High-heat-resistance self-repairing diaphragm as well as preparation method and application thereof
By forming a porous network structure of high heat-resistant self-healing separator through coaxial electrospun nanofibers with a core-shell structure, the problem of insufficient heat resistance and mechanical strength of traditional separators is solved, thereby improving the safety and electrochemical performance of the battery.
Patent Information
- Application Number
- CN202411187648.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-08-27
AI Technical Summary
Traditional separators cannot meet the heat resistance and mechanical strength requirements of high-capacity battery cells, which can easily lead to thermal runaway and safety issues.
A high-heat-resistant, self-healing separator with a porous network structure is formed by coaxial electrospun nanofibers with a core-shell structure. It utilizes free radical polymerized monomers and crosslinking agents to self-repair when the battery is damaged, thereby enhancing mechanical strength and heat resistance.
It improves the electrolyte absorption rate and ionic conductivity of the separator, enhances the safety and electrochemical performance of the battery, overcomes the wrinkling problem of the separator during battery assembly, storage and transportation, and meets the usage requirements of energy storage cells.
Smart Images

Figure CN118920013A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of battery separators, and more specifically to a highly heat-resistant self-repairing separator and a preparation method and application thereof. Background Art
[0002] In recent years, the development momentum of energy storage and power has been rapid. In this context, large-capacity batteries can reduce the unit capacity cost through scale effect. This cost advantage makes large-capacity batteries more economically attractive. However, large-capacity batteries have high energy density and high heat release, which can easily lead to thermal runaway. Due to production technology and raw materials used, traditional diaphragms cannot meet the requirements of energy storage batteries in terms of heat resistance, membrane rupture temperature, and mechanical strength.
[0003] Therefore, how to improve the performance of the diaphragm is a technical problem that needs to be urgently solved in this field. Summary of the invention
[0004] The present application provides a highly heat-resistant self-repairing diaphragm and a preparation method and application thereof, so as to solve the problem of poor heat resistance and mechanical strength of the diaphragm and meet the use requirements of energy storage cells.
[0005] The present application provides a highly heat-resistant self-healing membrane, which includes coaxial electrospun nanofibers with a core-shell structure; the nanofibers form a porous network structure; the nanofibers include a first nanofiber and a second nanofiber, the first nanofiber includes a first shell layer and a first core layer, the first shell layer is coated on the outside of the first core layer; the second nanofiber includes a second shell layer and a second core layer, the second shell layer is coated on the outside of the second core layer.
[0006] In an optional embodiment, the first core layer includes free radical polymerization monomers; the second core layer includes a cross-linking agent, and the cross-linking agent can induce cross-linking of the free radical polymerization monomers.
[0007] In an optional embodiment, the free radical polymerization monomer includes at least one of dicyclopentadiene, isoprene, methyl methacrylate, polydiethoxysiloxane, terminal hydroxylated polydimethylsiloxane and N,N-methylenebisacrylamide.
[0008] In an optional embodiment, the cross-linking agent includes at least one of Grubbs' catalyst, di-n-butyltin dilaurate, a tungsten hexachloride phenylacetylene mixture and an azide.
[0009] In an optional embodiment, the first shell layer and / or the second shell layer comprises a high temperature resistant polymer material, and the high temperature resistant polymer material comprises at least one of polyimide, polyarylethersulfoneketone, polyetherimide, polyphenylsulfone, polyisophthalamide and the like.
[0010] In an optional embodiment, the diaphragm satisfies at least one of the conditions (1)-(6):
[0011] (1) The diameter of the first nanofiber and / or the second nanofiber is 0.2 μm-2.0 μm;
[0012] (2) The mass ratio of the first nanofiber to the second nanofiber is 1:1;
[0013] (3) In the first nanofiber, the mass ratio of the first core layer to the first shell layer is 1:0.4-1:2.0;
[0014] (4) In the second nanofiber, the mass ratio of the second core layer to the second shell layer is 1:0.4-1:2.0;
[0015] (5) The thickness d of the diaphragm is in the range of 3 μm ≤ d ≤ 100 μm;
[0016] (6) The porosity of the diaphragm is 30%-60%.
[0017] The present application provides a method for preparing a highly heat-resistant self-repairing diaphragm, which is used to prepare the diaphragm as described above, comprising the following steps:
[0018] Dissolving the materials for preparing the first shell layer and the second shell layer in a solvent according to a preset ratio, and stirring and mixing them evenly to obtain a shell layer spinning solution;
[0019] Dissolving the material for preparing the first core layer in a solvent according to a preset ratio, and stirring and mixing to obtain a first core layer spinning solution;
[0020] Dissolving the material for preparing the second core layer in a solvent according to a preset ratio, and stirring and mixing to obtain a second core layer spinning solution;
[0021] The shell layer spinning solution, the first core layer spinning solution and the second core layer spinning solution are used as electrospinning solutions, and a highly heat-resistant self-repairing nanofiber membrane having a porous network structure including first nanofibers and second nanofibers is obtained on a receiver by a coaxial electrospinning method;
[0022] After the high heat-resistant self-repairing nanofiber membrane is vacuum-dried, it is hot-pressed under preset conditions to obtain the high heat-resistant self-repairing nanofiber membrane.
[0023] In an optional embodiment, the diaphragm satisfies at least one of the conditions (1)-(3):
[0024] (1) The first core layer includes free radical polymerizable monomers;
[0025] Optionally, the free radical polymerization monomer includes at least one of dicyclopentadiene, isoprene, methyl methacrylate, polydiethoxysiloxane, terminal hydroxylated polydimethylsiloxane and N,N-methylenebisacrylamide;
[0026] (2) the second core layer includes a crosslinking agent, and the crosslinking agent can induce crosslinking of the free radical polymerization monomer;
[0027] Optionally, the cross-linking agent includes at least one of Grubbs catalyst, di-n-butyltin dilaurate, tungsten hexachloride phenylacetylene mixture and azide;
[0028] (3) Both the first shell layer and the second shell layer are made of a high temperature resistant polymer material;
[0029] Optionally, the high temperature resistant polymer material includes at least one of polyimide, polyarylethersulfoneketone, polyetherimide, polyphenylsulfone, polyisophthalamide and the like.
[0030] In an optional embodiment, the diaphragm satisfies at least one of the conditions (1)-(8):
[0031] (1) In the shell layer spinning solution, the mass percentage of the material for preparing the first shell layer and the second shell layer is 5wt.%-30wt.%;
[0032] (2) In the first core layer spinning solution, the mass percentage of the material for preparing the first core layer is 5wt.%-30wt.%;
[0033] (3) In the second core layer spinning solution, the mass percentage of the material for preparing the second core layer is 5wt.%-30wt.%;
[0034] (4) The coaxial electrospinning method includes preparing the diaphragm by using a transmitter and a receiver in combination under the action of an electric field, the voltage of the electric field is 10kV-20kV, the distance between the transmitter and the receiver is 10cm-20cm, the injection rate of the shell layer spinning solution is 0.5mL / h-1.0mL / h, and the injection rate of the first core layer spinning solution and / or the second core layer spinning solution is 0.05mL / h-1.0mL / h;
[0035] (5) The thickness d of the diaphragm is in the range of 3 μm ≤ d ≤ 100 μm;
[0036] (6) The mass ratio of the first nanofiber to the second nanofiber is 1:1;
[0037] (7) The diameters of the first nanofiber and the second nanofiber are both 0.2 μm-2.0 μm;
[0038] (8) The preset conditions during hot pressing include hot pressing temperature and hot pressing pressure. The hot pressing temperature is in the range of 40°C-100°C, and the hot pressing pressure is in the range of 5MPa-20MPa.
[0039] The present application provides a secondary battery, comprising the separator as described above or the separator prepared by the preparation method as described above.
[0040] According to the high heat-resistant self-healing diaphragm in the above embodiment, the diaphragm includes coaxial electrospun nanofibers of a core-shell structure, the nanofibers form a porous network structure, the nanofibers include a first nanofiber and a second nanofiber, the first nanofiber includes a first shell layer and a first core layer, the first shell layer is coated on the outside of the first core layer; the second nanofiber includes a second shell layer and a second core layer, the second shell layer is coated on the outside of the second core layer. Since the diaphragm is a porous network structure mainly formed by two coaxial electrospun nanofibers, the diaphragm has the advantages of high porosity, unique pore structure and large specific surface area, which can significantly improve the electrolyte absorption rate and retention rate of the diaphragm, thereby allowing the battery to accommodate more electrolytes so that more ions can be freely transferred and transmitted, thereby improving the ionic conductivity of the diaphragm, and finally stably improving the electrochemical performance of the battery. Since the coaxial electrospun nanofibers have a large aspect ratio, the resulting diaphragm has high integrity, heat resistance and high mechanical strength. Since the diaphragm is formed by a plurality of nanofibers, there is a "loose" molecular force between the "microscopic" nanofibers, which gives the diaphragm a certain "macro" flexibility. Therefore, it can easily pass mechanical performance tests such as bending, twisting, and folding, overcoming the safety problems caused by the diaphragm being easily wrinkled during the assembly, storage, transportation and other uses of the battery. This makes the diaphragm promising as a new generation of battery diaphragm that can meet the use requirements of energy storage cells and improve the safety and electrochemical properties of the battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] Figure 1 A schematic diagram of the structure of a diaphragm in an embodiment;
[0042] Figure 2 Schematic diagram of the structure of nanofibers in one embodiment.
[0043] Wherein: 100, first nanofiber; 110, first shell layer; 120, first core layer; 200, second nanofiber; 210, second shell layer; 220, second core layer. DETAILED DESCRIPTION
[0044] The present application is further described in detail below by specific embodiments in conjunction with the accompanying drawings. Wherein similar elements in different embodiments adopt associated similar element numbers. In the following embodiments, many detailed descriptions are intended to enable the present application to be better understood. However, those skilled in the art can easily recognize that some of the features can be omitted in different situations, or can be replaced by other elements, materials, and methods. In some cases, some operations related to the present application are not shown or described in the specification, in order to avoid the core part of the present application being overwhelmed by too much description, and for those skilled in the art, it is not necessary to describe these related operations in detail, and they can fully understand the related operations based on the description in the specification and the general technical knowledge in the art.
[0045] In addition, the features, operations or characteristics described in the specification can be combined in any appropriate manner to form various implementations, and the operation steps involved in each embodiment can also be replaced or adjusted in a sequence in a manner that is obvious to those skilled in the art. Therefore, the specification and drawings are only for the purpose of clearly describing a certain embodiment and do not mean that the composition and / or sequence are necessary.
[0046] The serial numbers of the components in this document, such as "first", "second", etc., are only used to distinguish the objects described and do not have any order or technical meaning. The "connection" and "coupling" mentioned in this application, unless otherwise specified, include direct and indirect connections (couplings).
[0047] In this application, the so-called "secondary battery" refers to a battery that can be used continuously by activating the active material by charging after the battery is discharged. This type of battery usually uses the reversibility of chemical reactions, that is, after a chemical reaction is converted into electrical energy, the chemical system can be repaired by electrical energy, and then converted into electrical energy by chemical reaction. Among them, the more common secondary batteries include but are not limited to nickel-metal hydride batteries, nickel-cadmium batteries, lead-acid (or lead storage) batteries, lithium-ion batteries, polymer lithium-ion batteries, sodium-ion batteries, etc.
[0048] In this application, the so-called "diaphragm" is an important component of the secondary battery cell. The diaphragm is a thin film used to separate the positive and negative electrodes during the electrolysis reaction to prevent the loss of energy in the direct reaction. The performance of the diaphragm determines the interface structure and internal resistance of the battery, and directly affects the battery's capacity, cycle and safety performance. Excellent battery composite diaphragms play an important role in improving the overall performance of the battery.
[0049] The mechanical properties of battery separators can largely determine the durability and safety of the battery during cycling. The mechanical strength of the separator is characterized by testing the strength in the MD and TD directions, where MD is the machine direction and TD is the direction perpendicular to MD.
[0050] See also Figure 1 and Figure 2 The present application provides a highly heat-resistant self-healing diaphragm, which includes coaxial electrospun nanofibers of a core-shell structure, the nanofibers forming a porous network structure, the nanofibers including a first nanofiber 100 and a second nanofiber 200, the first nanofiber 100 including a first shell layer 110 and a first core layer 120, the first shell layer 110 being coated on the outside of the first core layer 120; the second nanofiber 200 including a second shell layer 210 and a second core layer 220, the second shell layer 210 being coated on the outside of the second core layer 220, the first nanofiber 100 and the second nanofiber 200 are both prepared by a coaxial electrospinning method, and then the first nanofiber 100 and the second nanofiber 200 are alternately arranged to form a diaphragm.
[0051] Different from the existing diaphragms prepared by forming various functional coatings on the base membrane, the present application pioneered the use of nanofibers to directly prepare the diaphragm, which simplifies the diaphragm preparation process and can reduce the cost of the diaphragm; when the first nanofiber 100 and the second nanofiber 200 are arranged, a plurality of pores are naturally formed between them, and the pores can be used as ion channels, which are equivalent to the pores on the base membrane. The pores of the base membrane are formed by dry stretching or wet stretching, while those in the present application are formed during the preparation of the diaphragm. The pores are easy to shape and control, and the pores are more uniform, which is more conducive to regulating the ionic conductivity and air permeability of the diaphragm.
[0052] Since the diaphragm is a porous network structure mainly formed by two coaxial electrospun nanofibers, the diaphragm has the advantages of high porosity, unique pore structure and large specific surface area, which can significantly improve the electrolyte absorption rate and retention rate of the diaphragm, thereby allowing the battery to accommodate more electrolytes so that more ions can be freely transferred and transmitted, thereby improving the ionic conductivity of the diaphragm and ultimately improving the electrochemical performance of the battery. Since the coaxial electrospun nanofibers have a large aspect ratio, the resulting diaphragm has high integrity, heat resistance and high mechanical strength. Since the diaphragm is formed by the arrangement of multiple nanofibers, there are "loose" molecular forces between the "microscopic" nanofibers, which gives the diaphragm a certain "macro" flexibility, so it can easily pass mechanical performance tests such as bending, twisting, and folding, overcoming the safety problems caused by the diaphragm's easy wrinkling during the assembly, storage, transportation and other uses of the battery, making the diaphragm promising as a new generation of battery diaphragms that can meet the test of the new national standard energy storage battery cell and improve the safety and electrochemical performance of the battery.
[0053] In some embodiments, the first core layer 120 includes free radical polymerization monomers; the second core layer 220 includes a cross-linking agent, which can induce cross-linking of the free radical polymerization monomers. When the battery is damaged, the first nanofiber 100 and the second nanofiber 200 can release free radical polymerization monomers and cross-linking agents, which will flow to the damaged interface of the battery separator after release, so that the free radical polymerization monomers undergo cross-linking reactions at the damaged interface, so as to perform self-repairing functions on the battery separator, improve the puncture resistance, prevent the occurrence of short circuits, and help improve the cycle life and safety of the secondary battery.
[0054] In some embodiments, the free radical polymerization monomer may be at least one of dicyclopentadiene, isoprene, methyl methacrylate, polydiethoxysiloxane, terminal hydroxylated polydimethylsiloxane, and N,N-methylenebisacrylamide. The crosslinking agent may be at least one of Grubbs catalyst, di-n-butyltin dilaurate, tungsten hexachloride phenylacetylene mixture, and azide.
[0055] It should be understood that the first shell layer 110 and the second shell layer 210 may be the same or different, and the present application does not make specific limitations on this. Exemplary, for example, the first shell layer 110 and / or the second shell layer 210 are made of a high temperature resistant polymer material, and the first shell layer 110 and the second shell layer 210 may be independently selected from at least one of polyimide, polyarylethersulfoneketone, polyetherimide, polyphenylsulfone, polyisophthalamide, etc. The selection of high temperature resistant polymer materials can enhance the mechanical stability and heat resistance of the nanofibers, and give the diaphragm high heat resistance and high film breaking performance. At the same time, the high temperature resistant polymer materials have high heat resistance and flame retardancy, so that the nanofibers have good thermal stability and self-extinguishing properties, and the diaphragm has excellent thermal stability and non-flammability, which can improve the safety performance of the secondary battery.
[0056] In some embodiments, the diameters of the first nanofiber 100 and the second nanofiber 200 may be the same or different, and the present application does not specifically limit this. The diameters of the first nanofiber 100 and / or the second nanofiber 200 are both 0.2 μm-2.0 μm, and for example, the diameters of the first nanofiber 100 and / or the second nanofiber 200 may be 0.2 μm, 0.5 μm, 1.0 μm, 1.5 μm or 2.0 μm.
[0057] In some embodiments, the mass ratio of the first nanofiber 100 to the second nanofiber 200 is 1:1, so that the free radical polymer can be fully cross-linked.
[0058] In some embodiments, in the first nanofiber 100, the mass ratio of the first core layer 120 to the first shell layer 110 is 1:0.4-1:2.0; in the second nanofiber 200, the mass ratio of the second core layer 220 to the second shell layer 210 is 1:0.4-1:2.0; the mass ratio of the core layer and the shell layer of the nanofiber is within the above range, which is conducive to the balance of heat resistance, high membrane rupture temperature, integrity, mechanical strength, and self-healing performance.
[0059] In some embodiments, the thickness d of the separator is in the range of 3 μm ≤ d ≤ 100 μm. For example, the thickness d of the separator is 3 μm, 10 μm, 20 μm, 30 μm, 40 μm, 50 μm or 100 μm. The thickness d of the separator within the above range is beneficial to improving the mechanical strength, heat resistance, and ionic conductivity of the separator, and is beneficial to improving the safety, cycle, power, and energy density of the secondary battery.
[0060] In some embodiments, the porosity of the diaphragm is 30%-60%. For example, the porosity of the diaphragm can be 30%, 35%, 40%, 45%, 50%, 55% or 60%. The porous grid structure formed by the first nanofiber 100 and the second nanofiber 200 can well meet this condition. By adjusting the size and gap between the first nanofiber 100 and the second nanofiber 200, the purpose of adjusting the porosity of the diaphragm is achieved.
[0061] It should be noted that porosity refers to the percentage of the pore volume in the diaphragm material to the total volume of the material in its natural state.
[0062] The present application provides a method for preparing a highly heat-resistant self-repairing diaphragm, comprising the following steps:
[0063] Dissolving the materials for preparing the first shell layer 110 and the second shell layer 210 in a solvent according to a preset ratio, and stirring and mixing them uniformly to obtain a shell layer spinning solution;
[0064] Dissolving the material for preparing the first core layer 120 in a solvent according to a preset ratio, stirring and mixing to obtain a spinning solution for the first core layer 120;
[0065] Dissolving the material for preparing the second core layer 220 in a solvent according to a preset ratio, stirring and mixing to obtain a spinning solution for the second core layer 220;
[0066] The shell layer spinning solution, the first core layer 120 spinning solution and the second core layer 220 spinning solution are used as electrospinning solutions, and a highly heat-resistant self-repairing nanofiber membrane having a porous network structure including the first nanofiber 100 and the second nanofiber 200 is obtained on a receiver by a coaxial electrospinning method;
[0067] After the high heat-resistant self-repairing nanofiber membrane is vacuum-dried, it is hot-pressed under preset conditions to obtain a high heat-resistant self-repairing nanofiber membrane.
[0068] In some embodiments, the solvent is a highly volatile solvent, including dimethylacetamide. During the process of preparing the diaphragm, the solvent can evaporate, thereby preparing a diaphragm that is resistant to high temperatures and has good mechanical strength.
[0069] In some embodiments, in the shell spinning solution, the mass percentage of the material for preparing the first shell layer 110 and the second shell layer 210 is 5wt.%-30wt.%; in the first core layer 120 spinning solution, the mass percentage of the material for preparing the first core layer 120 is 5wt.%-30wt.%; in the second core layer 220 spinning solution, the mass percentage of the material for preparing the second core layer 220 is 5wt.%-30wt.%, and the selection of the above mass ratio is conducive to forming a uniform spinning solution, thereby facilitating the improvement of the spinning rate and the uniformity of the nanofibers, and facilitating the improvement of the uniformity of the performance of the diaphragm. Exemplarily, for example, the mass percentages in the shell spinning solution, the first core layer 120 spinning solution, and the second core layer 220 spinning solution can be 5wt.%, 10wt.%, 15wt.%, 20wt.%, 25wt.%, or 30wt.%.
[0070] It should be further explained that the coaxial electrospinning method is a special electrospinning technology that allows solutions of different properties to be injected into two coaxial capillaries respectively, thereby preparing nanofibers with specific structures. The basic principle of this technology is that under the action of the electric field, the solutions in two coaxial capillaries with different inner diameters (one is the core solution and the other is the shell solution) converge at the end of the nozzle and solidify into composite nanofibers. When preparing a film with a core-shell structure, two capillaries are used as transmitters, and a rotating cylinder is set as a receiver. The nanofibers are fully and evenly laid (laid) by rotating the rotating cylinder, and the diaphragm is prepared after hot pressing and drying. Therefore, the distance between the receiver and the transmitter, the electric field voltage and the injection rate of the spinning solution can all affect the properties of the prepared nanofibers, and then affect the properties of the diaphragm.
[0071] In some embodiments, the coaxial electrospinning method includes using a transmitter and a receiver to cooperate to produce a diaphragm under the action of an electric field, and the voltage of the electric field is 10kV-20kV. For example, the voltage of the electric field can be 10kV, 12kV, 15kV, 17kV and 20kV.
[0072] In some embodiments, the distance between the transmitter and the receiver is 10 cm-20 cm. For example, the distance between the transmitter and the receiver may be 10 cm, 12 cm, 15 cm, 17 cm and 20 cm.
[0073] In some embodiments, the injection rate of the shell layer spinning solution is 0.5mL / h-1.0mL / h, and exemplarily, for example, the injection rate of the shell layer spinning solution is 0.5mL / h, 0.6mL / h, 0.7mL / h, 0.8mL / h, 0.9mL / h and 1.0mL / h. The injection rate of the first core layer 120 spinning solution and / or the second core layer 220 spinning solution is 0.05mL / h-1.0mL / h, and exemplarily, for example, the injection rate of the first core layer 120 spinning solution and / or the second core layer 220 spinning solution can be 0.05mL / h, 0.1mL / h, 0.5mL / h, 0.6mL / h, 0.7mL / h, 0.8mL / h, 0.9mL / h and 1.0mL / h. The injection rates of the first core layer 120 spinning solution and the second core layer 220 spinning solution can be the same or different. Preferably, the injection rates of the first core layer 120 spinning solution and the second core layer 220 spinning solution are the same. Controlling the injection rates of the core layer spinning solution and the shell layer spinning solution can effectively ensure the morphology and diameter of the prepared nanofibers, so that the fiber aspect ratio is appropriate and the morphology is smooth, which is conducive to filamentation and nanofiber bonding, can ensure production efficiency and enhance fiber strength, and effectively improve the mechanical properties of the diaphragm.
[0074] It should be understood that the injection rates of the first core layer 120 spinning solution, the second core layer 220 spinning solution and the shell layer spinning solution mentioned herein refer to the rate at which the syringe injects the liquid into the coaxial spinning needle.
[0075] In some embodiments, the preset conditions during hot pressing include hot pressing temperature and hot pressing pressure. The hot pressing temperature ranges from 40°C to 100°C. For example, the hot pressing temperature is 40°C, 50°C, 60°C, 70°C, 80°C, 90°C or 100°C. The hot pressing pressure ranges from 5MPa to 20MPa. For example, the hot pressing pressure is 5MPa, 6MPa, 7MPa, 8MPa, 9MPa, 10MPa, 15MPa or 20MPa. Hot pressing can improve the mechanical strength of the diaphragm. Since the nanofibers produced by coaxial electrospinning are often fluffy and the bonding force between the fibers is weak, resulting in insufficient mechanical strength. After hot pressing, the originally fluffy fibers can be in close contact to form bonding points, thereby effectively reducing the phenomenon of slippage between fibers under force, and can significantly improve the tensile strength and elongation at break of the diaphragm, and effectively improve the mechanical properties of the diaphragm. At the same time, hot pressing can also remove solvents and moisture in the fibers, thereby enhancing the bonding between the fibers, adjusting the porosity and structure of the diaphragm, and improving the flatness and density of the diaphragm.
[0076] In addition, the present application also provides a secondary battery, comprising the above-mentioned diaphragm or the diaphragm prepared by the above-mentioned preparation method.
[0077] In order to facilitate the description of the beneficial effects of the present application, the present application also provides the following several more specific embodiments.
[0078] Embodiment 1
[0079] The present embodiment provides a highly heat-resistant self-healing diaphragm, comprising a first nanofiber 100 and a second nanofiber 200. The first nanofiber 100 and the second nanofiber 200 are both core-shell structures, and both include a core layer and a shell layer coated on the outside of the core layer. The core layers of the first nanofiber 100 and the second nanofiber 200 are free radical polymerization monomers and cross-linking agents, respectively. The first nanofiber 100 and the second nanofiber 200 can release free radical polymerization monomers and cross-linking agents after being broken. After the free radical polymerization monomers and the cross-linking agents meet, a cross-linking reaction can occur and solidify to form a repair material to repair the damaged portion.
[0080] Calculated by mass ratio, the mass ratio of the core layer:shell layer in the first nanofiber 100 and the second nanofiber 200 is 1:0.4; wherein, the core layer component of the first nanofiber 100 and the core layer component of the second nanofiber 200 are dicyclopentadiene monomer and a crosslinking agent, respectively; and the shell layer of the first nanofiber 100 and the second nanofiber 200 is polyimide.
[0081] The above-mentioned highly heat-resistant self-repairing nanofiber membrane is prepared by a coaxial electrospinning method, which specifically includes the following steps:
[0082] (1) adding polyimide to DMA (dimethylacetamide) and stirring magnetically until the mixture is completely dissolved to obtain a shell spinning solution;
[0083] (2) adding dicyclopentadiene to DMA (dimethylacetamide) to prepare a first core layer 120 spinning solution, and adding tri(ethylene glycol) diazide formate to DMA (dimethylacetamide) to prepare a second core layer 220 spinning solution;
[0084] (3) A coaxial electrospinning device was used to prepare core-shell structured coaxial electrospinning nanofibers. The shell spinning solution was loaded into the needle tube of the outer layer solution. The first core layer 120 spinning solution and the second core layer 220 spinning solution were loaded into the needle tube of the inner layer solution for electrospinning. The voltage at both ends of the coaxial electrospinning device was set to 13.5 kV, the injection speed of the needle tube of the inner layer solution was 0.04 mL / h, the injection speed of the needle tube of the outer layer solution was 0.8 mL / h, and the vertical distance between the needle outlet and the receiver was 14 cm. Finally, a high heat-resistant self-healing nanofiber membrane was obtained on the receiver. The self-healing fibers were continuous, the diameter distribution was relatively uniform, there was a small amount of beads, and there was no leakage of the core layer material. The obtained high heat-resistant self-healing membrane was peeled off from the receiver, vacuum dried, and hot pressed at 80 ° C and 8 MPa. The final high heat-resistant self-healing membrane thickness was 5 μm.
[0085] Embodiment 2 to Embodiment 11, and Comparative Examples 1 to 7
[0086] Referring to the method provided in Example 1, Examples 2 to 10 were prepared, and the parameter settings of each example or comparative example are shown in Table 1 below.
[0087] Table 1
[0088]
[0089] The puncture resistance of the above embodiments and control examples was tested. The test method is as follows:
[0090] Before puncturing the battery membrane, the initial air permeability of the battery membrane is tested, and then the sample battery membrane and Teflon plate are placed on the puncture fixture, keeping the sample surface flat and wrinkle-free, and using a needle with a cross-sectional area of 0.5mm, press the battery membrane with a force of 2N for 5s to complete the puncture; after the battery membrane is punctured, the air permeability of the battery membrane is measured again. If the air permeability of the battery membrane can be improved before and after puncture, it means that the sample has good self-healing performance.
[0091] Air permeability test: The air permeability value of the diaphragm is tested with reference to the air permeability test method described in GB / T 458-2008. During the test, three samples are taken for testing using an air permeability meter, and the average value of the measurements is taken as the air permeability value.
[0092] Heat shrinkage test: Heat shrinkage: The test method is carried out in accordance with GB / T 12027-2004. Take 3 samples greater than or equal to 100mm×100mm and measure the size before heating. The samples are sandwiched between A4 papers and placed in an oven. After the set time is reached, take out and measure the size after heating, and calculate the heat shrinkage according to the formula.
[0093] Film rupture temperature test: Cut the sample into 80mm*4mm size; test the sample using a static thermomechanical analyzer under nitrogen atmosphere, with a tensile force of 0.03N, a heating rate of 5℃ / min, and a termination temperature of 400℃. Select the measured TMA curve, with temperature as the horizontal coordinate and deformation as the vertical coordinate. When the vertical coordinate direction variable of the curve is the maximum, the temperature on the horizontal coordinate at this time is the film rupture temperature.
[0094] The specific test results are shown in Table 2.
[0095] Table 2
[0096]
[0097] It can be seen from the above table that the high heat-resistant self-repairing membrane provided in the above embodiment has an initial air permeability value related to the core-shell ratio, the electrostatic spinning voltage, the distance from the transmitter to the receiver, and the hot pressing pressure. When the core layer ratio is high, the membrane air permeability, mechanical strength, and heat resistance deteriorate; when the spinning voltage is too low, due to insufficient electric field strength, it is difficult to overcome the surface tension of the spinning solution itself, resulting in insufficient stretching and splitting of the spinning solution in the electric field. Therefore, the prepared nanofibers have a larger diameter, and there may be uneven fiber diameters, rough surfaces, and even beaded fibers. When the spinning voltage is too high, the electric field strength is too large, which increases the jet volume of the spinning solution and speeds up the injection speed, which may cause the jet to be stretched excessively in the electric field, increase the fiber diameter, and deteriorate the uniformity. Due to the increase in fiber diameter and the decrease in uniformity, the mechanical properties of the formed membrane are reduced. When the distance between the receiver and the transmitter is too short, the flight time of the spinning jet in the electric field is reduced, and the solvent is not fully evaporated, which may cause the fibers to still contain a lot of solvent when they are deposited, thus forming beaded fibers or fiber bundles with collapsed structures and bonded together. Too long a distance may also cause the jet to be subject to more air resistance and disturbances during flight, making the distribution of the fibers on the receiving device uneven, and even causing the fibers to break or fail to be collected. The uneven distribution of the fibers will result in poor air permeability, porosity, and mechanical properties of the formed spinning membrane. However, too low a hot pressing pressure is not conducive to the formation of a dense and flat diaphragm. Too low a pressure will cause the fibers to stick excessively and block the pores, and will also cause the coaxial nanofibers to rupture and the diaphragm porosity to decrease.
[0098] The above specific examples are used to illustrate the present application, which is only used to help understand the present application and is not intended to limit the present application. For technicians in the technical field to which the present application belongs, they can also make some simple deductions, deformations or substitutions based on the ideas of the present application.
Claims
1. Highly heat-resistant self-repairing diaphragm, characterized in that: The diaphragm includes coaxial electrospun nanofibers of a core-shell structure; the nanofibers form a porous network structure; the nanofibers include a first nanofiber and a second nanofiber, the first nanofiber includes a first shell layer and a first core layer, the first shell layer is coated on the outside of the first core layer; the second nanofiber includes a second shell layer and a second core layer, the second shell layer is coated on the outside of the second core layer.
2. The high heat-resistant self-repairing diaphragm according to claim 1, characterized in that: The first core layer includes free radical polymerizable monomers; the second core layer includes a crosslinking agent, and the crosslinking agent can induce crosslinking of the free radical polymerizable monomers.
3. The high heat-resistant self-repairing diaphragm according to claim 2, characterized in that: The free radical polymerization monomer includes at least one of dicyclopentadiene, isoprene, methyl methacrylate, polydiethoxysiloxane, terminal hydroxylated polydimethylsiloxane and N,N-methylenebisacrylamide.
4. The high heat-resistant self-repairing diaphragm according to claim 2, characterized in that: The cross-linking agent includes at least one of Grubbs catalyst, di-n-butyltin dilaurate, tungsten hexachloride phenylacetylene mixture and azide.
5. The high heat-resistant self-repairing diaphragm according to any one of claims 1 to 4, characterized in that: The first shell layer and / or the second shell layer comprises a high temperature resistant polymer material, and the high temperature resistant polymer material comprises at least one of polyimide, polyarylethersulfoneketone, polyetherimide, polyphenylsulfone, polyisophthalamide and the like.
6. The high heat-resistant self-repairing diaphragm according to claim 1, characterized in that: The diaphragm satisfies at least one of the conditions (1) to (6): (1) The diameter of the first nanofiber and / or the second nanofiber is 0.2 μm-2.0 μm; (2) The mass ratio of the first nanofiber to the second nanofiber is 1:1; (3) In the first nanofiber, the mass ratio of the first core layer to the first shell layer is 1:0.4-1:2.0; (4) In the second nanofiber, the mass ratio of the second core layer to the second shell layer is 1:0.4-1:2.0; (5) The thickness d of the diaphragm is in the range of 3 μm ≤ d ≤ 100 μm; (6) The porosity of the diaphragm is 30%-60%.
7. A method for preparing a highly heat-resistant self-repairing diaphragm, used for preparing the diaphragm according to any one of claims 1 to 6, characterized in that: The following steps are involved: Dissolving the materials for preparing the first shell layer and the second shell layer in a solvent according to a preset ratio, and stirring and mixing them evenly to obtain a shell layer spinning solution; Dissolving the material for preparing the first core layer in a solvent according to a preset ratio, and stirring and mixing to obtain a first core layer spinning solution; Dissolving the material for preparing the second core layer in a solvent according to a preset ratio, and stirring and mixing to obtain a second core layer spinning solution; The shell layer spinning solution, the first core layer spinning solution and the second core layer spinning solution are used as electrospinning solutions, and a highly heat-resistant self-repairing nanofiber membrane having a porous network structure including first nanofibers and second nanofibers is obtained on a receiver by a coaxial electrospinning method; After the high heat-resistant self-repairing nanofiber membrane is vacuum-dried, it is hot-pressed under preset conditions to obtain the high heat-resistant self-repairing nanofiber membrane.
8. The method for preparing a highly heat-resistant self-repairing diaphragm according to claim 7, characterized in that: The diaphragm satisfies at least one of the conditions (1) to (3): (1) The first core layer includes free radical polymerizable monomers; Optionally, the free radical polymerization monomer includes at least one of dicyclopentadiene, isoprene, methyl methacrylate, polydiethoxysiloxane, terminal hydroxylated polydimethylsiloxane and N,N-methylenebisacrylamide; (2) the second core layer includes a crosslinking agent, and the crosslinking agent can induce crosslinking of the free radical polymerization monomer; Optionally, the cross-linking agent includes at least one of Grubbs catalyst, di-n-butyltin dilaurate, tungsten hexachloride phenylacetylene mixture and azide; (3) Both the first shell layer and the second shell layer are made of a high temperature resistant polymer material; Optionally, the high temperature resistant polymer material includes at least one of polyimide, polyarylethersulfoneketone, polyetherimide, polyphenylsulfone, polyisophthalamide and the like.
9. The method for preparing a highly heat-resistant self-repairing diaphragm according to claim 7 or 8, characterized in that: The diaphragm satisfies at least one of the conditions (1) to (8): (1) In the shell layer spinning solution, the mass percentage of the material for preparing the first shell layer and the second shell layer is 5wt.%-30wt.%; (2) In the first core layer spinning solution, the mass percentage of the material for preparing the first core layer is 5wt.%-30wt.%; (3) In the second core layer spinning solution, the mass percentage of the material for preparing the second core layer is 5wt.%-30wt.%; (4) The coaxial electrospinning method includes preparing the diaphragm by using a transmitter and a receiver in combination under the action of an electric field, the voltage of the electric field is 10kV-20kV, the distance between the transmitter and the receiver is 10cm-20cm, the injection rate of the shell layer spinning solution is 0.5mL / h-1.0mL / h, and the injection rate of the first core layer spinning solution and / or the second core layer spinning solution is 0.05mL / h-1.0mL / h; (5) The thickness d of the diaphragm is in the range of 3 μm ≤ d ≤ 100 μm; (6) The mass ratio of the first nanofiber to the second nanofiber is 1:1; (7) The diameters of the first nanofiber and the second nanofiber are both 0.2 μm-2.0 μm; (8) The preset conditions during hot pressing include hot pressing temperature and hot pressing pressure. The hot pressing temperature ranges from 40°C to 100°C, and the hot pressing pressure ranges from 5MPa to 20MPa.
10. A secondary battery, characterized in that: The invention comprises a diaphragm according to any one of claims 1 to 6 or a diaphragm prepared by the preparation method according to any one of claims 7 to 9.
Citation Information
Patent Citations
C / C coaxial nano-fiber composite membrane cathode material for lithium battery and preparation method thereof
CN101969123A
Lithium battery diaphragm prepared by coaxial parallel electrospinning, method and application
CN117219955A