Selective coarsening method for ceramic copper-clad plate
Through the selective coarse method of ceramic copper clad plate, a concave structure is formed and the anchoring effect is enhanced using nanosilicon and organosilane, which solves the problems of welding wetting and hollowing, improves welding quality and reliability, and is suitable for packaging of IGBT modules.
Patent Information
- Application Number
- CN202410899477.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-05
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-05
AI Technical Summary
The existing ceramic copper clad plate browning process is prone to form welding holes during welding, affecting the reliability of the IGBT module, and the browned film is difficult to remove, affecting the binding force of the plating, and the hot and cold impact performance of the plastic seal is poor, and the edge resin is easy to be with ceramics. The lining plate is cracked.
The ceramic copper clad plate is selected by printing active brazing between ceramic and copper, sintering to form ceramic copper clad plates, and forming concave structures in the functional area. Nanosilicon and organosilane are used to enhance the anchoring effect, combined with chemical grinding and plating technology to form a suitable roughness and concave structure to avoid welding holes and solder diffusion.
The wetting and solder diffusion problems of chip welding in the functional area are achieved, the bonding force between resin and ceramic copper clad plate is enhanced, the welding cavity and solder spillage is avoided, and the solder quality and reliability are improved.
Smart Images

Figure CN118921883A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of ceramic copper-clad laminates, and in particular to a selective roughening method for ceramic copper-clad laminates. Background Art
[0002] The potting gel process is often used in power devices. The glue material is mostly in the form of silicone gel. The potting form is used to protect the device and resist vibration and impact, and it plays a role in waterproofing and moisture-proofing, and realizes the sealing function. Compared with plastic encapsulation, the potting cost is relatively high. The encapsulation method used in plastic encapsulation is transfer molding, which is a thermosetting plastic molding method evolved from wet lamination and injection technology. It has low cost and high efficiency, but the thermal shock performance of plastic encapsulation is relatively poor, and the edge resin is easy to crack with the ceramic liner.
[0003] At present, the epoxy resin bonding strength can be improved by adding coupling agents to the resin and optimizing the formation of chemical bonds with inorganic media. Secondly, the ceramic copper-clad laminate can be treated with browning to improve the bonding strength with the resin. Patent No. CN202310488289.5 discloses a browning scheme, which forms a rough organic copper oxide layer with a honeycomb appearance on the copper surface through chemical bonding with Cu2O. During the lamination process, this organic copper oxide film layer undergoes a curing and cross-linking reaction with the resin, which can provide better interface bonding strength.
[0004] Browning treatment is often used for lamination of multilayer boards. It cannot be directly welded to the chip, which affects the WB capability. Too rough a structure can easily form welding voids in the welding layer, affecting the reliability of the IGBT module. The browning film has strong acid resistance and is difficult to effectively remove by pickling, which affects the bonding strength of the coating.
[0005] In summary, the present invention provides a method for selective roughening of a ceramic copper-clad laminate, which can effectively solve the problems of chip soldering wettability, voids and solder diffusion in the functional area. Summary of the invention
[0006] The object of the present invention is to provide a method for selective roughening of a ceramic copper-clad laminate, in which the ceramic copper-clad liner is roughened and pre-coated with nano-silicon and organic silane layers to enhance the anchoring effect, and after roughening, it is protected by a mask, and chemical grinding is used to achieve local roughening and plating schemes, and a concave structure is achieved in a functional area, effectively solving the problems of chip welding wettability, voids and solder diffusion in the functional area.
[0007] To achieve the above object, the present invention is implemented by the following technical solutions:
[0008] A method for selectively roughening a ceramic copper-clad plate comprises the following preparation steps:
[0009] S1 prints a layer of active brazing material between the ceramic and the copper foil;
[0010] S2 sintering the ceramic substrate printed with the solder layer and the copper foil at a sintering temperature of 800°C to 1000°C to form a ceramic copper clad laminate.
[0011] S3: laminating or coating the sintered ceramic copper-clad laminate with a layer of anti-corrosion layer, and then protecting the required copper layer and exposing the unnecessary copper layer through exposure and development to form a specific etching pattern, and placing it in a CuCl2 system or FeCl3 etching solution to complete copper etching;
[0012] S4: placing the copper-etched ceramic copper-clad laminate in a solder layer etching solution to remove unnecessary solder layers;
[0013] S5: The patterned ceramic copper-clad laminate is cleaned, cleaned, roughened with a roughening liquid, cleaned, pickled, cleaned, impregnated with an impregnation liquid, and dried to form a surface nest-shaped structure surface 4, and the coating is completely infiltrated into the concave and micropores of the rough surface by filling with nano-silicon and organic silane to enhance the anchoring and improve the resin bonding force, and the surface roughness Sa is greater than 0.2um, and Sdr is greater than 0.15;
[0014] S6: printing a heat-curable wet film (5) on the roughened surface 4 of the ceramic copper-clad laminate to form a structure as shown in FIG. C, exposing the area to be surface treated;
[0015] After S7 masking is completed, the ceramic copper clad board is placed in a chemical grinding treatment solution to remove the surface coarsening structure, reduce the surface roughness, and form a concave structure with a concave depth of 2-18um;
[0016] S8 finally processes the ceramic copper clad board through nickel plating and chemical silver deposition, and then stripping the film to form the final structure or grinding it to cover the non-plated area through the positioning hole secondary printing mask method, and then plating and stripping the film to finally form a composite form of bare copper and nickel plating and silver surface treatment.
[0017] As a further improvement of the present solution, the brazing layer in S1 is Ag, wherein the mass percentage of Ag is above 70-80%, and the rest is copper and TI.
[0018] As a further improvement of the present scheme, in S5, roughening is performed using a roughening liquid, wherein the roughening liquid is any one or more of an organic acid, cupric chloride, a complex, a copper corrosion inhibitor, and the like.
[0019] As a further improvement of this scheme, the roughening liquid is formic acid 0.15-2.3 mol / L, copper ion 15-26 g / L, sodium diethyldithiocarbamate 0.12-0.35 g / L, 2-thiol imidazoline 0.03-0.11 g / L, polyethyleneimine 0.45-1.1 g / L, and the roughening temperature is 23-30°C.
[0020] As a further improvement of this solution, in S5, the impregnation is performed with an impregnation liquid, wherein the impregnation liquid includes the following components in parts by volume:
[0021] 3 to 8 parts of 2 to 12 nm organic silicon solution;
[0022] KRN8026 organosilane 1-3 parts;
[0023] The rest is water.
[0024] As a further improvement of this solution, in S7, the chemical polishing solution comprises:
[0025] The content of hydrogen peroxide is 20V / V% to 70V / V%;
[0026] The content of alcohol is 2.5V / V~5V / V%;
[0027] Corrosion inhibitor 0.1-0.3g / L;
[0028] The content of the organic amine complex is 1.2V / V to 4.5V / V.
[0029] As a further improvement of this solution, in S7, the pH is 0.9-1.2, and the grinding rate is controlled to be 0.6-1.1 um / min.
[0030] Compared with the prior art, the selective roughening method of the ceramic copper-clad laminate of the present invention has the following beneficial effects:
[0031] 1. Realize selective roughening and plating, form appropriate roughness on the roughened surface, enhance the bonding force with the resin, and there is no organic film structure similar to browning on the surface, so the packaging factory does not need to open windows in the welding area;
[0032] 2. Pre-coat the roughened area with nano-silicon solution and organosilane, and use the small size of nano-silicon and the good flow of organosilane to infiltrate into the roughened concave structure to enhance the anchoring effect; at the same time, form hydrogen bonds, silicon-oxygen bonds and van der Waals bonds with the copper surface to enhance the bonding force;
[0033] 3. After chemical grinding of the functional area, the problem of welding voids caused by roughened surface pits is avoided, and the surface weldability is good. At the same time, the concave structure of the welding area effectively prevents solder overflow during the welding process and reduces micropores in the silver plating layer.
[0034] Instruction Manual
[0035] Figure 1 This is a schematic diagram of the structure after etching of the present invention;
[0036] Figure 2 This is a schematic diagram of the structure after surface roughening treatment of the present invention;
[0037] Figure 3This is a schematic diagram of the structure after mask processing of the present invention;
[0038] Figure 4 This is a schematic diagram of the structure after functional area processing of the present invention;
[0039] Figure 5 This is a schematic diagram of the structure after coating treatment of the present invention;
[0040] Figure 6 This is a schematic diagram of the structure of a ceramic copper-clad laminate treated by the selective roughening method of the present invention;
[0041] Figure 7 This is a diagram showing the weldability test results of Example 1 of the present invention;
[0042] Figure 8 This is a graph showing the weldability test results of Comparative Example 1 of the present invention;
[0043] Fig. 9 This is a diagram showing the surface structure analysis results before roughening in Example 1 of the present invention;
[0044] Fig.10 This is a diagram showing the roughened surface structure analysis result of Example 1 of the present invention;
[0045] Fig.11 This is a diagram showing the surface structure analysis results after grinding of Example 1 of the present invention;
[0046] Description of reference numerals:
[0047] 1- Ceramic layer;
[0048] 2- is the brazing layer;
[0049] 3- is copper foil;
[0050] 4-Surface roughening layer;
[0051] 5-mask processing layer;
[0052] 6- Functional area processing layer;
[0053] 7- Plating;
[0054] 8-Unroughened copper layer. DETAILED DESCRIPTION
[0055] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is further described below in conjunction with Examples 1 to 8:
[0056] A method for selectively roughening a ceramic copper-clad plate comprises the following preparation steps:
[0057] S1 prints a layer of active brazing material between the ceramic and the copper foil;
[0058] The brazing layer in S1 is Ag, wherein the mass percentage of Ag is more than 70-80%, and the rest is copper, TI and neodymium earth.
[0059] S2 sintering the ceramic substrate printed with the solder layer and the copper foil at a sintering temperature of 800°C to 1000°C to form a ceramic copper clad laminate.
[0060] S3: laminating or coating the sintered ceramic copper-clad laminate with a layer of anti-corrosion layer, and then protecting the required copper layer and exposing the unnecessary copper layer through exposure and development to form a specific etching pattern, and placing it in a CuCl2 system or FeCl3 etching solution to complete copper etching;
[0061] S4: placing the copper-etched ceramic copper-clad laminate in a solder layer etching solution to remove unnecessary solder layers;
[0062] S5: The patterned ceramic copper-clad laminate is cleaned, washed, roughened with a roughening liquid, washed, pickled, washed, impregnated with an impregnation liquid, and dried to form a surface dent-shaped structure surface 4 as shown in FIG. B, and the coating is completely infiltrated into the concave and micropores of the rough surface by filling with nano-silicon and organic silane to enhance the anchoring and improve the resin bonding force, and the surface roughness Sa is greater than 0.2um, and Sdr is greater than 0.15;
[0063] 2. In S5, the impregnation is carried out with an impregnation liquid, and the impregnation liquid includes the following components in parts by volume:
[0064] 2-12nm to obtain 3-8 parts of organosilicon solution;
[0065] KRN8026 organosilane 1-3 parts;
[0066] The rest is water.
[0067] In S5, roughening is performed using a roughening liquid.
[0068] S6: Printing a heat-cured wet film 5 on the roughened surface 4 of the ceramic copper-clad plate to form a Figure 3 structure, exposing the area to be surface treated;
[0069] After the S7 mask is completed, the ceramic copper clad board is placed in a chemical grinding treatment solution to remove the surface roughening structure, reduce the surface roughness, and form a concave structure such as Figure 4 , concave depth 2-18um;
[0070] In S7, the chemical polishing solution includes:
[0071] The content of hydrogen peroxide is 20V / V% to 70V / V%;
[0072] The content of alcohol is 2.5V / V~5V / V%;
[0073] The content of organic amine complex is 1.2V / V~4.5V / V%;
[0074] Corrosion inhibitor 0.1-0.3g / L.
[0075] In S7, the pH is 0.9-1.2, and the grinding rate is controlled at 0.6-1.1 um / min.
[0076] S8 finally forms the structure 4 ceramic copper clad board through nickel plating and chemical silver deposition. Figure 5 Structure, then stripping to form Figure 6 structure.
[0077] The selective roughening method for ceramic copper-clad laminates comprises a roughening liquid containing 0.15-2.3 mol / L formic acid, 15-26 g / L copper ions, 0.12-0.35 g / L sodium diethyldithiocarbamate, 0.03-0.11 g / L 2-thiol imidazoline, and 0.45-1.1 g / L polyethyleneimine, and a temperature of 23-30°C.
[0078] Example 1
[0079] 1. The patterned ceramic copper-clad substrate is cleaned, roughened, pickled, impregnated and dried, with a cleaning concentration of 5% and a temperature of 45°C;
[0080] The roughening solution preferably comprises 1.6 mol / L formic acid, 16 g / L copper ion, 0.12 g / L sodium diethyldithiocarbamate, 0.04 g / L 2-thiol imidazoline, and 0.5 g / L polyethyleneimine; the temperature is 23°C; the pickling concentration is 10% hydrochloric acid; the solution is impregnated with 3.5% 3 nanometer organic silicon solution and 1.5% KRN8026 organic silane coupling agent and dried, and the roughness Sdr is 0.71;
[0081] 2. A dry film is attached to the roughened surface 4 of the ceramic copper-clad laminate, and a mask layer 5 is formed by exposure and development. Figure 3 structure, exposing the area to be surface treated;
[0082] 3. The developed ceramic copper-clad laminate is further placed in a 5% acid wash; then placed in a 3% hydrogen peroxide, 6% sulfuric acid, and 3% 760 for 1 minute; further placed in a chemical grinding treatment solution, the content of hydrogen peroxide is 60V / V%, polyethylene glycol 3.5g / L, thiourea 2.6g / L, tetrahydroxypropyl ethylenediamine 1.7V / V%, sulfuric acid is used to adjust the pH to 1.2, and the grinding rate is controlled to 0.8um / min to remove the surface coarsening structure, reduce the surface roughness, and form a concave structure such as Figure 4 , concave depth 2-8um;
[0083] 4. Finally, the ceramic copper clad laminate is directly surface treated or Figure 4Structurally, the secondary printing mask is used to protect the copper layer 8 area through the positioning holes on the board surface, and some non-plated areas are covered and then chemically micro-etched and chemically silvered. The silver ion is controlled at 0.8g / L and the control temperature is set at 50℃ to form a certain thickness of plating layer. Figure 5 The coating 7 in the middle has good bonding strength and few micropores;
[0084] 5. Further stripping is performed, the stripping concentration is 5%, the temperature is 50℃ to form Figure 6 The structure realizes a local roughening layer 4, a low-roughness bare copper layer 8 and a plating layer 7; the solderability and binding ability of the functional area are ensured, the roughening surface improves the bonding strength with the plastic encapsulation resin, and the concave structure of the welding area effectively prevents the diffusion of solder.
[0085] The roughness test results of Example 1 are shown in Table 1
[0086]
[0087] Comparative Example 1
[0088] The browning treatment of CN202011329108.7 in the prior art is adopted:
[0089] 8wt% concentrated sulfuric acid 120g / L, 30wt% hydrogen peroxide 20g / L, compound corrosion inhibitor 15g / L, KH55020-50g / L, copper sulfate 70g / L, wetting agent 15g / L, polyethylene glycol monomethyl ether 8g / L, and deionized water as the balance.
[0090] The weldability test results of Example 1 and Comparative Example 1 are shown in Table 2
[0091]
[0092] The above description is only a preferred embodiment of the present invention, and does not limit the patent scope of the present invention. All equivalent changes made using the present invention are within the patent protection scope of the present invention.
Claims
1. A method for selective roughening of a ceramic copper-clad laminate, characterized in that: The method comprises the following preparation steps: S1 prints a layer of active brazing material between the ceramic and the copper foil; S2 sintering the ceramic substrate printed with the solder layer and the copper foil at a sintering temperature of 800°C to 1000°C to form a ceramic copper clad laminate. S3: laminating or coating the sintered ceramic copper-clad laminate with a layer of anti-corrosion layer, and then protecting the required copper layer and exposing the unnecessary copper layer through exposure and development to form a specific etching pattern, and placing it in a CuCl2 system or FeCl3 etching solution to complete copper etching; S4: placing the copper-etched ceramic copper-clad laminate in a brazing layer etching solution to remove unnecessary brazing layers; S5: The patterned ceramic copper-clad laminate is cleaned, cleaned, roughened with a roughening liquid, cleaned, pickled, cleaned, impregnated with an impregnation liquid, and dried to form a surface nest-shaped structure surface 4, and the coating is completely infiltrated into the concave and micropores of the rough surface by filling with nano-silicon and organic silane to enhance the anchoring and improve the resin bonding force, and the surface roughness Sa is greater than 0.2um, and Sdr is greater than 0.15; S6: printing a heat-curable wet film (5) on the roughened surface 4 of the ceramic copper-clad laminate to form a structure as shown in FIG. C, exposing the area to be surface treated; After S7 masking is completed, the ceramic copper clad board is placed in a chemical grinding treatment solution to remove the surface coarsening structure, reduce the surface roughness, and form a concave structure with a concave depth of 2-18um; S8 finally processes the ceramic copper clad board through nickel plating and chemical silver deposition, and then stripping the film to form the final structure or grinding it to cover the non-plated area through the positioning hole secondary printing mask method, and then plating and stripping the film to finally form a composite form of bare copper and nickel plating and silver surface treatment.
2. The method for selective roughening of a ceramic copper-clad laminate according to claim 1, characterized in that: The brazing layer in S1 is Ag, wherein the mass percentage of Ag is more than 70-80%, and the rest is copper, TI and neodymium earth.
3. The selective roughening method of a ceramic copper-clad laminate according to claim 1, characterized in that: In S5, roughening is performed using a roughening liquid, wherein the roughening liquid is any one or more of an organic acid, cupric chloride, a complex, and a copper corrosion inhibitor.
4. The method for selective roughening of a ceramic copper-clad laminate according to claim 3, characterized in that: The roughening liquid comprises formic acid 0.15-2.3 mol / L, copper ion 15-26 g / L, sodium diethyldithiocarbamate 0.12-0.35 g / L, 2-thiol imidazoline 0.03-0.11 g / L, polyethyleneimine 0.45-1.1 g / L, and the roughening temperature is 23-30°C.
5. The method for selective roughening of a ceramic copper-clad laminate according to claim 3, characterized in that: In S5, the impregnation is performed with an impregnation liquid, wherein the impregnation liquid comprises the following components in parts by volume: 3 to 8 parts of 2 to 12 nm organic silicon solution; KRN8026 organosilane 1-3 parts; The rest is water.
6. The method for selective roughening of a ceramic copper-clad laminate according to claim 1, characterized in that: In S7, the chemical polishing solution includes: The content of hydrogen peroxide is 20V / V% to 70V / V%; The content of alcohol is 2.5V / V~5V / V%; Corrosion inhibitor 0.1-0.3g / L; The content of the organic amine complex is 1.2V / V to 4.5V / V.
7. The method for selective roughening of a ceramic copper-clad laminate according to claim 6, characterized in that: In S7, the pH is 0.9-1.2, and the grinding rate is controlled at 0.6-1.1 um / min.
Citation Information
Patent Citations
Preparation method of lead frame with rough side wall
CN112133640A
Brown oxidation liquid for high-frequency high-speed circuit board and preparation method thereof
CN116463621A
Patterning method of nitride ceramic copper-clad plate and nitride ceramic copper-clad plate
CN106328544A
Electrolytic copper foil with special coarsening morphology and preparation method thereof
CN115652384A
Printed wiring board
JP1996242064A