Structure-hysteresis-dielectric ternary loss type wave-absorbing material as well as preparation method and application thereof
By combining a structural loss hollow core, a hysteresis loss shell, and a dielectric loss fiber material into the absorbing material, the problem that existing absorbing materials cannot simultaneously possess structural, hysteresis, and dielectric loss properties is solved, achieving a multi-band compatible absorbing effect for probed waves, and making it suitable for equipment surface coatings and structural components.
Patent Information
- Application Number
- CN202410925840.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-11
- Publication Date
- 2024-11-08
AI Technical Summary
Existing absorbing materials cannot simultaneously possess structural, hysteresis, and dielectric loss functions, resulting in poor loss performance for probed waves.
A combination of a structural loss hollow core, a hysteresis loss shell, and a dielectric loss fiber material is used to form a structural-hysteresis-dielectric ternary loss absorbing material by depositing a hysteresis loss shell on the surface of the hollow core and grafting dielectric loss fiber material.
It achieves multi-band compatible absorption of probe waves, has excellent loss performance, and is suitable for equipment surface coatings and structural components, reducing the intensity of reflected waves and converting electromagnetic energy into heat energy.
Smart Images

Figure CN118920122A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of absorbing materials, and in particular relates to a structure-hysteresis-dielectric ternary lossy absorbing material and a preparation method and application thereof. Background Art
[0002] In modern high-tech warfare, maximizing the loss of detection waves (such as radar waves, infrared waves, etc.) is an effective way to achieve equipment stealth. By performing three-dimensional loss (structural dissipation, hysteresis loss and dielectric loss) on the detection waves, the absorbing materials can maximize their stealth performance. Stealth technology involves many technical fields such as electronics, materials science, acoustics, and optics. Objects achieve stealth by reducing radar cross-sectional area and reducing their own infrared radiation. The main technical approaches include using unique shape design and absorbing and transparent materials to reduce their own reflection of radar waves. Adding "thin, light, wide, and strong" (thin layer, low density, wide absorbing frequency band and strong absorbing ability) absorbing materials to the surface of equipment to achieve structural absorbing is an important way to achieve its stealth.
[0003] At present, the development of structural dissipative units with "light trapping" capabilities, and making them have both hysteresis loss and dielectric loss functions, is the main goal of preparing absorbing powder materials with stealth performance. Traditional absorbing materials are often "structure-hysteresis-dielectric" three-dimensional discrete. However, when it has a stealth absorbing layer structure, it is often difficult to add hysteresis and dielectric capabilities to the material; ferromagnetic absorbing materials require a very thick coating when achieving hysteresis loss. Although the hysteresis loss is obvious, the dielectric loss is very weak; when using conductive fibers for dielectric loss, the material has almost no hysteresis loss capability.
[0004] In summary, the existing absorbing materials are difficult to overcome due to the contradictions of the three constraints of "structure-hysteresis-dielectric", resulting in poor loss effect of the absorbing materials on the detection waves. Summary of the invention
[0005] The purpose of the present invention is to provide a structure-hysteresis-dielectric ternary lossy absorbing material and a preparation method and application thereof. The structure-hysteresis-dielectric ternary lossy absorbing material provided by the present invention has excellent loss effect on detection waves.
[0006] In order to achieve the above object, the present invention provides the following technical solutions:
[0007] The invention provides a structural-hysteresis-dielectric ternary lossy absorbing material, comprising a structural lossy hollow core, a hysteresis lossy shell wrapped on the surface of the structural lossy hollow core, and a dielectric lossy fiber material grafted on the surface of the hysteresis lossy shell.
[0008] Preferably, the structural lossy hollow core comprises hollow glass microspheres.
[0009] Preferably, the thickness of the structural loss hollow core is 1 to 2 μm, and the outer diameter is 10 to 250 μm;
[0010] The structural loss hollow core is filled with one or more of air, nitrogen and inert gas.
[0011] Preferably, the hysteresis loss shell layer includes one or more of nickel-zinc ferrite, manganese-zinc ferrite and barium ferrite.
[0012] Preferably, the thickness of the hysteresis loss shell layer is 20 to 50 μm;
[0013] The ratio of the diameter of the structural loss hollow core to the thickness of the hysteresis loss shell is 10-250:20-50.
[0014] Preferably, the dielectric loss fiber material includes one or more of carbon nanotubes, carbon fibers and zinc oxide whiskers.
[0015] Preferably, the diameter of the dielectric loss fiber material is 2 to 30 nm;
[0016] The ratio of the length of the dielectric loss fiber material to the thickness of the hysteresis loss shell layer is 50-100:20-50.
[0017] The present invention provides a method for preparing the structure-hysteresis-dielectric ternary lossy absorbing material described in the above technical solution, comprising the following steps:
[0018] Depositing a hysteresis loss shell layer on the surface of the structural loss hollow core to obtain an absorbing material intermediate;
[0019] The dielectric loss fiber material is grafted onto the surface of the absorbing material intermediate to obtain the structure-hysteresis-dielectric ternary lossy absorbing material.
[0020] Preferably, the deposition includes one or more of chemical plating deposition, electroplating deposition and vapor deposition;
[0021] The grafting includes one or more of arc discharge grafting, chemical vapor grafting and laser evaporation grafting.
[0022] The present invention provides the use of the structure-hysteresis-dielectric ternary lossy absorbing material described in the above technical solution or the structure-hysteresis-dielectric ternary lossy absorbing material prepared by the preparation method described in the above technical solution in equipment surface coatings or structural parts.
[0023] The present invention provides a structural-hysteresis-dielectric ternary loss-type absorbing material, comprising a structural loss hollow core, a hysteresis loss shell wrapped on the surface of the structural loss hollow core, and a dielectric loss fiber material grafted on the surface of the hysteresis loss shell. The absorbing material provided by the present invention is similar to the "spherical thorns" microstructure of the new coronavirus strain. The mechanism for realizing the function of the absorbing material is: when the incident electromagnetic wave passes through the structural loss hollow core, refraction and scattering occur, and the intensity of the reflected wave is greatly reduced, achieving the purpose of structural loss; when the incident electromagnetic wave passes through the hysteresis loss shell, hysteresis loss occurs, and the electromagnetic energy is converted into heat energy and dissipated, achieving the purpose of magnetic loss; when the incident electromagnetic wave passes through the dielectric loss fiber material, it is affected by impedance, and the electromagnetic energy is converted into heat energy, achieving the purpose of electrical loss. The structural-hysteresis-dielectric ternary loss-type absorbing material provided by the present invention has the "structural-hysteresis-dielectric" ternary loss function at the same time, and is a new type of multi-band compatible absorbing material with energy concentration and selection, and has excellent loss effect on detection waves. The present invention provides a structural-hysteresis-dielectric ternary lossy absorbing material which can be used as a structural material to fill a structural part and become a component of a load-bearing structural part; it can also be used as a coating absorbing additive to play a loss function on the detection wave and be applied to the surface coating of equipment to achieve equipment stealth.
[0024] The preparation method of the structure-hysteresis-dielectric ternary loss-type absorbing material provided by the present invention performs adaptive assembly for the structural matching, impedance matching, and attenuation matching of the detection wave, first deposits a hysteresis loss shell layer on the surface of the structural loss hollow core to obtain an absorbing material intermediate, and realizes the "structure-hysteresis" double loss; then grafts a dielectric loss fiber material on the surface of the absorbing material intermediate to obtain the structure-hysteresis-dielectric ternary loss-type absorbing material, and realizes the "structure-hysteresis-dielectric" ternary loss of the absorbing material. Moreover, the preparation method provided by the present invention is simple to operate, low in cost, and suitable for industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 It is a schematic diagram of the functional realization principle of multiple structure-hysteresis-dielectric ternary lossy absorbing materials;
[0026] Figure 2 It is a schematic diagram of the functional realization principle of a single structure-hysteresis-dielectric ternary lossy absorbing material;
[0027] Figure 3 This is the principle diagram of "light trapping" of hollow glass microspheres;
[0028] Figure 4 This is a schematic diagram of the hysteresis loss principle of the nickel-zinc ferrite hysteresis loss layer on the surface of nickel-plated hollow glass microspheres;
[0029] Figure 5 It is a schematic diagram of the structure of a structural-hysteresis-dielectric ternary lossy absorbing material;
[0030] Figure 6 This is a microscopic schematic diagram of the structure-hysteresis-dielectric ternary lossy absorbing material prepared in Example 1;
[0031] Figure 7 This is a graph showing the thermal insulation performance of nickel-plated hollow glass microsphere coating;
[0032] Figure 8 This is the hysteresis loss diagram of nickel-plated hollow glass microsphere coating;
[0033] Fig. 9 The dielectric loss diagram of nickel-plated hollow glass microsphere coating;
[0034] Fig.10 This is the reflectivity graph of nickel-plated hollow glass microsphere coating;
[0035] Fig.11 This is the reflectivity diagram of the structural-hysteresis-dielectric ternary lossy absorbing material coating. DETAILED DESCRIPTION
[0036] The invention provides a structural-hysteresis-dielectric ternary lossy absorbing material, comprising a structural lossy hollow core, a hysteresis lossy shell wrapped on the surface of the structural lossy hollow core, and a dielectric lossy fiber material grafted on the surface of the hysteresis lossy shell.
[0037] In the present invention, unless otherwise specified, the materials used are commercially available products well known to those skilled in the art.
[0038] In the present invention, the structural loss hollow core preferably includes hollow glass microspheres; the hollow glass microspheres preferably include borosilicate hollow glass microspheres, more preferably high-boron low-silicon hollow glass microspheres; the composition of the borosilicate hollow glass microspheres preferably includes SiO 2 , B 2 O 3 、Na 2 O、Al 2 O 3 , BaO and CaO.
[0039] In the present invention, the structural loss hollow core is preferably filled with one or more of air, nitrogen and inert gas; the inert gas preferably includes argon. In the present invention, the thickness of the structural loss hollow core is preferably 1-2 μm, more preferably 1.2-1.8 μm, and most preferably 1.4-1.6 μm; the outer diameter of the structural loss hollow core is preferably 10-250 μm, more preferably 50-200 μm, and most preferably 100-150 μm; the ratio of the thickness to the diameter of the structural loss hollow core is preferably 1:10-100, more preferably 1:15-80, and most preferably 1:20-50. In the present invention, the hollow part in the structural loss hollow core is preferably spherical. The diameter of the structural loss hollow core used in the present invention is 10 to 250 μm. After a certain thickness of nickel-zinc ferrite and dielectric loss fiber material (such as carbon nanotube) coating is plated on its surface, it has a dissipation function for detection waves of different bands. Moreover, the hollow glass microspheres used in the present invention have a heat insulation effect and can have a lossy stealth effect in multiple bands such as infrared and millimeter waves. The obtained structural-hysteresis-dielectric ternary lossy absorbing material can fully cover multiple detection bands including thermal infrared, centimeter waves and millimeter waves, and has good absorbing capabilities for the most commonly used bands for search (warning) radars and tracking radars, namely, the 1 to 18 GHz band and the millimeter wave band in the frequency range of 30 to 300 GHz.
[0040] In the present invention, the hysteresis loss shell preferably includes one or more of nickel zinc ferrite, manganese zinc ferrite and barium ferrite. In the present invention, the thickness of the hysteresis loss shell is preferably 20-50 μm, more preferably 25-40 μm, and most preferably 30-35 μm; the ratio of the diameter of the structural loss hollow core to the thickness of the hysteresis loss shell is preferably 10-250:20-50, more preferably 50-200:25-40, and most preferably 100-150:30-35.
[0041] In the present invention, the dielectric loss fiber material preferably includes one or more of carbon nanotubes, carbon fibers and zinc oxide whiskers; the diameter of the dielectric loss fiber material is preferably 2 to 30 nm, more preferably 10 to 20 nm, and most preferably 15 to 18 nm; the ratio of the length of the dielectric loss fiber material to the thickness of the hysteresis loss shell is preferably 50 to 100:20 to 50, more preferably 60 to 80:25 to 40, and most preferably 70 to 75:30 to 35. The present invention does not specifically limit the distance between the centers of two adjacent dielectric loss fiber materials, and the distance well known in the art can be used.
[0042] In the embodiments of the present invention, the wall thickness of the hollow glass microspheres used is only 5% of the diameter of the hollow glass microspheres, and the material is a large ball thin shell structure. The carbon nanotubes are typical lightweight whisker materials, and the thickness of the ferromagnetic layer is small. The density of the obtained structure-hysteresis-dielectric ternary lossy absorbing material is very low, which is only 1 / 15 of that of aluminum alloy and about 1 / 3 to 1 / 2 of that of aviation paint layer, and will not have a negative impact on the density of the skin paint layer.
[0043] The present invention provides a method for preparing the structure-hysteresis-dielectric ternary lossy absorbing material described in the above technical solution, comprising the following steps:
[0044] Depositing a hysteresis loss shell layer on the surface of the structural loss hollow core to obtain an absorbing material intermediate;
[0045] The dielectric loss fiber material is grafted onto the surface of the absorbing material intermediate to obtain the structure-hysteresis-dielectric ternary lossy absorbing material.
[0046] The invention deposits a hysteresis loss shell layer on the surface of a structural loss hollow inner core to obtain a wave absorbing material intermediate.
[0047] In the present invention, the deposition preferably includes one or more of chemical plating deposition, electroplating deposition and vapor deposition. The present invention has no special limitation on the deposition conditions, as long as the hysteresis loss shell layer can be deposited on the surface of the structural loss hollow core.
[0048] After obtaining the absorbing material intermediate, the present invention grafts a dielectric loss fiber material onto the surface of the absorbing material intermediate to obtain the structure-hysteresis-dielectric ternary lossy absorbing material.
[0049] In the present invention, the grafting preferably includes one or more of arc discharge grafting, chemical vapor grafting and laser evaporation grafting. The present invention has no special restrictions on the grafting conditions, as long as the dielectric loss fiber material can be grafted on the surface of the absorbing material intermediate.
[0050] The present invention provides the application of the structure-hysteresis-dielectric ternary lossy absorbing material described in the above technical solution or the structure-hysteresis-dielectric ternary lossy absorbing material prepared by the preparation method described in the above technical solution in equipment surface coatings or structural parts. In the present invention, the application wavelength range of the structure-hysteresis-dielectric ternary lossy absorbing material preferably includes 1 to 18 GHz and / or 30 to 300 GHz. The structure-hysteresis-dielectric ternary lossy absorbing material provided by the present invention can be dispersed in the coating as an absorbing powder, and can play the role of dissipating the detection wave as a coating absorbing additive. Under the protection of the outermost protective layer, the absorbing powder is basically not eroded by the airflow, and can maintain a stable structural state in the coating; it can also be filled into the structural part as a structural material. On the one hand, the powder can be filled into a polymer material (such as a carbon fiber plate) to become a component of an aviation structural part, and the function is similar to that added to the coating; on the other hand, the powder can be filled into the hollow structure or gap of the aviation structural part, which can weaken the reflection intensity of the detection wave and play an absorbing effect.
[0051] In order to further illustrate the present invention, a structural-hysteresis-dielectric ternary lossy absorbing material provided by the present invention and its preparation method and application are described in detail below in combination with the accompanying drawings and embodiments, but they should not be understood as limiting the scope of protection of the present invention.
[0052] Example 1
[0053] A nickel-zinc ferrite hysteresis loss layer is deposited on the surface of the hollow glass microspheres by a hydrothermal chemical plating method, and after heat treatment at 450° C., nickel-plated hollow glass microspheres are obtained (the content of nickel in the nickel-zinc ferrite hysteresis loss layer is 95.71%), wherein the wall thickness of the hollow glass microspheres is 1.5±0.3 μm, the diameter is 100±30 μm, the wall thickness accounts for 1.5% of the diameter, and the hollow glass microspheres are filled with nitrogen gas; the thickness of the nickel-zinc ferrite hysteresis loss layer is 35±5 μm;
[0054] The chemical vapor grafting method was used to graft multi-walled carbon nanotubes onto the surface of nickel-plated hollow glass microspheres to obtain a structural-hysteresis-dielectric ternary lossy absorbing material. The structural schematic diagram is shown in Figure 5 As shown, the length of the multi-walled carbon nanotubes is 30±5μm and the diameter is 20±5nm.
[0055] Figure 1 It is a schematic diagram of the functional realization principle of multiple structure-hysteresis-dielectric ternary lossy absorbing materials; Figure 2 It is a schematic diagram of the functional realization principle of a single structure-hysteresis-dielectric ternary lossy absorbing material; Figure 3 This is the principle diagram of "light trapping" of hollow glass microspheres; Figure 4 This is a schematic diagram of the hysteresis loss principle of the nickel-zinc ferrite hysteresis loss layer on the surface of nickel-plated hollow glass microspheres; Figure 5 The schematic diagram of the structure of the structural-hysteresis-dielectric ternary lossy absorbing material is shown in FIG. Figure 1 to Figure 5 It can be seen that the mechanism for realizing the function of the structural-hysteresis-dielectric ternary lossy absorbing material provided by the present invention is as follows: when the incident electromagnetic wave passes through the structural loss hollow core, refraction and scattering occur, and the intensity of the reflected wave is greatly reduced, thereby achieving the purpose of structural loss; when the incident electromagnetic wave passes through the hysteresis loss shell, hysteresis loss occurs, and the electromagnetic energy is converted into heat energy and dissipated, thereby achieving the purpose of magnetic loss; when the incident electromagnetic wave passes through the dielectric loss fiber material, it is affected by impedance, and the electromagnetic energy is converted into heat energy (and electrical energy), thereby achieving the purpose of electrical loss (conductivity loss).
[0056] Figure 6 The microscopic diagram of the structure-hysteresis-dielectric ternary lossy absorbing material prepared in Example 1 is shown in FIG. Figure 6 It can be seen that the surface of the hollow glass microspheres is evenly covered with a relatively complete "nickel-zinc ferrite hysteresis loss layer + carbon nanotubes". The spherical structure of the hollow microspheres did not undergo structural changes during the grafting process of the nickel-zinc ferrite hysteresis loss layer and the carbon nanotubes. Since the hollow glass microspheres undergo two chemical reaction processes of hydrothermal chemical plating and chemical vapor grafting, the final structure-hysteresis-dielectric ternary loss-type absorbing material powder contains detached nickel-zinc ferrite hysteresis loss layer and carbon nanotube impurities.
[0057] The obtained nickel-plated hollow glass microspheres and PVC adhesive are dispersed and mixed, and cured at 140° C. to obtain a nickel-plated hollow glass microsphere coating, wherein the mass percentage of the nickel-plated hollow glass in the nickel-plated hollow glass microsphere coating is 0%, 8%, 12%, 16%, 20% and 30% respectively.
[0058] Figure 7 The thermal insulation performance diagram of nickel-plated hollow glass microsphere coating is shown in Figure 1. Figure 7 It can be seen that hollow glass microspheres have good thermal insulation properties. When the mass percentage of nickel-plated hollow glass in PVC adhesive is 16%, the temperature reduction difference compared with the PVC material with 8% filling amount reaches 4.3℃.
[0059] Figure 8 is the hysteresis loss diagram of nickel-plated hollow glass microsphere coating, Figure 8 It can be seen that within 2 to 18 GHz, when the mass percentage of nickel-plated hollow glass in the PVC adhesive is 16%, the magnetic loss gradually decreases, proving that the nickel-plated glass microbeads prepared in Example 1 have certain soft magnetic properties.
[0060] Fig. 9 The dielectric loss diagram of nickel-plated hollow glass microsphere coating is shown in Figure 2. Fig. 9It can be seen that within the range of 2 to 18 GHz, when the mass percentage of nickel-plated hollow glass in PVC adhesive reaches 12%, the increase in the electrical loss factor of nickel-plated hollow glass microspheres is no longer obvious; when the mass percentage of nickel-plated hollow glass in PVC adhesive reaches 16%, sufficient mutual contact has been achieved in the matrix to form a stable conductive network.
[0061] Fig.10 The reflectivity graph of the nickel-plated hollow glass microsphere coating is the reflectivity graph of the nickel-plated hollow glass microspheres prepared in Examples 1 to 4 and Comparative Example 1. Fig.10 It can be seen that within the range of 2 to 18 GHz, when the mass percentage of nickel-plated hollow glass in PVC adhesive is 16%, the band in which the average reflectivity of the nickel-plated hollow glass microbeads is less than -2dB is 10 GHz, and the frequency band is wide.
[0062] The obtained structure-hysteresis-dielectric ternary lossy absorbing material and PVC adhesive were dispersed and mixed, and cured at 140° C. to obtain a structure-hysteresis-dielectric ternary lossy absorbing material coating. The mass percentages of the structure-hysteresis-dielectric ternary lossy absorbing material in the structure-hysteresis-dielectric ternary lossy absorbing material coating were 0%, 10%, 17%, 22.5% and 28%, respectively.
[0063] Fig.11 is the reflectivity diagram of the structure-hysteresis-dielectric ternary lossy absorbing material coating, Fig.11 It can be seen that after carbon nanotubes are grafted on the surface of nickel-plated hollow glass microspheres, the absorbing performance of the absorbing material is significantly improved, and the maximum reflectivity is increased from -4.25dB (nickel-plated hollow glass microspheres) to -12.5dB (structural-hysteresis-dielectric ternary lossy absorbing material).
[0064] In summary, the nickel-plated hollow glass microspheres provided by the present invention have a "structure-hysteresis" ternary loss function. When the incident electromagnetic wave passes through the structural loss hollow core, it is refracted and scattered, and the intensity of the reflected wave is greatly reduced, achieving the purpose of structural loss; when the incident electromagnetic wave passes through the hysteresis loss shell, hysteresis loss occurs, and the electromagnetic energy is converted into heat energy and dissipated, achieving the purpose of magnetic loss. After the carbon nanotubes are grafted on the surface of the nickel-plated hollow glass microspheres, the resulting structure-hysteresis-dielectric ternary loss type wave absorbing material simultaneously possesses the "structure-hysteresis-dielectric" ternary loss function, and is a new type of multi-band compatible wave absorbing material with energy concentration and selection, and has excellent loss effect on the detection wave. When the incident electromagnetic wave passes through the structural loss hollow core, it is refracted and scattered, and the intensity of the reflected wave is greatly reduced; when passing through the hysteresis loss shell, hysteresis loss occurs, and the electromagnetic energy is converted into heat energy and dissipated; when passing through the dielectric loss fiber material, it is affected by impedance, and the electromagnetic energy is converted into heat energy. Therefore, according to different wave absorbing requirements, different structures and material combinations can be adopted to obtain the optimal wave absorbing effect for the detection wave.
[0065] Although the above-mentioned embodiments have made a detailed description of the present invention, they are only some embodiments of the present invention, rather than all embodiments. People can also obtain other embodiments based on the embodiments of the present invention without creative work, and these embodiments all fall within the scope of protection of the present invention.
Claims
1. A structural-hysteresis-dielectric ternary lossy absorbing material, characterized in that: The invention comprises a structural loss hollow core, a hysteresis loss shell layer wrapped on the surface of the structural loss hollow core, and a dielectric loss fiber material grafted on the surface of the hysteresis loss shell layer.
2. The structure-hysteresis-dielectric ternary lossy absorbing material according to claim 1, characterized in that: The structural lossy hollow core includes hollow glass microspheres.
3. The structural-hysteresis-dielectric ternary lossy absorbing material according to claim 1 or 2, characterized in that: The wall thickness of the structural loss hollow core is 1 to 2 μm, and the outer diameter is 10 to 250 μm; The structural loss hollow core is filled with one or more of air, nitrogen and inert gas.
4. The structure-hysteresis-dielectric ternary lossy absorbing material according to claim 1, characterized in that: The hysteresis loss shell layer includes one or more of nickel-zinc ferrite, manganese-zinc ferrite and barium ferrite.
5. The structural-hysteresis-dielectric ternary lossy absorbing material according to claim 1 or 4, characterized in that: The thickness of the hysteresis loss shell layer is 20 to 50 μm; The ratio of the diameter of the structural loss hollow core to the thickness of the hysteresis loss shell is 10-250:20-50.
6. The structure-hysteresis-dielectric ternary lossy absorbing material according to claim 1, characterized in that: The dielectric loss fiber material includes one or more of carbon nanotubes, carbon fibers and zinc oxide whiskers.
7. The structural-hysteresis-dielectric ternary lossy absorbing material according to claim 1 or 6, characterized in that: The diameter of the dielectric loss fiber material is 2 to 30 nm; The ratio of the length of the dielectric loss fiber material to the thickness of the hysteresis loss shell layer is 50-100:20-50.
8. The method for preparing the structure-hysteresis-dielectric ternary lossy absorbing material according to any one of claims 1 to 7, characterized in that: The following steps are involved: Depositing a hysteresis loss shell layer on the surface of the structural loss hollow core to obtain an absorbing material intermediate; The dielectric loss fiber material is grafted onto the surface of the absorbing material intermediate to obtain the structure-hysteresis-dielectric ternary lossy absorbing material.
9. The preparation method according to claim 8, characterized in that: The deposition includes one or more of chemical plating deposition, electroplating deposition and vapor deposition; The grafting includes one or more of arc discharge grafting, chemical vapor grafting and laser evaporation grafting.
10. Use of the structure-hysteresis-dielectric ternary lossy absorbing material according to any one of claims 1 to 7 or the structure-hysteresis-dielectric ternary lossy absorbing material prepared by the preparation method according to any one of claims 8 to 9 in coatings or structural parts.
Citation Information
Cited By
Wave absorbing structure, supporting system and target radar cross section testing system
CN120728257A