Preparation method and application of flexible liquid crystal elastomer laser

Flexible liquid crystal elastomer lasers prepared by combining liquid crystal monomers and chiral initiators, combined with laser dyes, achieve high tensile strain and wavelength regulation, solving the problem of failure to prepare tunable random lasers in the prior art, and are suitable for A variety of advanced application scenarios.

CN118920248APending Publication Date: 2024-11-08ANHUI UNIV
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202410963324.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The prior art has failed to produce tunable random lasers, and the application of liquid crystal elastomers in lasers has not been explored.

Method used

Using a combination of liquid crystal monomer, chiral initiator, thiol crosslinker, chain extender, photoinitiator and catalyst, the Michael addition reaction and ultraviolet curing, it can prepare high tensile strain and reversible color distortion through the use of Michael addition reaction and ultraviolet curing. The flexible liquid crystal elastomer laser combines laser dye to achieve dynamic wavelength regulation.

Benefits of technology

It has achieved high tensile strain (up to 795%), reversible structural color change and large-scale laser wavelength regulation (560-750nm) of flexible liquid crystal elastomer lasers, and is suitable for wearable technology and human-computer interactive interfaces and other fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118920248A_ABST
    Figure CN118920248A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method and application of a flexible liquid crystal elastomer laser, a liquid crystal monomer and a chiral initiator react, a mercaptan cross-linking agent, a chain extender, a photoinitiator and a catalyst are added to obtain a precursor solution, finally a laser dye is added, and the flexible liquid crystal elastomer laser is obtained through ultraviolet light curing. The flexible liquid crystal elastomer laser is simple in preparation process, and the tensile elongation of the flexible liquid crystal elastomer laser is as high as 795%. By stretching the flexible liquid crystal elastomer laser device, the reflection color of the flexible liquid crystal elastomer laser device continuously changes from red to blue, and the whole stretching process is completely reversible. The screw pitch of liquid crystal molecules is changed through stretching, so that the output wavelength of the flexible liquid crystal elastomer laser can be regulated and controlled within the range of 560-750 nm, and the flexible liquid crystal elastomer laser has good stability. The flexible liquid crystal elastomer laser can visually monitor and sense human joint movement.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of liquid crystal elastomer preparation, and in particular to a preparation method and application of a flexible liquid crystal elastomer laser. Background Art

[0002] With the development of science and technology, mankind is entering the intelligent era. Smart soft materials are active soft materials represented by electroactive polymers and gels. The characteristics of this type of material are that it produces deformation response and brings corresponding functions under external physical, chemical and other stimuli. It has the advantages of light weight, low price, fast response speed and large deformation. Smart soft materials have great application prospects in the fields of flexible driving and sensing. Liquid crystal elastomers (LCEs), as a stimulus-responsive soft material, have attracted widespread attention due to their ability to have large and reversible deformation, making them excellent candidates for soft actuators, artificial muscles, photonic devices, encryption and anti-counterfeiting, information security storage and biomedical engineering.

[0003] Compared with conventional lasers, a major advantage of random lasers is that they are inexpensive to produce, the technology required for their manufacture is relatively simple, they are easier to tune, and they do not require the high-precision microcavity of conventional lasers. Therefore, random lasers are suitable for large-scale production and have potential applications in many fields such as imaging, lighting, sensing, and information technology. There are currently no reports on the preparation of tunable random lasers using liquid crystal elastomers. Summary of the invention

[0004] In view of the problems in the prior art, the present invention provides a method for preparing a flexible liquid crystal elastic laser. The preparation process is simple, and the tensile elongation of the flexible liquid crystal elastic laser is as high as 795%.

[0005] In order to achieve the above technical objectives, the technical solution of the present invention is:

[0006] A method for preparing a flexible liquid crystal elastomer laser comprises the following steps:

[0007] Step 1, heating and dissolving a liquid crystal monomer and a chiral initiator in an organic solvent to obtain a uniform mixed solution; then adding a thiol crosslinking agent, a chain extender, a photoinitiator and a catalyst to the mixed solution and stirring the mixture to obtain a liquid crystal elastomer precursor solution after Michael addition reaction;

[0008] Step 2, putting the laser dye into the liquid crystal elastomer precursor solution and stirring it evenly, then transferring the solution onto the stretchable adhesive substrate of VHB 4910 and placing it in a vacuum drying oven to obtain the liquid crystal elastomer precursor;

[0009] Step 3, irradiating the liquid crystal elastomer with ultraviolet light and curing it to obtain a flexible liquid crystal elastomer laser.

[0010] The liquid crystal monomer is 1,4-bis-[4(3-propyleneoxypropoxy)benzoyloxy]-2-methylbenzene, referred to as RM257, and its structural formula is:

[0011]

[0012] The liquid crystal material contains liquid crystal primitives, and its molecular structure is designed to self-assemble into an ordered liquid crystal phase under certain conditions. In the prepolymer synthesis, the liquid crystal monomer forms a linear or branched prepolymer with a certain molecular weight through free radical polymerization, which is the basis for the subsequent cross-linking reaction. Its liquid crystal properties play a very important role in the optical and mechanical properties of the elastomer.

[0013] The chiral initiator is (3R, 3aR, 6S, 6aR)-hexahydrofuran[3,2-b]furan-3,6-diylbis(4-((acryloyloxy)butoxy)carbonyl)oxy)benzoyl)oxy)benzoate), referred to as LC756, and its structural formula is:

[0014]

[0015] The chiral initiator can introduce chirality into the liquid crystal phase to form cholesteric liquid crystals, and the addition of the chiral initiator causes the liquid crystal molecules to generate a helical structure during self-assembly, which can reflect light of a specific wavelength, thereby giving the material a unique color effect and response characteristics.

[0016] The mass ratio of the liquid crystal monomer to the chiral initiator is 15-35:1.

[0017] The temperature of the heating and dissolving is 85°C.

[0018] The organic solvent is one or more of dichloromethane (DCM), dichloroethane (DCE), chloroform (TCM), toluene (MB), N,N-dimethylformamide (DMF), tetrahydrofuran (THF), acetonitrile (ACN), dimethyl carbonate (DMC), methyl acetate (MAC), propylene glycol methyl ether acetate (PMA), preferably dichloromethane, which has good solubility and can dissolve liquid crystal monomers, chiral initiators and other reactants to form a uniform reaction medium. It helps to improve the dispersibility of reactants and the uniformity of reactions.

[0019] The thiol crosslinking agent is pentaerythritol tetrakis (3-mercaptopropionic acid), referred to as PETMP; the amount of the thiol crosslinking added is 10-15wt% of the total mass of the liquid crystal monomer and the chiral initiator. The thiol crosslinking agent is added after the prepolymer is formed, and the crosslinking is performed by the click chemistry reaction of thiol-acrylate. The multiple thiol groups in the thiol crosslinking agent can react with the acrylate groups in the prepolymer to form a stable thioether bond and construct a three-dimensional crosslinking network.

[0020] The chain extender adopts 2,2'-(1,2-ethylenedioxy)diethylmercaptan, referred to as EDDET, and the amount of the chain extender added is 20-30wt% of the total mass of the liquid crystal monomer and the chiral initiator. The chain extender contains two thiol groups, which can react with the reactive groups at the ends of the polymer chains. It promotes the extension and cross-linking of the polymer chains to form a more complex and stable network structure, which can effectively improve the mechanical strength and thermal stability. The right amount of chain extender can ensure that the material has sufficient elasticity and maintains a good shape memory effect when responding to external stimuli.

[0021] The photoinitiator is Irgacure 651, and the added amount of the initiator is 0.5-1wt% of the total mass of the liquid crystal monomer and the chiral initiator; the photoinitiator is mainly used for photocuring, and generates free radicals or anions under ultraviolet irradiation, thereby initiating a polymerization reaction to achieve the purpose of curing.

[0022] The catalyst is one or more of N,N-dimethylcyclohexylamine, bis(2-dimethylaminoethyl) ether, di-n-propylamine (DPA), N,N,N',N'-tetramethylalkylenediamine, triethylamine (TEA), N,N-dimethylbenzylamine, triethylenediamine (TEDA), N-ethylmorpholine, N-methylmorpholine (NMM), N,N'-diethylpiperazine, dimethylethanolamine (DMEA), pyridine (Py), and 4-N,N-dimethylpyridine (DMAP), and the amount of the catalyst added is 5-10wt% of the total mass of the liquid crystal monomer and the chiral initiator. The catalyst functions to accelerate the free radical polymerization reaction.

[0023] The laser dye is PM597 and NB, and the ratio of the two is 0.5-1.5:1. The added amount of the laser dye is 1-2wt% of the total mass of the liquid crystal monomer and the chiral initiator.

[0024] The structural formula of the laser dye PM597 is:

[0025]

[0026] The structural formula of the laser dye NB is:

[0027]

[0028] The prepared flexible liquid crystal elastomer laser has unique mechanical response characteristics, such as the reversible color change ability when stretched, which is caused by the change of the liquid crystal pitch. This structural change is directly related to the tunability of the laser wavelength, making the flexible liquid crystal elastomer an ideal candidate for tunable lasers; energy transfer occurs between the laser dye PM597 and NB, which broadens the gain range of the liquid crystal elastomer laser and further promotes the regulation of a wide range of laser wavelengths. The combination of the photophysical properties of the dye and the mechanical properties of the flexible liquid crystal elastomer enables the laser to change the laser wavelength when it is mechanically stretched, realizing dynamic regulation of the wavelength.

[0029] This technical solution successfully combines laser dyes with flexible liquid crystal elastomers to form lasers with unique mechanical structural color responsiveness and wavelength tunability, which are suitable for various advanced application scenarios, such as wearable technology, soft robots and human-machine interaction interfaces. That is, the flexible liquid crystal elastomer laser prepared by the above method is used as a visual interactive sensing device to monitor human joint movements, including neck joints, elbow joints, finger joints, and knee joints.

[0030] It can be seen from the above description that the present invention has the following advantages:

[0031] 1. The preparation method of the flexible liquid crystal elastomer laser provided by the present invention is simple, and its mechanical tensile strain can reach 795%.

[0032] 2. When the flexible liquid crystal elastomer laser prepared by the present invention is mechanically stretched, its structural color changes continuously from red to blue, and the entire change process is reversible.

[0033] 3. The output wavelength of the flexible liquid crystal elastomer laser prepared by the present invention can be adjusted to 560-750nm during the stretching process.

[0034] 4. The flexible liquid crystal elastomer prepared by the present invention adds laser dye as a gain medium to prepare a flexible and tunable liquid crystal elastomer laser. Thanks to the synergistic effect of mechanical color change and liquid crystal pitch change, the flexible liquid crystal elastomer is ensured to exhibit reversible and dynamic color change ability and a wide range of laser wavelength regulation function when mechanically stretched.

[0035] 5. The flexible liquid crystal elastomer laser prepared by the present invention has excellent properties such as flexibility and fatigue resistance. It can be used as a visual interactive sensing device to monitor human joint movements and has great application potential in the fields of optical communication, sensor detection, biomedicine, etc. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1is a stress-strain curve of the flexible liquid crystal elastomer laser prepared in Example 2 of the present invention;

[0037] Figure 2 It is the change of structural color during the stretching recovery process of the flexible liquid crystal elastomer laser prepared in Example 2 of the present invention;

[0038] Figure 3 is a laser emission spectrum diagram of the flexible liquid crystal elastomer laser prepared in Example 2 of the present invention at different stretching rates;

[0039] Figure 4 The flexible liquid crystal elastomer laser prepared in Example 2 of the present invention is stretched multiple times to restore the change in laser output wavelength;

[0040] Figure 5 It is a schematic diagram of the flexible liquid crystal elastomer laser prepared in Example 2 of the present invention attached to a human joint and the laser output changing with the movement of the joint. DETAILED DESCRIPTION

[0041] Combination Figures 1 to 5 , describes in detail a specific embodiment of the present invention, but does not limit the claims of the present invention.

[0042] Example 1

[0043] A method for preparing a flexible liquid crystal elastomer laser, comprising:

[0044] a1, preparation of precursor solution: 30 parts of liquid crystal monomer RM 257 and 1 part of chiral initiator LC 756 were heated to 85° C. and dissolved in an organic solvent of dichloromethane, and then cooled to 25° C. Then, 13 wt% of the total mass of the liquid crystal monomer and the chiral initiator, 25 wt% of the chain extender EDDET, 0.75 wt% of the photoinitiator Irgacure 651 and 6 wt% of the catalyst DPA were added to the solution to form a precursor solution, and the solution was stirred evenly for Michael addition reaction;

[0045] a2, add 0.5wt% of laser dye PM 597 and 0.6wt% of laser dye NB to the precursor solution, stir evenly and transfer the solution to the stretchable adhesive substrate of VHB 4910. Place in a vacuum drying oven at 35°C for 24h;

[0046] a3, using 365nm intensity of 70-80mW·cm -2 The liquid crystal elastomer was irradiated with ultraviolet light for 5 minutes to obtain a flexible liquid crystal elastomer laser. The sample is marked as S1.

[0047] Example 2

[0048] A method for preparing a flexible liquid crystal elastomer laser, comprising:

[0049] a1, preparation of precursor solution: 30 parts of liquid crystal monomer RM 257 and 1 part of chiral initiator LC 756 were heated to 85° C. and dissolved in an organic solvent of dichloromethane, and then cooled to 25° C. Then, 12 wt% of the total mass of the liquid crystal monomer and the chiral initiator, 24 wt% of the chain extender EDDET, 0.6 wt% of the photoinitiator Irgacure 651 and 7 wt% of the catalyst DPA were added to the solution to form a precursor solution, and the solution was stirred evenly for Michael addition reaction;

[0050] a2, add 0.5wt% of laser dye PM 597 and 0.5wt% of laser dye NB to the precursor solution, stir evenly and transfer the solution to the stretchable adhesive substrate of VHB 4910. Place in a vacuum drying oven at 35°C for 24h;

[0051] a3, using 365nm intensity of 70-80mW·cm -2 The liquid crystal elastomer was irradiated with ultraviolet light for 5 minutes to obtain a flexible liquid crystal elastomer laser. The sample is marked as S2.

[0052] Example 3

[0053] A method for preparing a flexible liquid crystal elastomer laser, comprising:

[0054] a1, preparation of precursor solution: 30 parts of liquid crystal monomer RM 257 and 1 part of chiral initiator LC 756 were heated to 85° C. and dissolved in an organic solvent toluene, and then cooled to 25° C. Then, 13 wt% of the total mass of the liquid crystal monomer and the chiral initiator, 20 wt% of the chain extender EDDET, 0.5 wt% of the photoinitiator Irgacure 651 and 7 wt% of the catalyst DPA were added to the solution to form a precursor solution, and the solution was stirred evenly for Michael addition reaction;

[0055] a2, add 0.6wt% of laser dye PM 597 and 0.5wt% of laser dye NB to the precursor solution, stir evenly and transfer the solution to the stretchable adhesive substrate of VHB 4910. Place in a vacuum drying oven at 35°C for 24h;

[0056] a3, using 365nm intensity of 70-80mW·cm -2 The liquid crystal elastomer was irradiated with ultraviolet light for 5 minutes to obtain a flexible liquid crystal elastomer laser. The sample is marked as S3.

[0057] Example 4

[0058] A method for preparing a flexible liquid crystal elastomer laser, comprising:

[0059] a1, preparation of precursor solution: 30 parts of liquid crystal monomer RM 257 and 1 part of chiral initiator LC 756 were heated to 85° C. and dissolved in an organic solvent toluene, and then cooled to 25° C. Then, 15 wt% of the total mass of the liquid crystal monomer and the chiral initiator, 28 wt% of the chain extender EDDET, 0.8 wt% of the photoinitiator Irgacure 651 and 8 wt% of the catalyst DPA were added to the solution to form a precursor solution, and the solution was stirred evenly for Michael addition reaction;

[0060] a2, 0.6wt% of laser dye PM597 and 0.6wt% of laser dye NB are added to the precursor solution, which accounts for the total mass of liquid crystal monomer and chiral initiator. After stirring evenly, the solution is transferred to the stretchable adhesive substrate of VHB 4910. Place it in a vacuum drying oven at 35°C for 24h;

[0061] a3, using 365nm intensity of 70-80mW·cm -2 The liquid crystal elastomer was irradiated with ultraviolet light for 5 minutes to obtain a flexible liquid crystal elastomer laser. The sample is labeled S4.

[0062] Performance Characterization

[0063] The flexible liquid crystal elastomer laser S2 prepared in Example 2 was used as an example for testing.

[0064] The mechanical properties of the prepared flexible liquid crystal elastomer laser S2 were tested, such as Figure 1 As shown, the flexible liquid crystal elastomer lasers show high stretchability, and the tensile strain of the laser can reach 795%. This high ductility enables them to be integrated into smart clothing or skin patches for health monitoring, further broadening the application of flexible liquid crystal elastomer laser devices.

[0065] The prepared flexible liquid crystal elastomer laser S2 was tested and showed color changes during the stretching process. By stretching the device, liquid crystal elastomer lasers with red, green and blue reflection colors can be easily obtained, such as Figure 2 As shown, upon mechanical stretching, its color changes continuously from red to blue, and the entire process is fully reversible, with no noticeable delay between mechanical relaxation and color recovery. Furthermore, no significant degradation is observed upon multiple stretch-release cycles.

[0066] The prepared flexible liquid crystal elastomer laser S2 was tested for laser performance:

[0067] Test method: The laser emission performance of the flexible liquid crystal elastomer device was tested. A pump laser beam was obtained using a Q-switched Nd:YAG second harmonic pulse laser (wavelength 532nm, pulse duration 10ns, repetition frequency 10Hz). The pump pulse energy was controlled by a Glan prism set. The pump beam excited the dye-doped flexible liquid crystal elastomer device sample through an optical microscope. The light emitted by the flexible liquid crystal elastomer device was collected by a fiber spectrometer (QE 65PRO, Ocean Optics, resolution ~0.4nm, integration time 100ms). The pump beam diameter on the sample was about 100μm. The test results of the flexible liquid crystal elastomer laser are shown in Figure 2. Figure 3 As shown. During the stretching process of the flexible liquid crystal elastomer laser, the laser wavelength blue-shifts as the stretching rate increases. It can be clearly observed from the laser spectrum that when the stretching rate is 0%, the main peak wavelength of the laser is at 750nm. As the stretching increases further, the laser spectrum shows an obvious blue shift. When the stretching rate is 120%, the main peak wavelength of the laser blue-shifts to 560nm, and the laser wavelength blue-shifts as much as 190nm. To this end, the 190nm output laser wavelength is regulated by stretching the flexible liquid crystal elastomer laser device.

[0068] The prepared flexible liquid crystal elastomer laser S2 was tested for laser wavelength tuning. Figure 4 As shown, under continuous stretching conditions, the output wavelength of the laser recovers to its original value. Dynamic and continuous laser wavelength tuning is attributed to the change in the pitch of the liquid crystal elastomer under stretching conditions, which causes the band gap of the liquid crystal to blue shift. The dynamic wavelength tuning range of a single flexible liquid crystal elastomer laser device is as high as 190nm. In addition, we verified the repeatability of the stretched wavelength tuning of the flexible liquid crystal elastomer laser by alternating stretching and recovery for multiple cycles. After dozens of stretching cycles, the wavelength and tuning range of the laser remained almost unchanged, fully demonstrating the excellent reversibility and reproducibility of the tunable flexible liquid crystal laser.

[0069] The flexible liquid crystal elastomer laser of this technical solution has excellent mechanical color change, excellent mechanical properties and wide range of laser wavelength control function. The designed flexible liquid crystal elastomer laser is used as a visual interactive sensing device for real-time monitoring of human joint movement. Figure 5As shown, the flexible liquid crystal elastomer laser is attached to the joints of the human body (fingers, palms, elbows, neck and knees). As the bending angle of the joint increases, it can be observed that the structural color of the flexible laser gradually transitions from red to green and blue, and the laser emission wavelength also blue-shifts accordingly. For example, when the finger changes from an extended state to a bent state, the structural color of the flexible laser gradually transitions from red to blue, and the corresponding band gap laser wavelength blue-shifts from 746nm in the initial state to 566nm. And as the bending of the finger is restored, the structural color of the flexible laser and the central wavelength of the laser emission return to the original state. Similarly, when the human neck joint, elbow joint, knee joint, etc. move, the flexible laser can monitor the movement of the joint by reflecting the different colors and laser emission wavelengths. These results show that the invented flexible liquid crystal elastomer can exhibit interactive color-changing properties in the dynamic activities of human joints and can be used as a biomechanical monitoring device during the movement of human joints.

[0070] It is understood that the above specific description of the present invention is only used to illustrate the present invention and is not limited to the technical solutions described in the embodiments of the present invention. Those skilled in the art should understand that the present invention can still be modified or replaced by equivalents to achieve the same technical effects; as long as the use requirements are met, they are within the protection scope of the present invention.

Claims

1. A method for preparing a flexible liquid crystal elastomer laser, characterized in that: The preparation method comprises the following steps: Step 1, heating and dissolving a liquid crystal monomer and a chiral initiator in an organic solvent to obtain a uniform mixed solution; then adding a thiol crosslinking agent, a chain extender, a photoinitiator and a catalyst to the mixed solution and stirring the mixture to obtain a liquid crystal elastomer precursor solution after Michael addition reaction; Step 2, putting the laser dye into the liquid crystal elastomer precursor solution and stirring it evenly, then transferring the solution onto the stretchable adhesive substrate of VHB4910 and placing it in a vacuum drying oven to obtain the liquid crystal elastomer precursor; Step 3, irradiating the liquid crystal elastomer with ultraviolet light and curing it to obtain a flexible liquid crystal elastomer laser.

2. The method for preparing a flexible liquid crystal elastomer laser according to claim 1, characterized in that: The liquid crystal monomer is 1,4-bis-[4(3-propyleneoxypropoxy)benzoyloxy]-2-methylbenzene, referred to as RM257, and its structural formula is:

3. The method for preparing a flexible liquid crystal elastomer laser according to claim 1, characterized in that: The chiral initiator is (3R, 3aR, 6S, 6aR)-hexahydrofuran[3,2-b]furan-3,6-diylbis(4-((acryloyloxy)butoxy)carbonyl)oxy)benzoyl)oxy)benzoate), referred to as LC756, and its structural formula is:

4. The method for preparing a flexible liquid crystal elastomer laser according to claim 1, characterized in that: The organic solvent is one or more of dichloromethane (DCM), dichloroethane (DCE), chloroform (TCM), toluene (MB), N,N-dimethylformamide (DMF), tetrahydrofuran (THF), acetonitrile (ACN), dimethyl carbonate (DMC), methyl acetate (MAC), and propylene glycol methyl ether acetate (PMA).

5. The method for preparing a flexible liquid crystal elastomer laser according to claim 1, characterized in that: The thiol crosslinking agent is pentaerythritol tetrakis (3-mercaptopropionate), referred to as PETMP.

6. The method for preparing a flexible liquid crystal elastomer laser according to claim 1, characterized in that: The chain extender is 2,2'-(1,2-ethylenedioxy)diethylmercaptan, referred to as EDDET.

7. The method for preparing a flexible liquid crystal elastomer laser according to claim 1, characterized in that: The photoinitiator used is Irgacure 651.

8. The method for preparing a flexible liquid crystal elastomer laser according to claim 1, characterized in that: The catalyst is one or more of N,N-dimethylcyclohexylamine, bis(2-dimethylaminoethyl) ether, di-n-propylamine (DPA), N,N,N',N'-tetramethylalkylenediamine, triethylamine (TEA), N,N-dimethylbenzylamine, triethylenediamine (TEDA), N-ethylmorpholine, N-methylmorpholine (NMM), N,N'-diethylpiperazine, dimethylethanolamine (DMEA), pyridine (Py), and 4-N,N-dimethylpyridine (DMAP).

9. The method for preparing a flexible liquid crystal elastomer laser according to claim 1, characterized in that: The laser dye is PM597 and NB, and the ratio of the two is 0.5-1.5:

1. The added amount of the laser dye is 1-2wt% of the total mass of the liquid crystal monomer and the chiral initiator.

10. The method for preparing a flexible liquid crystal elastomer laser according to any one of claims 1 to 9, characterized in that: The flexible liquid crystal elastomer laser prepared by the method is used as a visual interactive sensing device to monitor human joint movements, including neck joints, elbow joints, finger joints, and knee joints.

Citation Information

Cited By

  • Cesium tungsten bronze powder doped liquid crystal elastomer material and preparation method thereof

    CN119800541A

  • Intelligent wearable high-sensitivity visual mechanical sensor and preparation method thereof

    CN120352049A