158] From the viewpoint of more effectively performing the chemical conversion treatment on the surface of the barrier layer 3, it is preferred to perform a degreasing treatment by a known treatment method such as an alkali immersion method, an electrolytic cleaning method, an acid cleaning method, an electrolytic acid cleaning method, or an acid activation method before setting the barrier layer protective films 3a and 3b on the surface of the barrier layer 3.
[0159] [Thermal Fusible Resin Layer 4]
[0160] In the all-solid battery outer packaging material 10 of the present invention, the heat-fusible resin layer 4 corresponds to the innermost layer and is a layer (sealing layer) that performs the function of sealing the battery element by heat-fusion bonding the heat-fusible resin layers 4 when assembling the all-solid battery.
[0161] In the all-solid-state battery outer packaging material 10 of the present invention, the hydrogen sulfide permeation rate of the resin constituting the heat-fusible resin layer 4 is 1.0×10 -8 cc mm / cm 2 ·sec·cmHg or more The hydrogen sulfide permeation rate of the resin constituting the thermally adhesive resin layer 4 can be specifically measured by the method described in Examples.
[0162] The hydrogen sulfide permeation rate of the resin constituting the heat-adhesive resin layer 4 is preferably about 1.2×10 -8 cc mm / cm 2 ·sec·cmHg or more. The upper limit of the hydrogen sulfide permeation amount can be, for example, about 1.0×10 -6 cc mm / cm 2 ·sec·cmHg, etc.
[0163] In addition, as the heat-fusible resin layer 4, each 1m 2 The water vapor transmission rate is preferably about 10.0 g / m 2 / 24h or less, more preferably about 8.0g / m 2 / 24h or less. The lower limit of the total water vapor transmission rate can be, for example, about 5.0 g / m 2 / 24h, about 1.0g / m 2 / 24h, about 0.1g / m 2 / 24h, etc. The method for measuring the water vapor transmission rate is as follows.
[0164] <Every 1m 2 Determination of water vapor transmission rate
[0165] The thickness of each m2 of the heat-fusible resin layer 4 was measured by the following method. 2 Water vapor transmission rate (single-sided area) (g / m 2 / 24h). The water vapor transmission rate was measured using an isobaric method based on the method specified in ISO15106-5 2008, at a temperature of 40°C, a relative humidity of 90%, a measurement period of 24 hours, and a measurement area of 8cmφ. 2 The water vapor transmission rate is converted into m by the ISO water vapor transmission rate measurement method. 2 The numerical value of .
[0166] The hydrogen sulfide permeation rate is 1.0×10 -8 cc mm / cm 2 ·sec·cmHg or more, preferably a resin containing a polyolefin skeleton such as a polyolefin or an acid-modified polyolefin. The resin constituting the heat-fusible resin layer 4 containing a polyolefin skeleton can be analyzed by, for example, infrared spectroscopy, gas chromatography-mass spectrometry, etc. In addition, when analyzing the resin constituting the heat-fusible resin layer 4 by infrared spectroscopy, it is preferred to detect a peak derived from maleic anhydride. For example, when measuring maleic anhydride-modified polyolefin by infrared spectroscopy, the peak at wave number 1760cm -1 Nearby and wave number 1780cm -1 In the case where the heat-fusible resin layer 4 is a layer composed of maleic anhydride-modified polyolefin, when measured by infrared spectroscopy, a peak derived from maleic anhydride is detected. However, when the acid modification degree is low, the peak becomes smaller and sometimes cannot be detected. In this case, it is possible to analyze by nuclear magnetic resonance spectroscopy.
[0167] As polyolefins, specifically, polyethylenes such as low-density polyethylene, medium-density polyethylene, high-density polyethylene, and linear low-density polyethylene can be listed; ethylene-α-olefin copolymers; polypropylenes such as homopolymer polypropylene, block copolymers of polypropylene (e.g., block copolymers of propylene and ethylene), and random copolymers of polypropylene (e.g., random copolymers of propylene and ethylene); propylene-α-olefin copolymers; terpolymers of ethylene-butene-propylene, etc. Among them, polypropylene is preferred. The polyolefin resin in the case of a copolymer can be a block copolymer or a random copolymer. These polyolefin resins can be used alone or in combination of two or more.
[0168] In addition, the polyolefin may also be a cyclic polyolefin. Cyclic polyolefin is a copolymer of an olefin and a cyclic monomer. As the olefin constituting the above-mentioned cyclic polyolefin, for example, ethylene, propylene, 4-methyl-1-pentene, styrene, butadiene, isoprene, etc. can be cited. In addition, as the cyclic monomer constituting the cyclic polyolefin, for example, cyclic olefins such as norbornene, cyclic dienes such as cyclopentadiene, dicyclopentadiene, cyclohexadiene, and norbornene can be cited. Among them, cyclic olefins are preferably cited, and norbornene is further preferred.
[0169] Acid-modified polyolefin refers to a polymer modified by block polymerization or graft polymerization of polyolefin using an acid component. As the acid-modified polyolefin, the above-mentioned polyolefin, or a copolymer obtained by copolymerizing the above-mentioned polyolefin with a polar molecule such as acrylic acid or methacrylic acid, or a polymer such as a cross-linked polyolefin can also be used. In addition, as the acid component used for acid modification, for example, carboxylic acids or anhydrides thereof such as maleic acid, acrylic acid, itaconic acid, crotonic acid, maleic anhydride, and itaconic anhydride can be cited.
[0170] The acid-modified polyolefin may be an acid-modified cyclic polyolefin. The so-called acid-modified cyclic polyolefin refers to a polymer obtained by replacing a part of the monomers constituting the cyclic polyolefin with an acid component for copolymerization, or by block polymerization or graft polymerization of the acid component and the cyclic polyolefin. The acid-modified cyclic polyolefin is the same as described above. In addition, the acid component used for acid modification is the same as the acid component used for modification of the above-mentioned polyolefin.
[0171] Preferred examples of the acid-modified polyolefin include polyolefin modified with carboxylic acid or its anhydride, polypropylene modified with carboxylic acid or its anhydride, maleic anhydride-modified polyolefin, and maleic anhydride-modified polypropylene.
[0172] The heat-adhesive resin layer 4 may be formed of a single resin or a blended polymer of two or more resins. Furthermore, the heat-adhesive resin layer 4 may be formed of only one layer or two or more layers of the same or different resins.
[0173] In addition, the heat-fusible resin layer 4 may further contain a lubricant or the like as required. When the heat-fusible resin layer 4 contains a lubricant, the moldability of the outer packaging material 10 can be improved. There is no particular limitation on the lubricant, and a known lubricant can be used. One lubricant may be used alone, or two or more lubricants may be used in combination.
[0174] The lubricant is not particularly limited, but preferably an amide lubricant is used. Specific examples of the lubricant include the lubricants exemplified for the base material layer 1. The lubricant may be used alone or in combination of two or more.
[0175] When a lubricant is present on the surface of the heat-fusible resin layer 4, the amount of lubricant present is not particularly limited, but from the viewpoint of improving the moldability of the electronic packaging material, 10 to 50 mg / m 2 About 15 to 40 mg / m 2 about.
[0176] The lubricant present on the surface of the thermally adhesive resin layer 4 may be a lubricant seeping out from the resin constituting the thermally adhesive resin layer 4 , or may be a lubricant applied on the surface of the thermally adhesive resin layer 4 .
[0177] In addition, as for the thickness of the heat-fusible resin layer 4, there is no particular limitation as long as the heat-fusible resin layers are heat-fused to each other to perform the function of sealing the battery element. From the viewpoint of appropriately discharging hydrogen sulfide to the outside, it is preferably 10 μm or more, more preferably 20 μm or more, and further preferably 30 μm or more. In addition, the thickness of the heat-fusible resin layer 4 is, for example, about 100 μm or less, preferably about 85 μm or less, and more preferably about 60 μm or less. As a preferred range, about 10 to 100 μm, about 10 to 85 μm, about 10 to 60 μm, about 20 to 100 μm, about 20 to 85 μm, about 20 to 60 μm, about 30 to 100 μm, about 30 to 85 μm, and about 30 to 60 μm can be listed.
[0178] [Adhesive layer 5]
[0179] In the outer packaging material 10 , the adhesive layer 5 is a layer provided between the barrier layer protective film 3 a and the heat-fusible resin layer 4 as necessary in order to firmly adhere them.
[0180] The adhesive layer 5 is formed of a resin that can bond the barrier layer protective film 3a to the thermally fusible resin layer 4. As the resin used to form the adhesive layer 5, for example, the same adhesive as exemplified in the adhesive layer 2 can be used. Among them, the resin used to form the adhesive layer 5 preferably contains a polyolefin skeleton, and the polyolefins and acid-modified polyolefins exemplified in the above-mentioned thermally fusible resin layer 4 can be listed. The resin constituting the adhesive layer 5 contains a polyolefin skeleton, which can be analyzed by, for example, infrared spectroscopy, gas chromatography-mass spectrometry, etc., and the analysis method is not particularly limited. In addition, when analyzing the resin constituting the adhesive layer 5 by infrared spectroscopy, it is preferred to detect a peak derived from maleic anhydride. For example, when measuring maleic anhydride-modified polyolefin by infrared spectroscopy, at a wave number of 1760cm -1 Nearby and wave number 1780cm -1 A peak derived from maleic anhydride is detected near 1.5 Å. However, when the degree of acid modification is low, the peak becomes smaller and sometimes cannot be detected. In this case, analysis can be performed using nuclear magnetic resonance spectroscopy.
[0181] The adhesive layer 5 preferably contains an acid-modified polyolefin from the viewpoint of firmly bonding the barrier layer protective film 3a and the heat-fusible resin layer 4. As the acid-modified polyolefin, polyolefin modified with carboxylic acid or its anhydride, polypropylene modified with carboxylic acid or its anhydride, maleic anhydride-modified polyolefin, and maleic anhydride-modified polypropylene are particularly preferred.
[0182] In addition, from the viewpoint of making the outer packaging material 10 thinner and having excellent shape stability after molding, the adhesive layer 5 is more preferably a cured product of a resin composition containing an acid-modified polyolefin and a curing agent. Preferred examples of the acid-modified polyolefin include those listed above.
[0183] In addition, the adhesive layer 5 is preferably a cured product of a resin composition comprising at least one of an acid-modified polyolefin and a compound selected from a compound with an isocyanate group, a compound with an oxazoline group and a compound with an epoxy group, and is particularly preferably a cured product of a resin composition comprising at least one of an acid-modified polyolefin and a compound selected from a compound with an isocyanate group and a compound with an epoxy group. In addition, the adhesive layer 5 preferably comprises at least one selected from polyurethane, polyester and epoxy resin, and more preferably comprises polyurethane and epoxy resin. As polyester, for example, amide ester resin is preferably used. Amidoester resin is usually generated by the reaction of carboxyl and oxazoline groups. The adhesive layer 5 is more preferably a cured product of a resin composition comprising at least one of these resins and the above-mentioned acid-modified polyolefin. Wherein, in the case of unreacted products of curing agents such as compounds with isocyanate groups, compounds with oxazoline groups, and epoxy resins remaining in the adhesive layer 5, the presence of unreacted products can be confirmed, for example, by a method selected from infrared spectroscopy, Raman spectroscopy, time-of-flight secondary ion mass spectrometry (TOF-SIMS), etc.
[0184] In addition, from the viewpoint of further improving the adhesion between the barrier layer protective film 3a and the adhesive layer 5, the adhesive layer 5 is preferably a cured product of a resin composition containing a curing agent, and the curing agent has at least one selected from an oxygen atom, a heterocyclic ring, a C=N bond, and a C-O-C bond. As a curing agent having a heterocyclic ring, for example, a curing agent having an oxazoline group, a curing agent having an epoxy group, etc. can be listed. In addition, as a curing agent having a C=N bond, a curing agent having an oxazoline group, a curing agent having an isocyanate group, etc. can be listed. In addition, as a curing agent having a C-O-C bond, a curing agent having an oxazoline group, a curing agent having an epoxy group, polyurethane, etc. can be listed. The adhesive layer 5 is a cured product of a resin composition containing these curing agents, for example, by gas chromatography-mass spectrometry (GCMS), infrared spectroscopy (IR), time-of-flight secondary ion mass spectrometry (TOF-SIMS), X-ray photoelectron spectroscopy (XPS), and other methods.
[0185] There are no particular restrictions on the compound having an isocyanate group. From the viewpoint of effectively improving the adhesion between the barrier layer protective film 3a and the adhesive layer 5, a polyfunctional isocyanate compound is preferably cited. The polyfunctional isocyanate compound is not particularly limited as long as it is a compound having two or more isocyanate groups. Specific examples of polyfunctional isocyanate curing agents include pentane diisocyanate (PDI), isophorone diisocyanate (IPDI), hexamethylene diisocyanate (HDI), toluene diisocyanate (TDI), diphenylmethane diisocyanate (MDI), substances obtained by polymerizing or ureating them, mixtures thereof, or copolymers with other polymers. In addition, adducts, biuret bodies, isocyanurate bodies, etc. can be cited.
[0186] The content of the compound having an isocyanate group in the adhesive layer 5 is preferably in the range of 0.1 to 50 mass %, more preferably in the range of 0.5 to 40 mass %, in the resin composition constituting the adhesive layer 5. This can effectively improve the adhesion between the barrier layer protective film 3a and the adhesive layer 5.
[0187] The compound with oxazoline is just not particularly limited as long as it is the compound with oxazoline skeleton.As the specific example of the compound with oxazoline, the compound with polystyrene main chain, the compound with acrylic acid main chain etc. can be enumerated.In addition, as commercially available product, for example, the EPOCROS series etc. that Nippon Catalyst Co., Ltd. produces can be enumerated.
[0188] The proportion of the compound having an oxazoline group in the adhesive layer 5 is preferably in the range of 0.1 to 50 mass %, more preferably in the range of 0.5 to 40 mass %, in the resin composition constituting the adhesive layer 5. This can effectively improve the adhesion between the barrier layer protective film 3a and the adhesive layer 5.
[0189] As a compound having an epoxy group, for example, an epoxy resin can be cited. As the epoxy resin, there is no particular limitation as long as it is a resin that can form a cross-linked structure using the epoxy group present in the molecule, and a known epoxy resin can be used. As the weight average molecular weight of the epoxy resin, preferably about 50 to 2000, more preferably about 100 to 1000, and further preferably about 200 to 800. Among them, in the first invention, the weight average molecular weight of the epoxy resin is a value measured by gel permeation chromatography (GPC) under the condition of using polystyrene as a standard sample.
[0190] Specific examples of epoxy resins include glycidyl ether derivatives of trimethylolpropane, bisphenol A diglycidyl ether, modified bisphenol A diglycidyl ether, novolac glycidyl ether, glycerol polyglycidyl ether, polyglycerol polyglycidyl ether, etc. The epoxy resins may be used alone or in combination of two or more.
[0191] The proportion of the epoxy resin in the adhesive layer 5 is preferably in the range of 0.1 to 50 mass %, more preferably in the range of 0.5 to 40 mass %, in the resin composition constituting the adhesive layer 5. This can effectively improve the adhesion between the barrier layer protective film 3a and the adhesive layer 5.
[0192] The polyurethane is not particularly limited, and known polyurethanes can be used. The adhesive layer 5 may be, for example, a cured product of a two-component curing type polyurethane.
[0193] The ratio of the polyurethane in the adhesive layer 5 is preferably in the range of 0.1 to 50% by mass, and more preferably in the range of 0.5 to 40% by mass, in the resin composition constituting the adhesive layer 5 .
[0194] Among them, when the adhesive layer 5 is a cured product of a resin composition comprising at least one selected from a compound having an isocyanate group, a compound having an oxazoline group and an epoxy resin, and the above-mentioned acid-modified polyolefin, the acid-modified polyolefin functions as a main agent, and the compound having an isocyanate group, the compound having an oxazoline group and the compound having an epoxy group function as a curing agent, respectively.
[0195] The thickness of the adhesive layer 5 is preferably about 50 μm or less, about 40 μm or less, about 30 μm or less, about 20 μm or less, or about 5 μm or less, and preferably about 0.1 μm or more, or about 0.5 μm or more. As the range of the thickness, preferably about 0.1 to 50 μm, about 0.1 to 40 μm, about 0.1 to 30 μm, about 0.1 to 20 μm, about 0.1 to 5 μm, about 0.5 to 50 μm, about 0.5 to 40 μm, about 0.5 to 30 μm, about 0.5 to 20 μm, or about 0.5 to 5 μm. More specifically, in the case of a cured product of the adhesive or acid-modified polyolefin and a curing agent exemplified in the adhesive layer 2, preferably about 1 to 10 μm, more preferably about 1 to 5 μm. In addition, when the resin exemplified in the heat-fusible resin layer 4 is used, the thickness is preferably about 2 to 50 μm, and more preferably about 10 to 40 μm. Among them, when the adhesive layer 5 is a cured product of a resin composition containing an adhesive or an acid-modified polyolefin and a curing agent exemplified in the adhesive layer 2, the adhesive layer 5 can be formed, for example, by applying the resin composition and curing it by heating. In addition, when the resin exemplified in the heat-fusible resin layer 4 is used, it can be formed, for example, by extrusion molding of the heat-fusible resin layer 4 and the adhesive layer 5.
[0196] [Surface coating layer 6]
[0197] In the outer packaging material 10, in order to improve at least one of the design, damage resistance, and formability, a surface covering layer 6 may be provided on the substrate layer 1 of the laminate (on the side of the substrate layer 1 opposite to the barrier layer 3) as needed. The surface covering layer 6 is a layer located on the outermost side of the outer packaging material 10 when the outer packaging material 10 is used to assemble an all-solid battery.
[0198] The surface coating layer 6 can be formed of a resin such as polyvinylidene chloride, polyester, polyurethane, acrylic resin, epoxy resin, etc.
[0199] When the resin forming the surface coating layer 6 is a curable resin, the resin may be either a single-liquid curable resin or a two-liquid curable resin, preferably a two-liquid curable resin. Examples of the two-liquid curable resin include two-liquid curable polyurethane, two-liquid curable polyester, and two-liquid curable epoxy resin. Among them, two-liquid curable polyurethane is preferred.
[0200] As two-component curable polyurethane, for example, polyurethane containing a main agent containing a polyol compound and a curing agent containing an isocyanate compound can be cited. Preferably, a two-component curable polyurethane containing a polyol such as polyester polyol, polyether polyol and acrylic polyol as a main agent and an aromatic or aliphatic polyisocyanate as a curing agent is cited. In addition, as a polyol compound, a polyester polyol having a hydroxyl group in a side chain in addition to a hydroxyl group at the end of a repeating unit is preferably used.
[0201] In the surface coating layer 6, according to the functionality that the surface coating layer 6 or its surface should have, the above-mentioned lubricant or anti-blocking agent, matting agent, flame retardant, antioxidant, tackifier, antistatic agent and other additives may be contained on at least one of the surface and the inside of the surface coating layer 6 as needed. As additives, for example, microparticles with an average particle size of about 0.5nm to 5μm can be cited. The average particle size of the additive is the median particle size measured by a laser diffraction / scattering particle size distribution measuring device.
[0202] The additive may be any of inorganic and organic substances. In addition, there is no particular limitation on the shape of the additive, and examples thereof include spherical, fibrous, plate-like, amorphous, and flaky shapes.
[0203] As the specific example of additive, talc, silicon dioxide, graphite, kaolin, montmorillonite, mica, hydrotalcite, silica gel, zeolite, aluminum hydroxide, magnesium hydroxide, zinc oxide, magnesium oxide, aluminum oxide, neodymium oxide, antimony oxide, titanium oxide, cerium oxide, calcium sulfate, barium sulfate, calcium carbonate, calcium silicate, lithium carbonate, calcium benzoate, calcium oxalate, magnesium stearate, aluminum oxide, carbon black, carbon nanotube, high melting point nylon, acrylate resin, cross-linked acrylic acid, cross-linked styrene, cross-linked polyethylene, benzoguanamine, gold, aluminum, copper, nickel, etc. can be listed. One kind of additive can be used alone, and two or more kinds can be used in combination. Among these additives, from the viewpoints of dispersion stability and cost, silicon dioxide, barium sulfate, titanium oxide are preferably listed. In addition, various surface treatments such as insulation treatment and high dispersibility treatment can also be implemented on the surface of the additive.
[0204] The method of forming the surface coating layer 6 is not particularly limited, and an example thereof includes a method of applying a resin for forming the surface coating layer 6. When an additive is added to the surface coating layer 6, the resin mixed with the additive may be applied.
[0205] The thickness of the surface coating layer 6 is not particularly limited as long as the above-mentioned function as the surface coating layer 6 can be exhibited, and for example, it can be about 0.5 to 10 μm, preferably about 1 to 5 μm.
[0206] Regarding the manufacturing method of the outer packaging material 10, there is no particular limitation as long as a laminated body formed by laminating the layers possessed by the outer packaging material 10 can be obtained, and a method including the steps of laminating at least a substrate layer 1, a barrier layer 3, a barrier layer protective film 3a formed on the surface of the barrier layer 3, and a thermally fusible resin layer 4 in sequence can be listed.
[0207] An example of a method for manufacturing the outer packaging material 10 is as follows. First, a laminated body (hereinafter sometimes referred to as "laminated body A") is formed by laminating a substrate layer 1, an adhesive layer 2, a barrier layer 3, and a barrier layer protective film 3a formed on the surface of the barrier layer 3 in sequence. The formation of the laminated body A can be specifically carried out by a dry lamination method. In the above-mentioned dry lamination method, an adhesive for forming the adhesive layer 2 is applied on the substrate layer 1 or on the barrier layer 3 formed with the barrier layer protective film 3a (and further formed with the barrier layer protective film 3b as required) by a coating method such as a gravure coating method or a roll coating method, and after drying, the barrier layer 3 or the substrate layer 1 is laminated, and then the adhesive layer 2 is cured.
[0208] Next, a heat-fusible resin layer 4 is laminated on the barrier layer protective film 3a of the laminate A. When the heat-fusible resin layer 4 is laminated directly on the barrier layer protective film 3a, the resin component constituting the heat-fusible resin layer 4 can be coated on the barrier layer protective film 3a of the laminate A by a gravure coating method, a roll coating method, or the like. In addition, when an adhesive layer 5 is provided between the barrier layer protective film 3a and the heat-fusible resin layer 4, for example, the following methods can be cited: (1) a method of laminating an adhesive layer 5 and a heat-fusible resin layer 4 on the barrier layer protective film 3a of the laminate A by co-extrusion (co-extrusion lamination method); (2) a method of separately forming a laminate in which an adhesive layer 5 and a heat-fusible resin layer 4 are laminated, and laminating the laminate on the barrier layer protective film 3a of the laminate A by a heat lamination method; (3) a method of laminating a barrier layer 5 on the barrier layer protective film 3a of the laminate A. (4) a method in which a molten adhesive layer 5 is poured between the barrier layer protective film 3a of the laminate A and the hot-melt adhesive layer 4 prefabricated in sheet form, while the laminate A and the hot-melt adhesive layer 4 are bonded to each other via the adhesive layer 5 (sandwich lamination method).
[0209] When the surface covering layer 6 is provided, the surface covering layer 6 is laminated on the surface of the substrate layer 1 on the opposite side to the barrier layer 3. The surface covering layer 6 can be formed, for example, by applying the above-mentioned resin for forming the surface covering layer 6 to the surface of the substrate layer 1. The order of the process of laminating the barrier layer 3 on the surface of the substrate layer 1 and the process of laminating the surface covering layer 6 on the surface of the substrate layer 1 is not particularly limited. For example, after the surface covering layer 6 is formed on the surface of the substrate layer 1, the barrier layer 3 can be formed on the surface of the substrate layer 1 on the opposite side to the surface covering layer 6.
[0210] As described above, a laminated body is formed which has the following sequence: surface covering layer 6 provided as required / base material layer 1 provided as required / adhesive layer 2 provided as required / barrier layer protective film 3b provided as required / barrier layer 3 / barrier layer protective film 3a / adhesive layer 5 provided as required / thermo-fusible resin layer 4. In order to strengthen the adhesion between adhesive layer 2 provided as required and adhesive layer 5, the laminated body may be subjected to a heat treatment such as a hot roll contact type, a hot air type, a near infrared type, or a far infrared type. As the conditions for such a heat treatment, for example, a heat treatment at about 150 to 250° C. for about 1 to 5 minutes may be cited.
[0211] In order to improve the film-forming property, lamination processing, and the adaptability to secondary processing (bagging, embossing) of the final product, or to stabilize these properties, the layers constituting the outer packaging material 10 may be subjected to surface activation treatments such as corona treatment, sandblasting, oxidation treatment, and ozone treatment as needed. For example, by subjecting at least one surface of the substrate layer 1 to corona treatment, the film-forming property, lamination processing, and the adaptability to secondary processing of the final product can be improved or stabilized. In addition, for example, by subjecting the surface of the substrate layer 1 opposite to the barrier layer 3 to corona treatment, the printing adaptability of the ink on the surface of the substrate layer 1 can be improved.
[0212] (Example)
[0213] The present invention will be described in detail below with reference to Examples and Comparative Examples, but the present invention is not limited to the Examples.
[0214] <Hydrogen sulfide permeation rate of resin constituting thermally adhesive resin layer>
[0215] like Figure 8 As shown in the schematic diagram, under the test temperature (approximately 23±5°C), each resin film (thickness recorded in Table 1) used as a heat-fusible resin layer of the outer packaging material for the all-solid-state battery was used as a sample, and the hydrogen sulfide permeation amount of the resin constituting the heat-fusible resin layer was obtained according to the following steps. The results are shown in Table 1.
[0216] (1) The sample A is placed between the separable flask upper portion 100 and the separable flask lower portion 200 .
[0217] (2) Nitrogen gas was introduced at 50 ml / min from the vent 101 at the upper portion 100 of the removable flask, and hydrogen sulfide gas (H2S concentration: 20±5 volume ppm / N2) was introduced at 50 ml / min from the vent 201 at the lower portion 200 of the removable flask.
[0218] (3) Under the following sampling conditions, a resin bag was connected to the vent port 101 at the top of the removable flask 100, and 0.5 L of sample gas was collected over 10 minutes.
[0219] Sampling conditions: After 28 hours, 48 hours, and 96 hours, a total of 3 times
[0220] (4) The concentration of the sample gas collected in the resin bag was measured using a gas chromatograph-flame photometric detector (GC-FPD).
[0221] (5) Based on the sample gas concentration (volume ppb) obtained by measurement, the permeation amount per hour (nL / hr) was calculated using the following calculation formula 1, and the permeability (cc / m 2 ·day). The unit is converted to cc·mm / cm 2 ·sec·cmHg.
[0222] Calculation formula 1: Permeation (nL / hr) = concentration (volume ppb ≈ nL / L) × gas volume collected per unit time (L / hr)
[0223] Since the test flow rate is 50mL / min, the amount of gas collected per unit time is 3L.
[0224] Calculation formula 2: Transmittance (cc / m 2 ·day)=permeation (nL / hr)×24(hr) / 10 6 / Effective test area (m 2 )
[0225] The effective test area is 0.00465m2 using the opening area of the removable flask 2 .
[0226] <Every 1m 2 Water vapor transmission rate>
[0227] The hydrogen sulfide permeation rate per m of each resin film used in the measurement was measured by the following method. 2 Water vapor transmission rate (single-sided area) (g / m 2 / 24h). The measurement was conducted using a water vapor transmission rate measuring device based on the isobaric method (PERMATRAN manufactured by MOCON) under the conditions of a temperature of 40°C, a relative humidity of 90%, a measurement period of 24 hours, and a measurement area of 8 cmφ according to the method specified in ISO15106-52008. 2 The water vapor transmission rate is converted into m by the ISO water vapor transmission rate measurement method. 2 The results are shown in Table 1.
[0228] <Evaluation of hydrogen sulfide leakage when used as outer packaging material>
[0229] For two sheets of outer packaging materials (300 mm in length and 150 mm in width in plan view) composed of a laminated body composed of a substrate layer / adhesive layer / barrier layer / thermo-melting resin layer (thickness of the resin film described in Table 1) laminated in sequence, assuming that the peripheral edge (4 sides) are heat-fused with a width of 3 mm (the thickness of each heat-melting resin layer is reduced to 95% at the heat-fused portion), the hydrogen sulfide (hydrogen sulfide permeation cc) leaking from the heat-melting resin layer over 10 years was calculated using the value of hydrogen sulfide permeation obtained from the above <hydrogen sulfide permeation of the resin constituting the heat-melting resin layer>. However, in this calculation, the hydrogen sulfide permeation of the barrier layer is set to 0 cc, and hydrogen sulfide is permeated from the heat-fused portion of the heat-melting resin layer, and the calculation is performed. The results are shown in Table 1.
[0230] [Table 1]
[0231]
[0232] [Example 1]
[0233] As a substrate layer, a laminated film is prepared in which polyethylene terephthalate film (12 μm) / adhesive layer (two-liquid curing polyurethane adhesive (polyol compound and aromatic isocyanate compound), thickness 3 μm) / biaxially stretched nylon film (thickness 15 μm) are laminated in sequence. In addition, a barrier layer composed of aluminum alloy foil (JIS H4160: 1994A8021H-O, thickness 40 μm) is prepared. A chemical conversion treatment is performed on both sides of the barrier layer by the method described later to form a barrier layer protective film (thickness 10 nm). Then, the barrier layer and the substrate layer are laminated by a dry lamination method. Specifically, a two-liquid curing polyurethane adhesive (polyol compound and aromatic isocyanate compound) is applied to one surface of the barrier layer protective film formed on the surface of the barrier layer to form an adhesive layer (thickness 3 μm after curing). Next, the adhesive layer and the biaxially stretched nylon film were laminated and then subjected to an aging treatment to prepare a laminate of substrate layer / adhesive layer / barrier layer protective film / barrier layer / barrier layer protective film. Next, a two-component curable polyurethane adhesive (polyol compound and aromatic isocyanate compound, thickness 3 μm after curing) as an adhesive layer and a polypropylene film (thickness 35 μm) in Table 1 as a heat-fusible resin layer were laminated on the barrier layer protective film of the obtained laminate to form an adhesive layer / heat-fusible resin layer. Next, the obtained laminate is aged and heated to obtain an outer packaging material composed of a laminate composed of substrate layer (polyethylene terephthalate film (12 μm)) / adhesive layer (3 μm) / biaxially stretched nylon film (15 μm) / adhesive layer (3 μm) / barrier layer protective film (10 nm) / barrier layer (40 μm) / barrier layer protective film (10 nm) / adhesive layer (3 μm) / thermo-fusible resin layer (35 μm) stacked in sequence.
[0234] The barrier layer protective films on both sides of the barrier layer were formed as follows: a treatment liquid containing 43 parts by mass of an aminophenol polymer, 16 parts by mass of chromium fluoride, and 13 parts by mass of phosphoric acid relative to 100 parts by mass of water was prepared, the treatment liquid was applied to both sides of the barrier layer (the film thickness after drying was 10 nm), and the surface temperature of the barrier layer reached about 190° C., and then heated and dried for about 3 seconds.
[0235] [Example 2]
[0236] As the heat-fusible resin layer, the polyethylene film (thickness 40 μm) in Table 1 was used. The same operation as in Example 1 was carried out except that the above-mentioned operation was carried out to obtain an outer packaging material consisting of a laminated body formed by laminating in sequence base layer (polyethylene terephthalate film (12 μm)) / adhesive layer (3 μm) / biaxially stretched nylon film (15 μm) / adhesive layer (3 μm) / barrier layer protective film (10 nm) / barrier layer (40 μm) / barrier layer protective film (10 nm) / adhesive layer (3 μm) / heat-fusible resin layer (40 μm).
[0237] [Example 3]
[0238] Except that no barrier layer protective film is formed on the surface of the barrier layer, the same operation as in Example 1 is carried out to obtain an outer packaging material consisting of a laminated body formed by laminating in sequence substrate layer (polyethylene terephthalate film (12 μm)) / adhesive layer (3 μm) / biaxially stretched nylon film (15 μm) / adhesive layer (3 μm) / barrier layer (40 μm) / adhesive layer (3 μm) / thermofusible resin layer (35 μm).
[0239] [Example 4]
[0240] Except that no barrier layer protective film is formed on the surface of the barrier layer, the same operation as in Example 2 is carried out to obtain an outer packaging material consisting of a laminated body formed by laminating in sequence substrate layer (polyethylene terephthalate film (12 μm)) / adhesive layer (3 μm) / biaxially stretched nylon film (15 μm) / adhesive layer (3 μm) / barrier layer (40 μm) / adhesive layer (3 μm) / thermofusible resin layer (40 μm).
[0241] [Example 5]
[0242] A laminate of substrate layer / adhesive layer / barrier layer protective film / barrier layer / barrier layer protective film was prepared in the same manner as in Example 1. Then, maleic anhydride-modified polypropylene as an adhesive layer (thickness 40 μm) and polypropylene (having a hydrogen sulfide permeation rate shown in Table 1) as a heat-fusible resin layer (thickness 35 μm) were laminated on the barrier layer protective film of the obtained laminate, so that the adhesive layer / heat-fusible resin layer was laminated. Next, the obtained laminate is aged and heated to obtain an outer packaging material composed of a laminate composed of substrate layer (polyethylene terephthalate film (12 μm)) / adhesive layer (3 μm) / biaxially stretched nylon film (15 μm) / adhesive layer (3 μm) / barrier layer protective film (10 nm) / barrier layer (40 μm) / barrier layer protective film (10 nm) / adhesive layer (40 μm) / thermo-fusible resin layer (35 μm) stacked in sequence.
[0243] <Time-of-flight secondary ion mass spectrometry>
[0244] The barrier layer protective film is analyzed as follows. First, the barrier layer and the adhesive layer are peeled off. At this time, the peeling is not performed physically with water or an organic solvent, an acid or alkali aqueous solution, or the like. After the barrier layer and the adhesive layer are peeled off, since the adhesive layer remains on the surface of the barrier layer, the remaining adhesive layer is removed by etching using Ar-GCIB. The surface of the barrier layer obtained in this way is analyzed for the barrier layer protective film using time-of-flight secondary ion mass spectrometry. -PO2 - and PO3 - The peak intensity P CrPO4 , P PO2 , P PO3 , peak intensity P PO2 Relative to the peak intensity P CrPO4 Ratio P PO2 / CrPO4 , peak intensity P PO3 Relative to the peak intensity P CrPO4 Ratio P PO3 / CrPO4 As shown in Table 1. In Examples 3 and 4, since no barrier layer protective film is formed on the surface of the barrier layer, the CrPO4 - The peak intensity P CrPO4 Related items are indicated by “-”.
[0245] The details of the measurement apparatus and measurement conditions of time-of-flight secondary ion mass spectrometry are as follows.
[0246] Measuring device: Time-of-flight secondary ion mass spectrometer TOF.SIMS5 manufactured by ION-TOF
[0247] (Measurement conditions)
[0248] Primary ions: Doubly charged ions of bismuth cluster (Bi3 ++ )
[0249] Primary ion acceleration voltage: 30kV
[0250] Mass range (m / z): 0~1500
[0251] Measuring range: 100μm×100μm
[0252] Scan number: 16 scan / cycle
[0253] Number of pixels (1 side): 256 pixels
[0254] Etching ions: Ar gas cluster ion beam (Ar-GCIB)
[0255] Etching ion acceleration voltage: 5.0kV
[0256] <Evaluation of barrier layer degradation caused by confinement under high pressure pressing>
[0257] On the side of the heat-melting resin layer of the outer packaging material, a hole of φ1mm is opened in such a way that the surface of the barrier layer protective film is exposed. Specifically, in the above-mentioned Examples 1 to 5, as the heat-melting resin layer, a heat-melting resin layer with a hole of φ1mm opened in such a way that the surface of the barrier layer protective film is exposed is used to make the outer packaging material. Each of these outer packaging materials is used as a test piece, and high pressure pressing (50MPa) is applied in a state where a sulfide solid electrolyte (Li2S:P2S5=75:25, thickness 300μm) is arranged between the test piece and the lithium indium alloy (LiIn alloy). At this time, the sulfide solid electrolyte is arranged in a portion of the outer packaging material where a hole of φ1mm is opened. Among them, since the barrier layer protective film is not provided in Examples 3 and 4, the surface of the barrier layer is exposed. In this state, a voltage of 0.53V is applied between the barrier layer and the LiIn alloy of the test piece and left to stand for 1 hour. After 1 time, the surface of the barrier layer at the portion of the test piece where the hole of φ1 mm was opened was observed under a microscope to confirm whether an alloy was formed on the surface of the barrier layer. The case where no alloy was formed on the surface of the barrier layer was evaluated as A, and the case where an alloy was formed was evaluated as C. The results are shown in Table 2.
[0258] [Table 2]
[0259]
[0260] As described above, the present invention provides the following aspects of the invention.
[0261] Item 1. An outer packaging material for an all-solid-state battery, for an all-solid-state battery containing a sulfide solid electrolyte material, the outer packaging material for an all-solid-state battery comprising, in order from the outside, at least a substrate layer, a barrier layer, a barrier layer protective film formed on the surface of the barrier layer, and a thermally fusible resin layer.
[0262] The hydrogen sulfide permeation rate of the resin constituting the thermally fusible resin layer is 1.0×10 -8 cc mm / cm 2 ·sec·cmHg or more.
[0263] Item 2. The all-solid-state battery outer casing material according to Item 1, wherein the thickness of the thermally fusible resin layer is 10 μm or more.
[0264] Item 3. The all-solid battery outer casing material according to Item 1 or 2, wherein the base layer comprises a polyester, an adhesive layer, and a polyamide in this order from the outside.
[0265] Item 4. The all-solid-state battery outer casing material according to Item 1 or 2, wherein the base layer is composed of a single layer of a polyester resin.
[0266] Item 5. The all-solid-state battery outer packaging material according to any one of Items 1 to 4, wherein, when the barrier layer protective film is analyzed using time-of-flight secondary ion mass spectrometry, the PO3 - The peak intensity P PO3 Relative to CrPO4 - The peak intensity P CrPO4 Ratio P PO3 / CrPO4 In the range of 6 to 120.
[0267] Item 6. A total solid battery packaging body obtained by molding the total solid battery outer packaging material according to any one of Items 1 to 5.
[0268] Item 7. An all-solid-state battery, comprising a battery element at least comprising a single cell contained in a packaging body formed of an outer packaging material for an all-solid-state battery, wherein the single cell comprises a positive electrode active material layer, a negative electrode active material layer, and a solid electrolyte layer stacked between the positive electrode active material layer and the negative electrode active material layer, wherein:
[0269] The solid electrolyte layer comprises a sulfide solid electrolyte material.
[0270] The all-solid-state battery outer packaging material is composed of a laminate having at least a base layer, a barrier layer, a barrier layer protective film formed on the surface of the barrier layer, and a heat-fusible resin layer in this order from the outside.
[0271] The hydrogen sulfide permeation rate of the resin constituting the thermally fusible resin layer is 1.0×10 -8 cc mm / cm 2 ·sec·cmHg or more.
[0272] Item 8. A method for producing an outer packaging material for an all-solid-state battery, the outer packaging material for an all-solid-state battery being used for an all-solid-state battery containing a sulfide solid electrolyte material, the method comprising the step of laminating a substrate layer, a barrier layer, a barrier layer protective film formed on the surface of the barrier layer, and a heat-fusible resin layer in order from at least the outside to obtain a laminated body,
[0273] The hydrogen sulfide permeation rate of the resin constituting the thermally fusible resin layer is 1.0×10 -8 cc mm / cm 2 ·sec·cmHg or more.
Claims
1. An outer packaging material for an all-solid-state battery, which is used for an all-solid-state battery containing a sulfide solid electrolyte material, the outer packaging material for an all-solid-state battery is composed of a laminate having at least a substrate layer, a barrier layer, a barrier layer protective film formed on the surface of the barrier layer, and a heat-fusible resin layer in this order from the outside, and the outer packaging material for an all-solid-state battery is characterized in that: The barrier layer is formed of aluminum alloy foil, The hydrogen sulfide permeation rate of the resin constituting the thermally fusible resin layer is 1.0×10 -8 cc mm / cm 2 ·sec·cmHg or more.
2. The outer packaging material for an all-solid-state battery according to claim 1, characterized in that: The thickness of the thermally fusible resin layer is 10 μm or more.
3. The outer packaging material for an all-solid-state battery according to claim 1 or 2, characterized in that: The base material layer has polyester, an adhesive layer, and polyamide in this order from the outside.
4. The outer packaging material for an all-solid-state battery according to claim 1 or 2, characterized in that: The substrate layer is composed of a single layer of polyester resin.
5. The all-solid battery outer packaging material according to any one of claims 1 to 4, characterized in that: When the barrier layer protective film was analyzed using time-of-flight secondary ion mass spectrometry, the PO3 - The peak intensity P PO3 Relative to CrPO4 - The peak intensity P CrPO4 Ratio P PO3 / CrPO4 In the range of 6 to 120.
6. The all-solid battery outer packaging material according to any one of claims 1 to 5, characterized in that: When the barrier layer protective film was analyzed using time-of-flight secondary ion mass spectrometry, the PO2 - The peak intensity P PO2 Relative to CrPO4 - The peak intensity P CrPO4 Ratio P PO2 / CrPO4 In the range of 7 to 70.
7. A package for an all-solid-state battery, characterized in that: The all-solid-state battery packaging material is formed by molding the all-solid-state battery packaging material according to any one of claims 1 to 6.
8. An all-solid-state battery, wherein a battery element including at least a single cell is housed in a packaging body formed of an outer packaging material for an all-solid-state battery, wherein the single cell includes a positive electrode active material layer, a negative electrode active material layer, and a solid electrolyte layer stacked between the positive electrode active material layer and the negative electrode active material layer, wherein the all-solid-state battery is characterized in that: The solid electrolyte layer comprises a sulfide solid electrolyte material, The all-solid-state battery outer packaging material is composed of a laminate having at least a base layer, a barrier layer, a barrier layer protective film formed on the surface of the barrier layer, and a heat-fusible resin layer in this order from the outside. The barrier layer is formed of aluminum alloy foil, The hydrogen sulfide permeation rate of the resin constituting the thermally fusible resin layer is 1.0×10 -8 cc mm / cm 2 ·sec·cmHg or more.
9. A method for producing an outer packaging material for an all-solid-state battery, wherein the outer packaging material for an all-solid-state battery is used for an all-solid-state battery containing a sulfide solid electrolyte material, wherein the method for producing an outer packaging material for an all-solid-state battery is characterized by: The method comprises the steps of laminating at least a base material layer, a barrier layer, a barrier layer protective film formed on the surface of the barrier layer, and a heat-fusible resin layer in this order from the outside to obtain a laminated body, The barrier layer is formed of aluminum alloy foil, The hydrogen sulfide permeation rate of the resin constituting the thermally fusible resin layer is 1.0×10 -8 cc mm / cm 2 ·sec·cmHg or more.
Citation Information
Patent Citations
All-solid battery
JP2008103288A
Method for manufacturing electrode body, and method for manufacturing battery
JP2012142228A
Substrate support mechanism
JP2020002424A