Aerogel slurry as well as preparation method and application thereof

By using aerogel slurry prepared by aerogel powder that controls particle size, thermal conductivity and specific surface area, the problems of complex composition and poor thermal insulation performance of lithium-ion battery separator coating materials are solved, and the weight loss of battery separator is achieved and the thermal insulation performance improves the safety and performance of the battery cell.

CN118920019AActive Publication Date: 2024-11-08CNCEC HUALU NEW MATERIALS CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411191820.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-11-08
Estimated Expiration
2044-08-28

AI Technical Summary

Technical Problem

The existing lithium-ion battery separator coating composition is complex, resulting in poor weight reduction effect and insufficient thermal insulation performance of the battery separator.

Method used

Aerogel slurry composed of aerogel powder, dispersant, defoaming agent and film-forming substance are used to control the particle size, thermal conductivity, specific surface area and moisture absorption rate of the aerogel powder, and obtained through a simple preparation method. Lightweight thermally insulated coating material.

Benefits of technology

The weight reduction and thermal insulation performance of the battery separator are improved, the safety and performance of the battery cell are improved, the occurrence of battery short circuits is avoided, and the preparation cost is reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005015314260000051
    Figure BDA0005015314260000051
  • Figure HDA0005015314270000011
    Figure HDA0005015314270000011
  • Figure HDA0005015314270000012
    Figure HDA0005015314270000012
Patent Text Reader

Abstract

The invention discloses aerogel slurry as well as a preparation method and application thereof, and the aerogel slurry comprises the following components in parts by mass: 20-50 parts of aerogel powder, 3-6 parts of a dispersing agent, 8-12 parts of a defoaming agent, 120-200 parts of a film-forming substance and 250-350 parts of water. When the aerogel slurry is used for the battery diaphragm, under the coating condition of the same thickness, the weight increment of the diaphragm coated with the aerogel powder is smaller, and the mass energy density of a subsequent battery cell is improved; the weight reduction of the battery diaphragm is realized under the condition of ensuring the battery performance; and the heat insulation performance of the diaphragm is remarkably improved, and the heat-sensitive diaphragm is better protected, so that the safety of the battery cell is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of aerogels, and in particular to an aerogel slurry and a preparation method and application thereof. Background Art

[0002] Lithium-ion battery separator is one of the key components of lithium-ion batteries, and its performance directly affects the battery's capacity, cycle performance, safety and other characteristics. The separator substrate is prone to shrinkage when heated, causing a short circuit in the battery. Therefore, in actual use, a layer of slurry needs to be coated on the separator substrate to improve the thermal stability and safety of the separator substrate.

[0003] At present, the coating slurry used for the separator substrate is mostly prepared with ceramic powder and boehmite as raw materials. The obtained separator is heavy, which makes the battery heavy and inconvenient to transport and carry, and the thermal insulation performance is also poor. Therefore, a lightweight and thermal insulation coating material is urgently needed to solve the above problems.

[0004] Aerogel is a lightweight three-dimensional porous material with the advantages of low density, low hardness, and low thermal conductivity. It is widely used in the technical fields of thermal insulation and heat preservation. CN109244328A discloses a lithium-ion battery separator and a preparation method thereof, including a polyolefin microporous membrane and a coating slurry, wherein the coating slurry is coated on the polyolefin microporous membrane; the coating slurry is composed of the following components: 3 to 6 parts of chitosan, 5 to 10 parts of nano zinc oxide, 8 to 16 parts of nano carbon black, 4 to 8 parts of nano zirconium oxide, 8 to 16 parts of silica aerogel, 0.6 to 5 parts of amphoteric dispersant, 2 to 8 parts of amphoteric adhesive, 10 to 20 parts of aqueous acrylic emulsion, and 40 to 60 parts of deionized water. Although the coating slurry used in this technical solution adds aerogel powder as a raw material, which can reduce the weight of the slurry to a certain extent, its composition is too complex, and the weight reduction effect on the battery separator is poor, and the thermal insulation performance is also poor. Summary of the invention

[0005] In view of the above-mentioned deficiencies in the prior art, the purpose of the present invention is to provide an aerogel slurry to solve the problem that the existing aerogel slurry has too complex composition, poor weight reduction effect on battery diaphragms when used for battery diaphragms, and poor thermal insulation performance.

[0006] In order to solve the above technical problems, the technical solution adopted by the present invention is as follows:

[0007] An aerogel slurry comprises the following components by weight: 20 to 50 parts of aerogel powder, 3 to 6 parts of dispersant, 8 to 12 parts of defoamer, 120 to 200 parts of film-forming substance and 250 to 350 parts of water.

[0008] Furthermore, the aerogel powder includes silicon-based aerogel powder, alumina aerogel powder or titanium dioxide aerogel powder.

[0009] Furthermore, the particle size of the aerogel powder is 5 to 50 um. The present invention controls the particle size of the aerogel powder to be 5 to 50 um, on the one hand because the aerogel powder particles are too large, which is not conducive to coating, and on the other hand because the aerogel powder particles are too small, which may destroy the microstructure of the aerogel powder and affect the thermal insulation performance of the aerogel slurry.

[0010] Furthermore, the thermal conductivity of the aerogel powder is less than 0.016W / (m·k). The present invention controls the thermal conductivity of the aerogel powder to be less than 0.016W / (m·k) because the smaller the thermal conductivity, the better the thermal insulation performance of the produced coated diaphragm and the higher the safety of the battery core.

[0011] Furthermore, the specific surface area of ​​the aerogel powder is ≥ 600 m 2 / g. The specific surface area of ​​the aerogel powder controlled by the present invention is ≥600m 2 / g, because the larger the specific surface area, the more microporous structures of the powder, the better the intrinsic performance, and the better the porous adsorption performance of the subsequent coating, which is conducive to the adsorption of oxygen and hydrogen and avoids short circuit of the battery.

[0012] Furthermore, the mass moisture absorption rate of the aerogel powder is ≤5.0%. The present invention controls the mass moisture absorption rate of the aerogel powder to be ≤5.0% because the use of hydrophobic aerogel powder can make the aerogel powder more stable in the slurry and will not cause the physical and chemical properties of the powder to change due to the fluctuation of moisture.

[0013] Furthermore, the viscosity of the aerogel slurry is 6000 to 12000 mPa·s.

[0014] Furthermore, the film-forming substance includes pure acrylic emulsion or styrene acrylic emulsion.

[0015] The method for preparing the aerogel slurry comprises the following steps:

[0016] (1) Add the film-forming material into water and stir at a speed of 700 to 1000 r / min for 10 to 20 minutes;

[0017] (2) Add dispersant and stir for 5 to 8 minutes;

[0018] (3) adding part of the defoaming agent to the mixed solution obtained in step (2) and stirring for 5 to 8 minutes;

[0019] (4) adding aerogel powder to the mixed solution obtained in step (3) in small amounts and multiple times, then adding the remaining defoaming agent, and continuously stirring at a speed of 1000 to 1800 r / min for 2 to 3 hours;

[0020] (5) The slurry obtained in step (4) is vacuum degassed for 30 to 50 minutes to obtain an aerogel slurry.

[0021] Furthermore, the present invention provides application of the aerogel slurry in a battery separator.

[0022] Compared with the prior art, the present invention has the following beneficial effects:

[0023] 1. The aerogel slurry of the present invention is prepared with aerogel powder as a base material, water as a solvent, an aqueous surfactant as a dispersant, and supplemented with a defoamer and a film-forming substance. The obtained aerogel slurry has simple ingredients, low cost, and is easy to prepare. And because the specific gravity of aerogel powder in the aerogel slurry of the present invention is relatively large, with the assistance of other additives, the aerogel slurry of the present invention, when used for battery diaphragms, perfectly retains the characteristics of low density and excellent thermal insulation performance of aerogel powder. When used for battery diaphragms, under the coating conditions of the same thickness, the weight gain of the coated diaphragm is smaller, and the mass energy density of the subsequent battery core is improved; while ensuring the battery performance, the weight reduction of the battery diaphragm is achieved; and compared with traditional coating materials, the aerogel slurry of the present invention also significantly improves the thermal insulation performance of the diaphragm, better protects the heat-sensitive diaphragm, thereby improving the safety of the battery core.

[0024] 2. The inventors of the present invention have found that due to the large porosity of aerogel powder, when trace amounts of oxygen and hydrogen are generated at the initial stage of failure on the positive and negative electrode sides of the battery cell, the oxygen and hydrogen will be adsorbed by the aerogel powder, thereby preventing the battery from short-circuiting.

[0025] 3. The aerogel slurry of the present invention does not drop powder after being coated on the battery separator, and since the hardness of the aerogel powder is relatively low, there is no damage to the roller when the roller coating process is adopted. In addition, since the impurity content in the oxide of the aerogel is less, the side effects on the battery system are also less. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 This is a scanning electron microscope image (SEM image) of the silica aerogel powder used in Example 1;

[0027] Figure 2 This is a picture of a PP diaphragm manually coated with the slurry obtained in Example 1. DETAILED DESCRIPTION

[0028] The specific implementation modes of the present invention are further described in detail below in conjunction with specific examples.

[0029] The numerical ranges in the present invention are understood to also specifically disclose each intermediate value between the upper and lower limits of the range. Each smaller range between any intermediate value in the stated value or stated range and any other stated value or intermediate value in the stated range is also included in the present invention. The upper and lower limits of these smaller ranges may be independently included or excluded in the range.

[0030] Unless otherwise stated, all technical and scientific terms used herein have the same meanings as those of ordinary skill in the art described in the present invention are generally understood. Although the present invention only describes preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials related to the documents. In the event of conflict with any incorporated document, the content of this specification shall prevail. Regarding "comprising", "including", "having", "containing", etc. used herein, they are all open terms, which means including but not limited to.

[0031] Unless otherwise specified, the experimental methods used in the present invention are all conventional methods.

[0032] Unless otherwise specified, the materials, reagents, etc. used in the present invention can be purchased or synthesized by known methods.

[0033] The quantitative tests in the present invention were all repeated three times, and the results were averaged.

[0034] The dispersants used in the present invention are all water-based surfactants, including HL-FS-01 (manufacturer: Hualu (Tianjin) New Material Technology Co., Ltd.) or SN5040 (manufacturer: Shenzhen Yoshida Chemical Co., Ltd.). The defoamers used in the present invention include BYK-025 (manufacturer: German BYK Chemical Co., Ltd.) or 681-F (manufacturer: Linyi Kaiao Chemical Co., Ltd.).

[0035] Example 1

[0036] A method for preparing an aerogel slurry comprises the following steps:

[0037] (1) Add 150 g of styrene-acrylic emulsion to 300 g of desalted water and stir at a speed of 800 r / min for 15 min;

[0038] (2) Add 3 g SN5040 and stir for 6 min;

[0039] (3) Add 4 g of defoamer (BYK-025) to the mixed solution obtained in step (2) and stir for 6 min;

[0040] (4) Adding silica aerogel powder (particle size 25 μm, thermal conductivity 0.015 W / (m·k), specific surface area 600 m 2 / g, mass moisture absorption rate 5.0%), add 10g each time, then add 6g of defoamer (BYK-025), and continue stirring at a speed of 1400r / min for 2.5h;

[0041] Figure 1 This is a scanning electron microscope image (SEM image) of silica aerogel powder. Figure 1 It can be seen that the powder used in the experiment of this embodiment has a regular spherical morphology and good quality, and can be used for the subsequent preparation of aerogel slurry.

[0042] (5) The slurry obtained in step (4) is vacuum degassed for 30 minutes to obtain an aerogel slurry.

[0043] Viscosity test: The obtained slurry was subjected to a viscosity test, and the viscosity was 8600 mPa·s.

[0044] Preparation of diaphragm: The aerogel slurry obtained in this example is evenly coated on the PP diaphragm with a scraper with a thickness of 100 μm, and then placed at 25°C for 4 hours, and then placed in a vacuum drying oven at 60°C for 2 hours to obtain a finished battery diaphragm (such as Figure 2 ). Figure 2 It can be seen that the surface of the diaphragm coated with the slurry of the present invention has no abnormality, no flow, no accumulation, is overall flat and uniform, and the slurry coating effect is good.

[0045] Example 2

[0046] A method for preparing an aerogel slurry comprises the following steps:

[0047] (1) Add 120 g pure propylene emulsion into 250 ml of desalted water and stir at 700 r / min for 20 min;

[0048] (2) Add 5 g HL-FS-01 and stir for 5 min;

[0049] (3) Add 6 g of defoamer (681-F) to the mixed solution obtained in step (2) and stir for 5 min;

[0050] (4) Alumina aerogel powder (particle size 5 μm, thermal conductivity 0.015 W / (m·k), specific surface area 700 m2) was added to the mixed solution obtained in step (3) in three portions. 2 / g, mass moisture absorption rate 4.0%), add 15g each time, then add 4g of defoamer (681-F), and continue stirring at a speed of 1200r / min for 3h;

[0051] (5) The slurry obtained in step (4) is vacuum degassed for 40 minutes to obtain an aerogel slurry.

[0052] Viscosity test: The obtained slurry was subjected to a viscosity test, and the viscosity was 6500 mPa·s.

[0053] Preparation of diaphragm: The aerogel slurry obtained in this example is evenly coated on the PP diaphragm with a scraper with a thickness of 100 um, and after standing at 40°C for 2 hours, it is placed in a vacuum drying oven at 60°C and dried for 2 hours to obtain a finished battery diaphragm.

[0054] Example 3

[0055] A method for preparing an aerogel slurry comprises the following steps:

[0056] (1) Add 200 g of styrene-acrylic emulsion to 350 g of desalted water and stir at a speed of 1000 r / min for 10 min;

[0057] (2) Add 6 g SN5040 and stir for 8 min;

[0058] (3) Add 5 g of defoamer (BYK-025) to the mixed solution obtained in step (2) and stir for 8 min;

[0059] (4) Add titanium dioxide aerogel powder (particle size 50 μm, thermal conductivity 0.015 W / (m·k), specific surface area 600 m2) into the mixed solution obtained in step (3) in three portions; 2 / g, mass moisture absorption rate 5.0%), add 8g each time, then add 7g defoamer (BYK-025), and continue stirring at a speed of 1800r / min for 2h;

[0060] (5) The slurry obtained in step (4) is vacuum degassed for 50 minutes to obtain an aerogel slurry.

[0061] Viscosity test: The obtained slurry was subjected to a viscosity test, and the viscosity was 11000 mPa·s.

[0062] Preparation of diaphragm: The aerogel slurry obtained in this example is evenly coated on the PP diaphragm with a scraper with a thickness of 100 um, and after standing at 60°C for 30 minutes, it is placed in a 60°C vacuum drying oven and dried for 2 hours to obtain a finished battery diaphragm.

[0063] A comparison table of the weight and thermal conductivity of the battery separator obtained by the present invention, the existing battery separator, the base film (PP separator) and the viscosity of the obtained aerogel slurry is shown in Table 1.

[0064] Table 1 Comparison of density and thermal conductivity of finished battery separator and base film and viscosity of obtained aerogel slurry

[0065]

[0066] As can be seen from Table 1, compared with the existing ceramic powder oil slurry and aluminum oxide aqueous slurry, the aerogel slurry of the present invention is used to coat the substrate diaphragm, and the density of the diaphragm after coating is low, which effectively achieves the weight reduction of the battery diaphragm, thereby achieving the weight reduction of the battery; and the thermal conductivity of the diaphragm coated with the aerogel slurry of the present invention is effectively reduced, and the protective effect on the heat-sensitive diaphragm is good, thereby improving the safety of the battery cell. And the viscosity of the obtained aerogel slurry fluctuates between 6000 and 12000 mPa·s, and the fluctuation range is small, indicating that the aerogel slurry obtained by the present invention is evenly dispersed, avoiding uneven subsequent slurry coating, causing the battery cell to fail the HIPOT test.

[0067] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the technical solution. Those skilled in the art should understand that those modifications or equivalent substitutions of the technical solution of the present invention that do not depart from the purpose and scope of the technical solution should be included in the scope of the claims of the present invention.

Claims

1. An aerogel slurry, characterized in that: The composition comprises the following components by weight: 20 to 50 parts of aerogel powder, 3 to 6 parts of dispersant, 8 to 12 parts of defoamer, 120 to 200 parts of film-forming substance and 250 to 350 parts of water.

2. The aerogel slurry according to claim 1, characterized in that: The aerogel powder includes silicon-based aerogel powder, alumina aerogel powder or titanium dioxide aerogel powder.

3. The aerogel slurry according to claim 1, characterized in that: The particle size of the aerogel powder is 5 to 50 μm.

4. The aerogel slurry according to claim 1, characterized in that: The thermal conductivity of the aerogel powder is less than 0.016 W / (m·k).

5. The aerogel slurry according to claim 1, characterized in that: The specific surface area of ​​the aerogel powder is ≥600m 2 / g.

6. The aerogel slurry according to claim 1, characterized in that: The mass moisture absorption rate of the aerogel powder is ≤5.0%.

7. The aerogel slurry according to claim 1, characterized in that: The viscosity of the aerogel slurry is 6000-12000 mPa·s.

8. The aerogel slurry according to claim 1, characterized in that: The film-forming substance comprises pure acrylic emulsion or styrene acrylic emulsion.

9. The method for preparing aerogel slurry according to any one of claims 1 to 8, characterized in that: The following steps are involved: (1) Add the film-forming material into water and stir at a speed of 700 to 1000 r / min for 10 to 20 minutes; (2) Add dispersant and stir for 5 to 8 minutes; (3) adding part of the defoaming agent to the mixed solution obtained in step (2) and stirring for 5 to 8 minutes; (4) adding aerogel powder to the mixed solution obtained in step (3) in small amounts and multiple times, then adding the remaining defoaming agent, and continuously stirring at a speed of 1000 to 1800 r / min for 2 to 3 hours; (5) The slurry obtained in step (4) is vacuum degassed for 30 to 50 minutes to obtain an aerogel slurry.

10. Use of any aerogel slurry according to claims 1 to 8 in battery separators.

Citation Information

Patent Citations

  • Lithium ion battery separator and preparation method thereof

    CN109244328A

  • Solid polymer separator for lithium ion battery

    CN115552680A

  • Jet fire impact-resistant insulating heat-insulating flame-retardant coating as well as preparation method and application thereof

    CN117987000A