Photoelectric device, preparation method of photoelectric device and electronic equipment

By introducing nucleophilic functional layer and multi-layer electronic transmission layer structure into optoelectronic devices, the problem of carrier transmission imbalance is solved, the photoelectric performance and device life are improved, and the performance stability of electronic devices is improved.

CN118922009APending Publication Date: 2024-11-08TCL TECHNOLOGY GROUP CORPORATION
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310511994.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-08
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

There is room for improvement in the photoelectric performance and device life of existing optoelectronic devices, especially the problem of unbalanced carrier transmission has led to limited improvement in the photoelectric performance and life.

Method used

The nucleophilic functional layer is introduced into the electronic functional layer of the optoelectronic device. The nucleophilic functional layer is composed of nucleophilic compound materials and is arranged between the electron transport layers to attract holes and promote electron-hole transmission balance. At the same time, multi-layer electrons are used Transport layer structure and auxiliary functional layer to enhance mechanical stress and acid and alkali resistance.

Benefits of technology

It effectively improves the hole injection level and photoelectric performance of optoelectronic devices, extends the device life, and improves the display effect and service life of electronic devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118922009A_ABST
    Figure CN118922009A_ABST
Patent Text Reader

Abstract

The invention discloses a photoelectric device, a preparation method of the photoelectric device and electronic equipment, the photoelectric device comprises an anode, a cathode and an electronic function layer, the anode and the cathode are oppositely arranged, the electronic function layer is arranged between the cathode and the anode, the electronic function layer comprises N electron transport layers arranged between the anode and the cathode at intervals, n is a positive integer greater than or equal to 2, the electron function layer further comprises a nucleophilic function layer, the nucleophilic function layer is arranged between two adjacent electron transport layers, the material of the nucleophilic function layer contains a nucleophilic compound, electron-hole transport balance is promoted, the photoelectric performance of the photoelectric device is improved, the service life of the device is prolonged, and the photoelectric device is suitable for large-scale production. When the photoelectric device or the photoelectric device prepared by the preparation method of the photoelectric device is applied to electronic equipment, the display effect of the electronic equipment is improved, the service life of the electronic equipment is prolonged, and the performance stability of the electronic equipment is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of optoelectronic technology, and in particular to an optoelectronic device, a method for preparing an optoelectronic device, and an electronic device. Background Art

[0002] Photoelectric devices refer to a type of device made using the photoelectric effect of semiconductors, including but not limited to light-emitting devices, solar cells or photodetectors. Taking light-emitting devices as an example, light-emitting devices include but are not limited to organic light-emitting diodes (OLED) and quantum dot light-emitting diodes (QLED). OLED / QLED has a "sandwich" structure, that is, it includes an anode, a cathode and a light-emitting layer, wherein the anode and the cathode are arranged opposite to each other, and the light-emitting layer is arranged between the anode and the cathode. The light-emitting principle of OLED / QLED is: electrons are injected from the cathode of the device into the light-emitting area, and holes are injected from the anode of the device into the light-emitting area. Electrons and holes recombine in the light-emitting area to form excitons, and the recombined excitons release photons in the form of radiation transition, thereby emitting light.

[0003] After years of development, optoelectronic devices have made great progress in performance indicators and have shown great potential for application development. However, there are still some shortcomings, and the optoelectronic performance and device life of optoelectronic devices need to be further improved. Summary of the invention

[0004] The present application provides a method for preparing a photoelectric device, a photoelectric device, and an electronic device comprising the photoelectric device, so as to improve the photoelectric performance and device life of the photoelectric device.

[0005] The technical solution of this application is as follows:

[0006] In a first aspect, the present application provides an optoelectronic device, the optoelectronic device comprising:

[0007] an anode and a cathode disposed opposite to each other; and

[0008] An electronic functional layer, disposed between the cathode and the anode;

[0009] Among them, the electronic functional layer includes N electron transport layers spaced between the anode and the cathode, and N is a positive integer greater than or equal to 2; the electronic functional layer also includes a nucleophilic functional layer, which is arranged between two adjacent electron transport layers, and the material of the nucleophilic functional layer includes a nucleophilic compound.

[0010] Optionally, at least one nucleophilic functional layer is provided between any two adjacent electron transport layers; and / or

[0011] The nucleophilic compound is selected from one or more of NaNH2, Grignard reagent, Gilman reagent, organic lithium reagent, NaBH4, LiAlH4, amino-substituted coumarin, a first compound and a second compound, wherein the first compound has a structure shown in the following general formula (I):

[0012]

[0013] The second compound has a structure shown in the following general formula (II):

[0014]

[0015] wherein R1 to R6 are independently selected from aliphatic hydrocarbon groups or aromatic hydrocarbon groups; and / or

[0016] The material of the electron transport layer includes a first metal oxide, which is selected from one or more of zinc oxide, titanium oxide, tin oxide, barium oxide, tantalum oxide, aluminum oxide, zirconium oxide, magnesium zinc oxide, calcium zinc oxide, zirconium oxide, gallium zinc oxide, aluminum zinc oxide, lithium zinc oxide, titanium zinc oxide, yttrium zinc oxide, indium tin oxide and lithium titanium oxide.

[0017] Optionally, the carbon number of the aliphatic hydrocarbon group is 1 to 10, and the aliphatic hydrocarbon group is selected from pentyl, hexyl, heptyl or octyl; the carbon number of the aromatic hydrocarbon group is 6 to 20, and the aromatic hydrocarbon group is selected from phenyl, naphthyl or biphenyl; and / or

[0018] When there are at least two nucleophilic functional layers, the nucleophilic compounds in each nucleophilic functional layer are independently selected from one or more of NaNH2, Grignard reagent, Gilman reagent, organic lithium reagent, NaBH4, LiAlH4, amino-substituted coumarin, the first compound and the second compound.

[0019] Optionally, the total thickness of the electronic functional layer is 40 nm to 200 nm; and / or

[0020] The thickness of each electron transport layer is 7nm to 15nm; and / or

[0021] The total thickness of the N electron transport layers is 30 nm to 80 nm; and / or

[0022] When there are at least two nucleophilic functional layers, the total thickness of the nucleophilic functional layers is 7 nm to 40 nm, and / or the thickness of each nucleophilic functional layer is 7 nm to 15 nm.

[0023] Optionally, the electronic functional layer further comprises at least one auxiliary functional layer, wherein the auxiliary functional layer is disposed between the adjacent electron transport layer and the nucleophilic functional layer, and / or the auxiliary functional layer is disposed between two adjacent nucleophilic functional layers; the material of the auxiliary functional layer comprises a cross-linking compound, wherein the cross-linking compound is a compound formed by a self-cross-linking reaction of a third compound;

[0024] Wherein, the third compound has a structure shown by the following general formula (III):

[0025]

[0026] In the general formula (III), each occurrence of R7 is independently selected from hydrogen atom, -NH2, carboxyl group, hydrocarbon group or -X, X is halogen, and y is a positive integer of 1 to 4.

[0027] Optionally, the auxiliary functional layer has a thickness of 7 nm to 15 nm; and / or

[0028] The hydrocarbon group has 1 to 10 carbon atoms, and optionally, the hydrocarbon group is selected from methyl, ethyl or propyl; and / or

[0029] The material of the nucleophilic functional layer does not contain coumarin and / or coumarin derivatives.

[0030] Optionally, the optoelectronic device further comprises a light-emitting layer, which is disposed between the anode and the electronic functional layer; the material of the light-emitting layer comprises one or more of an organic light-emitting material and quantum dots;

[0031] Wherein, the material of the light-emitting layer comprises one or more of an organic light-emitting material and a quantum dot; wherein, the organic light-emitting material is selected from 4,4'-bis(N-carbazole)-1,1'-biphenyl:tri[2-(p-tolyl)pyridine iridium(III), 4,4',4"-tri(carbazole-9-yl)triphenylamine:tri[2-(p-tolyl)pyridine iridium, diaromatic anthracene derivatives, distilbene aromatic derivatives, pyrene derivatives, fluorene derivatives, TBPe fluorescent materials, TTPX fluorescent materials, TBRb fluorescent materials, DBP fluorescent materials, delayed fluorescent materials, TTA materials, thermally activated delayed materials, polymers containing BN covalent bonds, hybrid localized charge transfer excited state materials and exciplex light-emitting materials; the quantum dots are selected from one or more of single component quantum dots, core-shell structure quantum dots, inorganic perovskite quantum dots, organic perovskite quantum dots and organic-inorganic hybrid perovskite quantum dots; and / or

[0032] The material of the single-component quantum dot, the material of the core of the core-shell structure quantum dot, and the material of the shell of the core-shell structure quantum dot are independently selected from at least one of a II-VI group compound, a III-V group compound, a IV-VI group compound, or a I-III-VI group compound, wherein the II-VI group compound is selected from CdS, CdSe, CdTe, ZnS, ZnSe, ZnTe, ZnO, HgS, HgSe, HgTe, CdSeS, CdSeTe, CdSTe, ZnSeS, ZnSeTe, ZnSTe, HgSeS, HgSeT e, HgSTe, CdZnS, CdZnSe, CdZnTe, CdHgS, CdHgSe, CdHgTe, HgZnS, HgZnSe, HgZnTe, CdZnSeS, CdZnSeTe, CdZnSTe, CdHgSeS, CdHgSeTe, CdHgSTe, HgZnSeS, HgZnSeTe and HgZnSTe, and the III-V group compound is selected from GaN, GaP, GaAs, GaSb, AlN, AlP, AlAs, AlSb, InN, InP, InA s, InSb, GaNP, GaNAs, GaNSb, GaPAs, GaPSb, AlNP, AlNAs, AlNSb, AlPAs, AlPSb, InNP, InNAs, InNSb, InPAs, InPSb, GaAlNP, GaAl NAs, GaAlNSb, GaAlPAs, GaAlPSb, GaInNP, GaInNAs, GaInNSb, GaInPAs, GaInPSb, InAlNP, InAlNAs, InAlNSb, InAlPAs and InAlPS b, the IV-VI group compound is selected from one or more of SnS, SnSe, SnTe, PbS, PbSe, PbTe, SnSeS, SnSeTe, SnSTe, PbSeS, PbSeTe, PbSTe, SnPbS, SnPbSe, SnPbTe, SnPbSSe, SnPbSeTe and SnPbSTe, the I-III-VI group compound is selected from one or more of CuInS, CuInSe and AgInS; the general structural formula of the inorganic perovskite quantum dot is AMX3, wherein A is Cs + ion, M is a divalent metal cation, M is selected from Pb 2+ Sn 2+ , Cu 2+ 、Ni 2+ 、Cd 2 + Cr 2+ , Mn 2+ 、Co2+ , Fe 2+ ,Ge 2+ , Yb 2+ and Eu 2+ One or more of, X is a halogen anion; the general structural formula of the organic perovskite quantum dot is CMX3, C is a carboxamidine group; the general structural formula of the organic-inorganic hybrid perovskite quantum dot is BMX3, B is selected from an organic amine cation; and / or

[0033] The materials of the anode and the cathode are independently selected from one or more of a metal, a carbon material and a second metal oxide, the metal is selected from one or more of Al, Ag, Cu, Mo, Au, Ba, Pt, Ca, Ir, Ni and Mg, the carbon material is selected from one or more of graphite, carbon nanotubes, graphene and carbon fibers, and the third metal oxide is selected from one or more of indium-doped tin oxide, fluorine-doped tin oxide, antimony-doped tin oxide, aluminum-doped zinc oxide, gallium-doped zinc oxide, indium-doped zinc oxide, magnesium-doped zinc oxide, aluminum-doped magnesium oxide, SnO2, ZnO and In2O3; and / or

[0034] The photoelectric device also includes a hole functional layer arranged between the anode and the electronic functional layer, and the material of the hole functional layer includes poly (3,4-ethylenedioxythiophene): poly (styrene sulfonic acid), copper phthalocyanine, titanium phthalocyanine, 2,3,5,6-tetrafluoro-7,7',8,8'-tetracyanodimethyl-p-benzoquinone, 2,3,6,7,10,11-hexycyano-1,4,5,8,9,12-hexaazatriphenylene, 3-hexyl substituted polythiophene, poly (9-vinyl carbazole), 4,4'-bis (9-carbazole) biphenyl, poly [bis (4-phenyl) (4-butylphenyl) amine], 4, 4'-cyclohexylbis[N,N-di(4-methylphenyl)aniline], poly[(9,9-dioctylfluorenyl-2,7-diyl)-co-(4,4'-(N-(4-sec-butylphenyl)diphenylamine)], poly[(9,9-dioctylfluorenyl-2,7-diyl)-co-(4,4'-(N-(p-butylphenyl))diphenylamine)], poly(N,N'-di(4-butylphenyl)-N,N'-diphenyl-1,4-phenylenediamine-co-9,9-dioctylfluorene), 4,4',4'-tri(N-3-methylphenyl-N-phenylamino)triphenylamine, 4,4',4"-tri (Carbazole-9-yl) triphenylamine, 4,4',4'-tri(2-naphthylphenylamino) triphenylamine, N,N'-diphenyl-N,N'-(1-naphthyl)-1,1'-biphenyl-4,4'-diamine, N,N'-diphenyl-N,N'-di(3-methylphenyl)-1,1'-biphenyl-4,4'-diamine, N,N'-bis[4-(diphenylamino)phenyl]-N,N'-diphenylbenzidine, N,N'-bis(3-methylphenyl)-N,N'-diphenyl-9,9-spirobifluorene-2,7-diamine, N2,N7-di-1-naphthyl-N2,N7-diphenyl One or more of 9,9'-spirobi[9H-fluorene]-2,7-diamine, poly[bis(4-phenyl)(2,4,6-trimethylphenyl)amine], 2,2',7,7'-tetrakis[N,N-di(4-methoxyphenyl)amino]-9,9'-spirobifluorene, doped or undoped graphene, C60, doped or undoped nickel oxide, doped or undoped molybdenum oxide, doped or undoped tungsten oxide, doped or undoped vanadium oxide, doped or undoped P-type gallium nitride, doped or undoped chromium oxide, doped or undoped copper oxide, transition metal sulfide and transition metal selenide.

[0035] In a second aspect, the present application provides a method for preparing a photoelectric device, comprising the following steps:

[0036] providing a bottom electrode, and forming an electronic functional layer on one side of the bottom electrode; and

[0037] forming a top electrode on a side of the electronic functional layer away from the bottom electrode;

[0038] Among them, one of the bottom electrode and the top electrode is an anode, and the other is a cathode; the electronic functional layer includes N electron transport layers spaced between the anode and the cathode, and N is a positive integer greater than or equal to 2; the electronic functional layer also includes a nucleophilic functional layer, which is arranged between two adjacent electron transport layers, and the material of the nucleophilic functional layer includes a nucleophilic compound.

[0039] Optionally, at least one nucleophilic functional layer is formed between any two adjacent electron transport layers; and / or

[0040] The nucleophilic compound is selected from one or more of NaNH2, Grignard reagent, Gilman reagent, organic lithium reagent, NaBH4, LiAlH4, amino-substituted coumarin, a first compound and a second compound, wherein the first compound has a structure shown in the following general formula (I):

[0041]

[0042] The second compound has a structure shown in the following general formula (II):

[0043]

[0044] wherein R1 to R6 are independently selected from aliphatic hydrocarbon groups or aromatic hydrocarbon groups; and / or

[0045] The method for forming the electron transport layer comprises the steps of:

[0046] depositing a first solution comprising a first metal oxide; and

[0047] performing a first drying process on the deposited first solution to obtain the electron transport layer;

[0048] Wherein, the first metal oxide is selected from one or more of zinc oxide, titanium oxide, tin oxide, barium oxide, tantalum oxide, aluminum oxide, zirconium oxide, magnesium zinc oxide, calcium zinc oxide, zirconium zinc oxide, gallium zinc oxide, aluminum zinc oxide, lithium zinc oxide, titanium zinc oxide, yttrium zinc oxide, indium tin oxide and lithium titanium oxide; and / or

[0049] The method for forming the nucleophilic functional layer comprises the steps of:

[0050] depositing a second solution comprising a nucleophilic compound; and

[0051] The deposited second solution is subjected to a second drying process to obtain the nucleophilic functional layer.

[0052] Optionally, before the step of performing a first drying treatment on the deposited first solution, the method for forming an electron transport layer further comprises the steps of: placing the deposited first solution in an inert gas atmosphere and allowing it to stand; and / or

[0053] Before the step of performing a second drying treatment on the deposited second solution, the method for forming a nucleophilic functional layer further comprises the step of placing the deposited second solution in an inert gas atmosphere and allowing it to stand.

[0054] Optionally, the electronic functional layer further comprises at least one auxiliary functional layer, wherein the auxiliary functional layer is formed between the adjacent electron transport layer and the nucleophilic functional layer, and / or the auxiliary functional layer is formed between two adjacent nucleophilic functional layers;

[0055] The method for forming the auxiliary functional layer comprises the steps of:

[0056] depositing a third solution comprising a third compound;

[0057] performing a third drying process on the deposited third solution to obtain a solidified film layer whose material is the third compound; and

[0058] Performing light treatment on the cured film layer to cause at least a portion of the third compound to undergo a self-crosslinking reaction to form a crosslinked compound, thereby obtaining the auxiliary functional layer;

[0059] Wherein, the third compound has a structure shown by the following general formula (III):

[0060]

[0061] In the general formula (III), each occurrence of R7 is independently selected from hydrogen atom, -NH2, carboxyl group, hydrocarbon group or -X, X is halogen, and y is a positive integer of 1 to 4.

[0062] Optionally, before the step of performing a third drying treatment on the deposited third solution, the method for forming the auxiliary functional layer further comprises the step of placing the deposited third solution in an inert gas atmosphere and allowing it to stand.

[0063] In a third aspect, the present application provides an electronic device, wherein the electronic device comprises the optoelectronic device as described in any one of the first aspects, or the electronic device comprises the optoelectronic device manufactured by the preparation method as described in any one of the second aspects.

[0064] The present application provides an optoelectronic device, a method for preparing an optoelectronic device, and an electronic device, which have the following technical effects:

[0065] In the optoelectronic device of the present application, the electronic functional layer includes a nucleophilic functional layer, the material of the nucleophilic functional layer includes a nucleophilic compound, the nucleophilic functional layer exhibits the ability to attract holes, and the nucleophilic functional layer is arranged between two adjacent electron transport layers, and will not adversely affect the interface state between the electron transport layer and the light-emitting layer and the interface state between the electron transport layer and the cathode. Therefore, without affecting the electron injection level and reducing the risk of quantum dot quenching, the hole injection level of the optoelectronic device is effectively improved, the electron-hole transfer balance is promoted, and the optoelectronic performance and device life of the optoelectronic device are improved.

[0066] In the preparation method of the optoelectronic device, physical and / or chemical methods can be used to form various functional film layers, which can meet the needs of large-scale industrial production. The optoelectronic device or the optoelectronic device prepared by the preparation method of the optoelectronic device is applied to electronic devices, which is beneficial to improving the display effect and service life of the electronic devices, and is beneficial to improving the performance stability of the electronic devices. BRIEF DESCRIPTION OF THE DRAWINGS

[0067] The technical solution and other beneficial effects of the present application will be made apparent by describing in detail the specific implementation methods of the present application in conjunction with the accompanying drawings.

[0068] Figure 1 A schematic diagram of the structure of a first optoelectronic device provided in an embodiment of the present application;

[0069] Figure 2 A schematic diagram of the structure of a second optoelectronic device provided in an embodiment of the present application;

[0070] Figure 3 A schematic diagram of the structure of a third optoelectronic device provided in an embodiment of the present application;

[0071] Figure 4 A schematic diagram of the structure of a fourth optoelectronic device provided in an embodiment of the present application;

[0072] Figure 5 A schematic diagram of the structure of a fifth optoelectronic device provided in an embodiment of the present application;

[0073] Figure 6 A schematic diagram of the structure of a sixth optoelectronic device provided in an embodiment of the present application;

[0074] Figure 7 A schematic diagram of the structure of the optoelectronic device provided for Comparative Example 1;

[0075] Figure 8 This is a schematic diagram of the structure of the optoelectronic device provided for Comparative Example 2.

[0076] The reference numerals are as follows:

[0077] 1: optoelectronic device, 10: substrate, 11: anode, 12: cathode, 13: light-emitting layer, 14: electron functional layer, 15: hole functional layer, 141: electron transport layer, 142: nucleophilic functional layer, 143: auxiliary functional layer, 151: hole injection layer, 152: hole transport layer. DETAILED DESCRIPTION

[0078] The technical solutions in the embodiments of the present application will be described clearly and completely below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, rather than all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by those skilled in the art without creative work are within the scope of protection of the present application.

[0079] Unless otherwise defined, all professional and scientific terms used herein have the same meanings as those familiar to those skilled in the art. In addition, any methods and materials similar or equivalent to those described herein may be applied to the present invention. The preferred implementation methods and materials described herein are for demonstration purposes only and are not intended to limit the content of this application.

[0080] It should be noted that the order of description of the following embodiments is not intended to limit the preferred order of the embodiments. The various embodiments of the present application may be in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the invention; therefore, it should be considered that the range description has specifically disclosed all possible sub-ranges and single values ​​within the range. For example, it should be considered that the range description from 1 to 6 has specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated in this article, it is meant to include any cited numbers (fractions or integers) within the indicated range.

[0081] In the description of the present application, the term “including” means “including but not limited to”.

[0082] The term "at least one" means one or more, and "multiple" means two or more. The term "at least one", "at least one of the following" or similar expressions refer to any combination of these items, including any combination of single items or plural items. For example, "at least one of a, b or c" or "at least one of a, b and c" can be expressed as: a, b, c, ab (i.e. a and b), ac, bc or abc, where a, b and c can be single or plural, respectively.

[0083] In the present application, the description of "layer A is formed on one side of layer B" or "layer A is formed on the side of layer B away from layer C" may mean that layer A is directly formed on one side of layer B or on the side of layer B away from layer C, that is, layer A is in direct contact with layer B; it may also mean that layer A is indirectly formed on one side of layer B or on the side of layer B away from layer C, that is, other film layers may be formed between layer A and layer B.

[0084] The selection scope of the term "and / or" includes any one of two or more related listed items, and also includes any and all combinations of the related listed items, and the said any and all combinations include any combination of two related listed items, any more related listed items, or all related listed items. For example, "A and / or B" includes three parallel solutions of A, B and A+B. For another example, the technical solution of "A, and / or, B, and / or, C, and / or, D" includes any one of A, B, C, and D (that is, the technical solution connected by "logical or"), and also includes any and all combinations of A, B, C, and D, that is, the combination of any two or any three of A, B, C, and D, and also includes the combination of four items of A, B, C, and D (that is, the technical solution connected by "logical and").

[0085] This embodiment provides a photoelectric device, such as Figure 1 As shown, the photoelectric device 1 includes an anode 11, a cathode 12 and an electronic functional layer 14, wherein the anode 11 and the cathode 12 are arranged opposite to each other, the electronic functional layer 14 is arranged between the anode 11 and the cathode 12, the electronic functional layer 14 includes N electron transport layers 141 arranged between the anode 11 and the cathode 12, N is a positive integer greater than or equal to 2, and the electronic functional layer 14 also includes a nucleophilic functional layer 142, the nucleophilic functional layer 142 is arranged between two adjacent electron transport layers 141, and the material of the nucleophilic functional layer 142 includes a nucleophilic compound. The photoelectric device 1 includes but is not limited to a light emitting device, a solar cell or a photodetector.

[0086] Existing optoelectronic devices have the problem of unbalanced carrier transport. For example, existing QLEDs generally have the problem that the electron injection level is greater than the hole injection level, resulting in limited improvement in the optoelectronic performance and device life of the optoelectronic device. In the optoelectronic device 1 of the embodiment of the present application, the electronic functional layer 14 includes a nucleophilic functional layer 142, and the material of the nucleophilic functional layer 142 includes a nucleophilic compound. The nucleophilic functional layer 142 exhibits the effect of attracting holes, which can promote the electron-hole transport balance, thereby improving the optoelectronic performance and device life of the optoelectronic device 1. In addition, the nucleophilic functional layer 142 is arranged between two adjacent electron transport layers 141, and will not adversely affect the interface state between the electron transport layer 141 and the light-emitting layer 13 and the interface state between the electron transport layer 141 and the cathode 12, thereby effectively improving the hole injection level of the optoelectronic device 1 without affecting the electron injection level and reducing the risk of quantum dot quenching. It can be understood that when the hole injection level of the optoelectronic device 1 is too low, the number of nucleophilic functional layers 142 can be appropriately increased.

[0087] In order to further enhance the charge balance control effect of the optoelectronic device 1 , in some embodiments of the present application, at least one nucleophilic functional layer 142 is provided between any two adjacent electron transport layers 141 .

[0088] In order to further improve the comprehensive performance of the optoelectronic device 1, in some embodiments of the present application, the nucleophilic compound is selected from one or more of NaNH2, Grignard reagent, Gilman reagent, organic lithium reagent, NaBH4, LiAlH4, amino-substituted coumarin, the first compound and the second compound.

[0089] Wherein, the first compound has the structure shown in the following general formula (I):

[0090]

[0091] In the general formula (I), R1 to R3 are independently selected from aliphatic hydrocarbon groups or aromatic hydrocarbon groups. The carbon number of the aliphatic hydrocarbon group can be 1 to 10 or 1 to 20, for example, it can be 1, 3, 5, 7, 9, 10 and a value between any two of the above values. As an example, the aliphatic hydrocarbon group is selected from pentyl, hexyl, heptyl or octyl. The carbon number of the aromatic hydrocarbon group can be 6 to 20, for example, it can be 6, 10, 12, 18, 20 and a value between any two of the above values. As an example, the aromatic hydrocarbon group is selected from phenyl, naphthyl or biphenyl.

[0092] The second compound has the structure shown in the following general formula (II):

[0093]

[0094] In the general formula (II), R4 to R6 are independently selected from aliphatic hydrocarbon groups or aromatic hydrocarbon groups. The carbon number of the aliphatic hydrocarbon group can be 1 to 10 or 1 to 20, for example, 1, 3, 5, 7, 9, 10, and values ​​between any two of the aforementioned values. As an example, the aliphatic hydrocarbon group is selected from pentyl, hexyl, heptyl or octyl. The carbon number of the aromatic hydrocarbon group can be 6 to 20, for example, 6, 10, 12, 18, 20, and values ​​between any two of the aforementioned values. As an example, the aromatic hydrocarbon group is selected from phenyl, naphthyl or biphenyl.

[0095] "Grignard reagent" refers to an organometallic compound containing a magnesium halide, with the general formula R a -Mg-X, where R a is an aliphatic hydrocarbon group or an aromatic hydrocarbon group, and X is a halogen. In the embodiments of the present application, the Grignard reagent includes but is not limited to one or more of CH3-Mg-Br, CH3CH2-Mg-Br, CH3-Mg-Cl and CH3CH2-Mg-Cl.

[0096] "Gilman reagent" is also known as dialkyl copper lithium, and its general structural formula is R b R c CuLi, where R b and R c In the present embodiment, the Gilman reagent includes but is not limited to one or more of (CH3)2CuLi and (CH3CH2)2CuLi.

[0097] "Organolithium reagent" refers to a compound obtained by replacing the hydrogen atoms in an organic compound with lithium, with the general structural formula R d Li, where R d Selected from aliphatic hydrocarbon group or aromatic hydrocarbon group. In the embodiment of the present application, the organic lithium reagent includes but is not limited to one or more of n-butyl lithium, methyl lithium and phenyl lithium.

[0098] "Amino-substituted coumarin" refers to a compound obtained by replacing any one or more hydrogen atoms on coumarin with -NH2. In the present embodiment, amino-substituted coumarin includes but is not limited to one or more of 7-aminocoumarin and 3-aminocoumarin.

[0099] In some embodiments of the present application, when the number of nucleophilic functional layers 142 is at least two, the nucleophilic compounds in each nucleophilic functional layer 142 are independently selected from one or more of NaNH2, Grignard reagent, Gilman reagent, organic lithium reagent, NaBH4, LiAlH4, amino-substituted coumarin, the first compound and the second compound.

[0100] In some embodiments of the present application, the material of the electron transport layer includes a first metal oxide, and the first metal oxide may be undoped or doped. The undoped first metal oxide is, for example, selected from one or more of ZnO, TiO2, SnO2, BaO, Ta2O3, Al2O3 and ZrO2. The doped first metal oxide is, for example, selected from one or more of zinc magnesium oxide, zinc calcium oxide, zinc zirconium oxide, zinc gallium oxide, zinc aluminum oxide, lithium zinc oxide, zinc titanium oxide, yttrium zinc oxide, indium tin oxide and lithium titanium oxide. The doped first metal oxide is exemplified by Zn (1-x) Mg x O, Zn (1-x) Ca x O, Zn (1-x) Zr x O, Zn (1-x) Ga x O, Zn (1-x) Al x O, Zn (1-x) Li x O、Al (1-x) Zn x O, Zn (1-x) Ti x O, Zn (1-x) Y x O、In (1-x) Sn x O and Ti (1-x) Li x One or more of O, where 0<x<1.

[0101] In some embodiments of the present application, the first metal oxide is in the form of nanoparticles, and the average particle size of the first metal oxide is 2nm to 20nm, for example, 2nm, 5nm, 8nm, 10nm, 12nm, 15nm, 18nm, 20nm and values ​​between any two of the aforementioned values.

[0102] In order to improve the comprehensive performance of the optoelectronic device 1 and reduce the manufacturing cost, in some embodiments of the present application, the thickness of the electronic functional layer 14 is 40nm to 200nm, for example, 40nm, 60nm, 70nm, 80nm, 90nm, 100nm, 150nm, 200nm and a value between any two of the foregoing values; and / or, the thickness of each electron transport layer 141 is 7nm to 15nm, for example, 7nm, 8nm, 9nm, 10nm, 11nm, 12nm, 13nm, 14nm, 15nm and a value between any two of the foregoing values; and / or, the total thickness of the N electron transport layers 141 is 30nm to 80nm, for example, 30nm, 40nm, 50nm, 60nm, 70nm, 80nm and values ​​between any two of the aforementioned values; and / or, the total thickness of the nucleophilic functional layer 142 is 7nm~40nm, for example, 7nm, 10nm, 20nm, 30nm, 40nm and values ​​between any two of the aforementioned values. It can be understood that when there is only one nucleophilic functional layer 142, the thickness of the nucleophilic functional layer 142 is 7nm~40nm; and / or, when there are at least two nucleophilic functional layers 142, the thickness of each nucleophilic functional layer 142 is 7nm~15nm, for example, 7nm, 8nm, 9nm, 10nm, 11nm, 12nm, 13nm, 14nm, 15nm and values ​​between any two of the aforementioned values.

[0103] In order to improve the mechanical stress and acid and alkali resistance of the electronic functional layer 14, thereby improving the performance stability of the optoelectronic device 1, in some embodiments of the present application, such as Figure 2 As shown, the electronic functional layer 14 further includes at least one auxiliary functional layer 143, the auxiliary functional layer 143 is disposed between the adjacent electron transport layer 141 and the nucleophilic functional layer 142, and / or the auxiliary functional layer 143 is disposed between two adjacent nucleophilic functional layers 142, and the material of the auxiliary functional layer includes a cross-linking compound, and the cross-linking compound is a compound formed by a self-cross-linking reaction of the third compound. The third compound has a structure shown in the following general formula (III):

[0104] In the general formula (III), each occurrence of R7 is independently selected from a hydrogen atom, -NH2, a carboxyl group, a hydrocarbon group or -X, X is a halogen, and y is a positive integer from 1 to 4; the hydrocarbon group can be an aliphatic hydrocarbon group or an aromatic hydrocarbon group, and the hydrocarbon group is, for example, selected from a methyl group, an ethyl group or a propyl group.

[0105] The third compound contains a coumarin group. Since the coumarin group has a reversible photoresponse property, the third compound also has a reversible photoresponse property. As shown in the following reaction formula (IV), two adjacent third compounds can undergo chemical cross-linking to form a four-membered ring structure under specific lighting conditions (ultraviolet light with an emission wavelength of 363nm to 367nm). It can be deduced that (A+1) third compound molecules can undergo chemical cross-linking to form A four-membered ring structures under specific lighting conditions, where A is a positive integer greater than or equal to 1, so that (A+1) third compound molecules react to form a cross-linked compound.

[0106]

[0107] In order to improve the comprehensive performance of the optoelectronic device 1 and reduce the manufacturing cost, in some embodiments of the present application, the thickness of the auxiliary functional layer is 7nm to 15nm, for example, 7nm, 8nm, 9nm, 10nm, 11nm, 12nm, 13nm, 14nm, 15nm and values ​​between any two of the aforementioned values.

[0108] In order to improve the hole injection level of the optoelectronic device 1 and the mechanical stress and acid and alkali resistance of the electronic functional layer 14, when the optoelectronic device 1 includes the auxiliary functional layer 143, the material of the nucleophilic functional layer 142 does not include coumarin and / or coumarin derivatives, and the coumarin derivatives are, for example, amino-substituted coumarin. The auxiliary functional layer is mainly used as an adhesion layer.

[0109] In some embodiments of the present application, the materials of the anode 11 and the cathode 12 are independently selected from one or more of metals, carbon materials and second metal oxides, wherein the metals include but are not limited to one or more of Al, Ag, Cu, Mo, Au, Ba, Pt, Ca, Ir, Ni and Mg, the carbon materials include but are not limited to one or more of graphite, carbon nanotubes, graphene and carbon fibers, and the second metal oxides include but are not limited to one or more of indium tin oxide (ITO), fluorine-doped tin oxide (FTO), antimony tin oxide (ATO), aluminum-doped zinc oxide (AZO), gallium-doped zinc oxide (GZO), indium-doped zinc oxide (IZO), magnesium-doped zinc oxide (MZO), SnO2, ZnO and In2O3. The anode 11 or the cathode 12 may also be a composite electrode, which has a structure similar to a "sandwich", wherein the materials of the upper and lower layers are respectively doped or undoped transparent metal oxides, and the material of the middle layer is a metal, for example, it may be one or more of AZO / Ag / AZO, AZO / Al / AZO, ITO / Ag / ITO, ITO / Al / ITO, ZnO / Ag / ZnO, ZnO / Al / ZnO, TiO2 / Ag / TiO2, TiO2 / Al / TiO2, ZnS / Ag / ZnS, ZnS / Al / ZnS, TiO2 / Ag / TiO2 and TiO2 / Al / TiO2, and the thickness of the middle layer does not exceed 35nm. The thickness of the anode 11 may be, for example, 20nm to 300nm, and the thickness of the cathode 12 may be, for example, 20nm to 300nm.

[0110] In some embodiments of the present application, the optoelectronic device 1 is a light emitting device. Figure 1 The optoelectronic device 1 further includes a light-emitting layer 13, which is disposed between the anode 11 and the electronic functional layer 14. The light-emitting layer 13 is a single-layer structure or a multi-layer structure. The light-emitting layer 13 may be, for example, two or more layers. The thickness of the light-emitting layer 13 may be, for example, 10 nm to 100 nm. In some embodiments of the present application, the material of the light-emitting layer 13 includes one or more of an organic light-emitting material and a quantum dot.

[0111] Among them, the organic light-emitting materials include but are not limited to 4,4'-bis(N-carbazole)-1,1'-biphenyl:tri[2-(p-tolyl)pyridine iridium(III), 4,4',4"-tri(carbazole-9-yl)triphenylamine:tri[2-(p-tolyl)pyridine iridium, diaromatic anthracene derivatives, distilbene aromatic derivatives, pyrene derivatives, fluorene derivatives, TBPe fluorescent materials, TTPX fluorescent materials, TBRb fluorescent materials, DBP fluorescent materials, delayed fluorescent materials, TTA materials, thermally activated delayed materials, polymers containing BN covalent bonds, hybrid localized charge transfer excited state materials and exciplex light-emitting materials. One or more.

[0112] Quantum dots include but are not limited to one or more of red quantum dots, green quantum dots and blue quantum dots, and quantum dots include but are not limited to one or more of single component quantum dots, core-shell structure quantum dots, inorganic perovskite quantum dots, organic perovskite quantum dots and organic-inorganic hybrid perovskite quantum dots. The average particle size of the quantum dots can be, for example, 5nm to 10nm, and the average particle size of the quantum dots is exemplified as 5nm, 6nm, 7nm, 8nm, 9nm or 10nm.

[0113] For single-component quantum dots and core-shell structure quantum dots, the material of the single-component quantum dots, the material of the core of the core-shell structure quantum dots or the material of the shell of the core-shell structure quantum dots is, but is not limited to, at least one of a II-VI group compound, a III-V group compound, a IV-VI group compound or a I-III-VI group compound, wherein the II-VI group compound is selected from CdS, CdSe, CdTe, ZnS, ZnSe, ZnTe, ZnO, HgS, HgSe, HgTe, CdSeS, CdSeTe, CdSTe, ZnSeS, ZnSeTe, Zn One or more of CdZnS, CdZnSe, CdZnTe, CdHgS, CdHgSe, CdHgTe, HgZnS, HgZnSe, HgZnTe, CdZnSeS, CdZnSeTe, CdZnSTe, CdHgSeS, CdHgSeTe, CdHgSTe, HgZnSeS, HgZnSeTe and HgZnSTe, and the III-V compound is selected from GaN, GaP, GaAs, GaSb, AlN, AlP, Al As, AlSb, InN, InP, InAs, InSb, GaNP, GaNAs, GaNSb, GaPAs, GaPSb, AlNP, AlNAs, AlNSb, AlPAs, AlPSb, InNP, InNAs, InNSb, I nPAs, InPSb, GaAlNP, GaAlNAs, GaAlNSb, GaAlPAs, GaAlPSb, GaInNP, GaInNAs, GaInNSb, GaInPAs, GaInPSb, InAlNP, InAlNA s, InAlNSb, InAlPAs and InAlPSb, the IV-VI group compound is selected from one or more of SnS, SnSe, SnTe, PbS, PbSe, PbTe, SnSeS, SnSeTe, SnSTe, PbSeS, PbSeTe, PbSTe, SnPbS, SnPbSe, SnPbTe, SnPbSSe, SnPbSeTe and SnPbSTe, and the I-III-VI group compound is selected from one or more of CuInS, CuInSe and AgInS. It should be noted that for the material of the aforementioned single-component quantum dots, or the material of the core of the core-shell structure quantum dots, or the material of the shell of the core-shell structure quantum dots, the chemical formula provided only indicates the elemental composition, and does not indicate the content of each element. For example: CdZnSe only indicates that it is composed of three elements: Cd, Zn and Se. If the content of each element is indicated, it corresponds to Cd x Zn 1-x Se,0 <x<1。

[0114] For inorganic perovskite quantum dots, the general structural formula of inorganic perovskite quantum dots is AMX3, where A is Cs + ion, M is a divalent metal cation, M includes but is not limited to Pb 2+ Sn 2+ , Cu 2+ 、Ni 2+ 、Cd 2+ Cr 2+ , Mn 2+ 、Co 2+ , Fe 2+ ,Ge 2+ , Yb 2+ or Eu 2+ , X is a halogen anion, including but not limited to Cl - Br - or I - .

[0115] For organic perovskite quantum dots, the general structural formula of organic perovskite quantum dots is CMX3, wherein C is a carboxamidine group, and M is a divalent metal cation, and M includes but is not limited to Pb 2+ Sn 2+ , Cu 2+ 、Ni 2+ 、Cd 2+ Cr 2+ , Mn 2+ 、Co 2+ , Fe 2+ ,Ge 2+ , Yb 2+ or Eu 2+ , X is a halogen anion, including but not limited to Cl - Br - or I - .

[0116] For organic-inorganic hybrid perovskite quantum dots, the general structural formula of organic-inorganic hybrid perovskite quantum dots is BMX3, wherein B is selected from organic amine cations, and the organic amine cations include but are not limited to CH3(CH2) n-2 NH 3+ (n≥2) or NH3(CH2) n NH3 2+ (n≥2), M is a divalent metal cation, including but not limited to Pb 2+ Sn 2+ , Cu 2+ 、Ni 2+ 、Cd 2+ Cr 2+ , Mn 2+ 、Co 2+ , Fe2+ ,Ge 2+ , Yb 2+ or Eu 2+ , X is a halogen anion, including but not limited to Cl - Br - or I - .

[0117] It is understood that when the material of the light-emitting layer 13 includes quantum dots, the material of the light-emitting layer 13 also includes ligands connected to the surface of the quantum dots, and the ligands include but are not limited to at least one of amine ligands, carboxylic acid ligands, thiol ligands, (oxy)phosphine ligands, phospholipids, phospholipids or polyvinyl pyridine, and the amine ligands are selected from one or more of methylamine, ethylamine, propylamine, butylamine, pentylamine, hexylamine, octylamine, nonylamine, decylamine, dodecylamine, hexadecylamine, octadecylamine, dimethylamine, diethylamine, dipropylamine, tributylamine and trioctylamine. The carboxylic acid ligand is, for example, selected from one or more of formic acid, acetic acid, propionic acid, butyric acid, pentanoic acid, hexanoic acid, heptanoic acid, octanoic acid, dodecanoic acid, hexadecanoic acid, octadecanoic acid, oleic acid and benzoic acid; the thiol ligand is, for example, selected from one or more of methyl mercaptan, ethyl mercaptan, propyl mercaptan, butyl mercaptan, pentyl mercaptan, hexanethiol, octadecyl mercaptan, dodecanethiol, hexadecanethiol, octadecanethiol and benzyl mercaptan; the (oxygen) phosphine ligand is selected from one or more of methyl phosphine, ethyl phosphine, propyl phosphine, butyl phosphine, pentyl phosphine, octyl phosphine, dioctyl phosphine, tributyl phosphine and trioctyl phosphine.

[0118] In order to further improve the photoelectric performance and device life of the photoelectric device 1, in some embodiments of the present application, continue to refer to Figure 1 and Figure 2 The photoelectric device 1 further includes a hole functional layer 15 disposed between the anode 11 and the electronic functional layer 14. When the photoelectric device 1 is a light-emitting device, the hole functional layer 15 is located between the anode 11 and the light-emitting layer 13. The hole functional layer 15 may be a single-layer structure or a multi-layer structure. The hole functional layer 15 may include, for example, one or more of a hole injection layer, a hole transport layer, and an electron blocking layer. For the electronic functional layer 14 including the hole injection layer, the hole transport layer, and the electron blocking layer, the hole injection layer, the hole transport layer, and the electron blocking layer may be disposed in sequence, and the hole injection layer is closer to the anode 11 than the electron blocking layer. The thickness of the hole functional layer 15 may be, for example, 10 nm to 200 nm.

[0119] The material of the hole functional layer 15 includes, but is not limited to, poly(3,4-ethylenedioxythiophene):poly(styrenesulfonic acid), copper phthalocyanine, titanium phthalocyanine, 2,3,5,6-tetrafluoro-7,7',8,8'-tetracyanodimethyl-p-benzoquinone, 2,3,6,7,10,11-hexycyano-1,4,5,8,9,12-hexaazatriphenylene, 3-hexyl substituted polythiophene, poly(9-vinylcarbazole), 4,4'-di(9-carbazole)biphenyl, poly[bis(4-phenyl)(4-butylphenyl)amine], 4,4'-cyclohexylbis[N,N-di(4-methylphenyl)aniline], poly[(9,9-dioctylfluorenyl-2,7-diyl)-co-(4,4'-(N-(4-sec-butylphenyl)phenyl)amine] )diphenylamine)], poly[(9,9-dioctylfluorenyl-2,7-diyl)-co-(4,4'-(N-(p-butylphenyl))diphenylamine)], poly(N,N'-di(4-butylphenyl)-N,N'-diphenyl-1,4-phenylenediamine-co-9,9-dioctylfluorene), 4,4',4'-tri(N-3-methylphenyl-N-phenylamino)triphenylamine, 4,4',4"-tri(carbazol-9-yl)triphenylamine, 4,4',4'-tri(2-naphthylphenylamino)triphenylamine, N,N'-diphenyl-N,N'-(1-naphthyl)-1,1'-biphenyl-4,4'-diamine, N,N'-diphenyl-N,N'-di(3-methylphenyl)-1,1'-biphenyl -4,4'-diamine, N,N'-bis[4-(diphenylamino)phenyl]-N,N'-diphenylbenzidine, N,N'-bis(3-methylphenyl)-N,N'-diphenyl-9,9-spirobifluorene-2,7-diamine, N2,N7-di-1-naphthyl-N2,N7-diphenyl-9,9'-spirobi[9H-fluorene]-2,7-diamine, poly[bis(4-phenyl)(2,4,6-trimethylphenyl)amine], 2,2',7,7'-tetrakis[N,N-di(4-methoxyphenyl)amino]-9,9'-spirobifluorene, doped or undoped graphene, C60, doped or undoped nickel oxide, doped or undoped molybdenum oxide, doped or undoped tungsten oxide, doped or undoped oxide Vanadium sulfide, doped or undoped P-type gallium nitride, doped or undoped chromium oxide, doped or undoped copper oxide, transition metal sulfide and transition metal selenide. Among them, transition metal sulfide includes but is not limited to one or more of molybdenum sulfide, tungsten sulfide and copper sulfide; transition metal selenide includes but is not limited to one or more of molybdenum selenide and tungsten selenide; doped or undoped nickel oxide is exemplified by NiO, doped or undoped molybdenum oxide is exemplified by MoO3, doped or undoped tungsten oxide is exemplified by WO3, doped or undoped vanadium oxide is exemplified by V2O5, doped or undoped chromium oxide is exemplified by CrO3, doped or undoped copper oxide is exemplified by CuO and Cu2O.

[0120] The present application also provides a method for preparing a photoelectric device, which can be used to prepare any of the photoelectric devices described above. The method for preparing a photoelectric device comprises the following steps:

[0121] S1. providing a bottom electrode and forming an electronic functional layer on one side of the bottom electrode;

[0122] S2. Form a top electrode on a side of the electronic functional layer away from the bottom electrode.

[0123] Among them, one of the bottom electrode and the top electrode is an anode, and the other is a cathode; the electronic functional layer includes N electron transport layers arranged between the anode and the cathode, N is a positive integer greater than or equal to 2; the electronic functional layer also includes a nucleophilic functional layer, the nucleophilic functional layer is arranged between two adjacent electron transport layers, and the material of the nucleophilic functional layer includes a nucleophilic compound. The structural composition of the anode, cathode, electron transport layer and nucleophilic functional layer and the positional relationship between them are all referred to the above description, and the selection of the types of nucleophilic compounds is also referred to the above description.

[0124] In some embodiments of the present application, the method for forming an electron transport layer comprises the following steps:

[0125] S11, depositing a first solution containing a first metal oxide;

[0126] S12, performing a first drying process on the deposited first solution to obtain an electron transport layer.

[0127] The first metal oxide is described above. The solvent of the first solution includes, but is not limited to, one or more of alkanes, aromatic hydrocarbons, halogenated alkanes, alcohol compounds, ether compounds, furan compounds, pyridine compounds, and amide compounds, wherein alkanes include, but are not limited to, one or more of nonane, decane, dodecane, terpene, butylcyclohexane, n-octane, n-hexane, n-heptane, n-nonane, n-decane, cyclohexane, and cyclopentane, and aromatic hydrocarbons include, but are not limited to, one or more of diethylbenzene, trimethylbenzene, propylbenzene, isopropylbenzene, p-toluene isopropylbenzene, butylbenzene, and 1-methylnaphthalene or indene. , halogenated alkanes include but are not limited to one or more of dichloromethane, chloroform and carbon tetrachloride, alcohol compounds include but are not limited to one or more of methanol, ethanol, propanol, butanol, ethylene glycol and glycerol, ether compounds include but are not limited to ethylene glycol monomethyl ether, furan compounds include but are not limited to tetrahydrofuran, pyridine compounds include but are not limited to pyridine, amide compounds include but are not limited to N,N-dimethylformamide, and the solvent of the first solution is exemplified by alcohol compounds with 1 to 10 carbon atoms (such as methanol or ethanol). The concentration of the first metal oxide in the first solution is, for example, 10 mg / mL to 50 mg / mL.

[0128] In step S11, the deposition method of the first solution includes but is not limited to one or more of spin coating, printing, inkjet printing, doctor blading, printing, dip-coating, immersion, spraying, roll coating, casting, slit coating, strip coating and solution electrodeposition.

[0129] In step S12, "drying treatment" includes all processes that can enable the deposited first solution to obtain higher energy and solidify into a film, including but not limited to heating treatment, vacuum drying treatment or air drying treatment, wherein the temperature of the heating treatment can be constant temperature or non-constant temperature (for example, the temperature changes in a gradient). As an example, the drying treatment is a heating treatment, and the temperature of the heating treatment is 80°C to 300°C. It should be noted that after a cured film layer is formed by a low-temperature (temperature not higher than 80°C) drying treatment process such as vacuum drying treatment and air drying treatment, in order to further improve the film quality, the cured film layer can be further annealed by a process that can control the annealing depth, such as pulsed laser annealing, electron beam annealing, atomic annealing, infrared radiation annealing, etc.

[0130] In order to achieve mutual dissolution between adjacent film layers to enhance the mechanical stress and acid-base resistance of the electronic functional layer, in some embodiments of the present application, between step S11 and step S12, the method for forming an electron transport layer also includes the step of: placing the deposited first solution in an inert gas atmosphere and letting it stand for, for example, 1 min to 5 min, and the gas pressure of the inert gas atmosphere is, for example, not less than 10 KPa.

[0131] In some embodiments of the present application, the method for forming the nucleophilic functional layer comprises the following steps:

[0132] S21, depositing a second solution containing a nucleophilic compound;

[0133] S22, performing a second drying process on the deposited second solution to obtain the nucleophilic functional layer.

[0134] The solvent of the second solution refers to the above description of the solvent of the first solution. For example, the solvent of the second solution is an alcohol compound having 1 to 10 carbon atoms (such as methanol or ethanol).

[0135] In step S21, the deposition method of the second solution includes, but is not limited to, one or more of spin coating, printing, inkjet printing, doctor blade coating, printing, dip-coating, immersion, spraying, roll coating, casting, slit coating, strip coating, and solution electrodeposition. The concentration of the nucleophilic compound in the second solution is, for example, 1 mg / mL to 10 mg / mL.

[0136] In step S22, the second drying process is carried out with reference to the above description of the first drying process.

[0137] In order to achieve mutual dissolution between adjacent film layers to enhance the mechanical stress and acid-base resistance of the electronic functional layer, in some embodiments of the present application, between step S21 and step S22, the method for forming a nucleophilic functional layer also includes the step of: placing the deposited second solution in an inert gas atmosphere and letting it stand for, for example, 1 min to 5 min, and the gas pressure of the inert gas atmosphere is, for example, not less than 10 KPa.

[0138] In order to further improve the mechanical stress and acid and alkali resistance of the electronic functional layer, thereby further improving the performance stability of the optoelectronic device, in some embodiments of the present application, the electronic functional layer further includes at least one auxiliary functional layer, the auxiliary functional layer is formed between the adjacent electron transport layer and the nucleophilic functional layer, and / or the auxiliary functional layer is formed between two adjacent nucleophilic functional layers. The structural composition of the auxiliary functional layer is described above.

[0139] The method for forming the auxiliary functional layer comprises the following steps:

[0140] S31, depositing a third solution containing a third compound;

[0141] S32, performing a third drying process on the deposited third solution to obtain a solidified film layer whose material is the third compound;

[0142] S33, subjecting the cured film layer obtained in step S32 to light treatment to allow at least a portion of the third compound to undergo a self-crosslinking reaction to form a crosslinked compound, thereby obtaining an auxiliary functional layer.

[0143] Wherein, in step S31, the third compound is described in the foregoing description, and the solvent of the third solution is described in the foregoing description of the solvent of the first solution. The solvent of the third solution is an alcohol compound having 1 to 10 carbon atoms (e.g., methanol or ethanol). The concentration of the third compound in the third solution is, for example, 1 mg / mL to 10 mg / mL. The deposition method of the third solution includes, but is not limited to, one or more of spin coating, printing, inkjet printing, blade coating, printing, dip-coating, immersion, spraying, roll coating, casting, slit coating, strip coating, and solution electrodeposition.

[0144] In step S32, the third drying treatment includes but is not limited to heating treatment, vacuum drying treatment or air drying treatment. It should be noted that during the third drying treatment, the third compound will not undergo self-crosslinking reaction to form a crosslinked compound.

[0145] In step S33, "light treatment" is to irradiate the cured film layer with ultraviolet light having an emission wavelength of 363nm to 367nm, so that at least part of the third compound therein undergoes a self-crosslinking reaction to form a cross-linked compound. The pulse width of the ultraviolet laser is, for example, 22ns, the power is, for example, 5W, the frequency is, for example, 1.2Hz, and the time is, for example, 30s to 90s.

[0146] In order to achieve mutual dissolution between adjacent film layers to further enhance the mechanical stress and acid and alkali resistance of the electronic functional layer, thereby further enhancing the performance stability of the optoelectronic device, in some embodiments of the present application, between step S31 and step S32, the method for forming an auxiliary functional layer also includes the step of: placing the deposited third solution in an inert gas atmosphere and allowing it to stand for, for example, 1 min to 5 min, and the pressure of the inert gas atmosphere is, for example, not less than 10 KPa.

[0147] In some embodiments of the present application, when the optoelectronic device is a light-emitting device, the method for preparing the optoelectronic device further includes the step of: forming a light-emitting layer between the electronic functional layer and the anode. The structural composition of the light-emitting layer refers to the above description. For example, when the optoelectronic device is an upright structure, before the step of forming the electronic functional layer on one side of the bottom electrode, the method for preparing the optoelectronic device further includes the step of: forming a light-emitting layer on one side of the bottom electrode; the electronic functional layer is formed on the side of the light-emitting layer away from the bottom electrode. For another example, when the optoelectronic device is an inverted structure, before the step of forming the top electrode on the side of the electronic functional layer away from the bottom electrode, the method for preparing the optoelectronic device further includes the step of: forming a light-emitting layer on the side of the electronic functional layer away from the bottom electrode; the top electrode is formed on the side of the light-emitting layer away from the electronic functional layer.

[0148] When the optoelectronic device is a light-emitting device, in order to further improve the hole injection level of the optoelectronic device, in some embodiments of the present application, when the optoelectronic device is a positive structure, before the step of forming the light-emitting layer on one side of the bottom electrode, the method for preparing the optoelectronic device further includes the steps of: forming a hole functional layer on one side of the bottom electrode; the light-emitting layer is formed on the side of the hole functional layer away from the bottom electrode. Alternatively, in other embodiments of the present application, when the optoelectronic device is an inverted structure, before the step of forming the top electrode on the side of the light-emitting layer away from the electron functional layer, the method for preparing the optoelectronic device further includes the steps of: forming a hole functional layer on the side of the light-emitting layer away from the electron functional layer; the top electrode is formed on the side of the hole functional layer away from the light-emitting layer.

[0149] It should be noted that, in addition to the electronic functional layer, the preparation methods of other functional film layers in the optoelectronic device include but are not limited to chemical methods and / or physical methods. Among them, the chemical method includes but is not limited to one or more of chemical vapor deposition, continuous ion layer adsorption and reaction, anodization, electrolytic deposition and coprecipitation. Physical methods include but are not limited to physical plating and solution methods. Physical plating methods include but are not limited to thermal evaporation, electron beam evaporation, magnetron sputtering, multi-arc ion plating, physical vapor deposition, atomic layer deposition and pulsed laser deposition. One or more of solution methods include but are not limited to spin coating, printing, inkjet printing, scraping, printing, dip-pull, immersion, spraying, roll coating, casting, slit coating and strip coating. When a solution method is used to form a functional film layer, a drying process needs to be added to transform the wet film into a cured film. The drying process includes but is not limited to heat treatment, vacuum drying, air drying, etc. Among them, for the functional film layer located above the light-emitting layer (the material is an inorganic compound, especially inorganic nanoparticles), after a cured film is formed by a low-temperature (temperature not higher than 80°C) drying process such as vacuum drying and air drying, in order to further improve the film quality, the cured film can be further annealed by a process that can control the annealing depth, such as pulsed laser annealing, electron beam annealing, atomic annealing, infrared radiation annealing, etc.

[0150] After the preparation of each functional film layer of the optoelectronic device is completed, a packaging process is required. The packaging process can be carried out by commonly used machine packaging or manual packaging. In the packaging process environment, the oxygen content and water content are both lower than 0.1ppm to ensure the stability of the optoelectronic device.

[0151] The present application also provides an electronic device, the electronic device includes any one of the optoelectronic devices described in the present application, or the electronic device includes the optoelectronic device prepared by any one of the preparation methods described in the present application. The electronic device can be, for example, any electronic product with a display function, including but not limited to a smart phone, a tablet computer, a laptop computer, a digital camera, a digital video camera, a smart wearable device, a smart weighing electronic scale, a car display, a television or an e-book reader, wherein the smart wearable device can be, for example, a smart bracelet, a smart watch, a virtual reality (VR) helmet, etc.

[0152] The technical scheme and technical effects of the present application are described in detail below through specific embodiments, comparative examples and experimental examples. The following embodiments are only some embodiments of the present application and do not specifically limit the present application.

[0153] Example 1

[0154] This embodiment provides a photoelectric device and a method for preparing the same. The photoelectric device is a quantum dot light emitting diode of an upright structure, such as Figure 3 As shown, in the direction from bottom to top, the photoelectric device 1 includes a substrate 10, an anode 11, a hole functional layer 15, a light-emitting layer 13, an electronic functional layer 14 and a cathode 12 which are stacked in sequence, wherein the hole functional layer 15 is composed of a hole injection layer 151 and a hole transport layer 152 which are stacked, and the hole injection layer 151 is closer to the anode 11 than the hole transport layer 152. The electronic functional layer 14 includes a first electron transport layer 141-1, a first auxiliary functional layer 143-1, a first nucleophilic functional layer 142-1, a second auxiliary functional layer 143-2, a second electron transport layer 141-2, a third auxiliary functional layer 143-3, a second nucleophilic functional layer 142-2, a fourth auxiliary functional layer 143-4, a third electron transport layer 141-3, a fifth auxiliary functional layer 143-5, a third nucleophilic functional layer 142-3, a sixth auxiliary functional layer 143-6 and a fourth electron transport layer 141-4, which are stacked in sequence, wherein the first electron transport layer 141-1 is closer to the light-emitting layer 13 than the fourth electron transport layer 141-4.

[0155] The materials and thicknesses of the various layers in the optoelectronic device 1 are as follows:

[0156] The material of the substrate 10 is glass, and the thickness of the substrate 10 is 2 mm;

[0157] The material of the anode 11 is ITO, and the thickness of the anode 11 is 20 nm;

[0158] The material of the cathode 12 is Ag, and the thickness of the cathode 12 is 100 nm;

[0159] The material of the light-emitting layer 13 is CdZnSe (core) / ZnSe (shell) quantum dots, the light-emitting color is blue, the average particle size of the quantum dots is 7nm, and the thickness of the light-emitting layer 13 is 30nm;

[0160] The material of the hole injection layer 151 is PEDOT:PSS, and the thickness of the hole injection layer 151 is 25 nm;

[0161] The material of the hole transport layer 152 is TFB, and the thickness of the hole transport layer 152 is 30 nm;

[0162] The materials of the first electron transport layer 141 - 1 to the fourth electron transport layer 141 - 4 are respectively nano ZnO (average particle size is 5 nm), and the thicknesses of the first electron transport layer 141 - 1 to the fourth electron transport layer 141 - 4 are respectively 15 nm;

[0163] The materials of the first nucleophilic functional layer 142 - 1 to the third nucleophilic functional layer 142 - 3 are LiAlH 4 , and the thicknesses of the first nucleophilic functional layer 142 - 1 to the third nucleophilic functional layer 142 - 3 are 7 nm, respectively;

[0164] The materials of the first to sixth auxiliary functional layers 143 - 1 to 143 - 6 respectively include cross-linked compounds formed by self-cross-linking reaction of 7-aminocoumarin, and the thicknesses of the first to sixth auxiliary functional layers 143 - 1 to 143 - 6 are respectively 7 nm.

[0165] The method for preparing the optoelectronic device in this embodiment comprises the following steps:

[0166] S1.1. Provide a substrate, sputter ITO on one side of the substrate to obtain an ITO layer, wipe the surface of the ITO layer with a cotton swab dipped in a small amount of soapy water to remove impurities visible to the naked eye on the surface, and then ultrasonically clean the substrate including the ITO with deionized water for 15 minutes, acetone for 15 minutes, ethanol for 15 minutes, and isopropanol for 15 minutes, and then dry and perform ultraviolet-ozone surface treatment for 20 minutes to obtain a substrate including an anode;

[0167] S1.2, in an air environment at room temperature and pressure, spin-coating a 2.8% by mass PEDOT:PSS aqueous solution on the side of the anode away from the substrate, and then subjecting the anode to a constant temperature heat treatment at 150°C to solidify the film to obtain a hole injection layer;

[0168] S1.3, in a nitrogen environment at room temperature and pressure, spin-coat a TFB-chlorobenzene solution with a concentration of 8 mg / mL on the side of the hole injection layer away from the anode, and then heat-treat at 150°C to solidify the film to obtain a hole transport layer;

[0169] S1.4. Under a nitrogen environment at room temperature and pressure, a 20 mg / mL CdZnSe / ZnSe quantum dot-n-octane solution was spin-coated on the side of the hole transport layer away from the hole injection layer, and then placed at 10 -2 Perform vacuum drying treatment under MPa environment to solidify into a film to obtain a light-emitting layer;

[0170] S1.5. In a nitrogen environment at room temperature and pressure, a 30 mg / mL nano ZnO-ethanol solution was spin-coated on the side of the light-emitting layer away from the hole transport layer, and then placed in a 10 -2 Perform vacuum drying treatment under MPa environment to solidify into a film, thereby obtaining a first electron transport layer;

[0171] S1.6. In a nitrogen environment at room temperature and pressure, a 3 mg / mL 7-aminocoumarin-ethanol solution was spin-coated on the side of the first electron transport layer away from the light-emitting layer, and then the ambient pressure was adjusted to 35 KPa, and the mixture was allowed to stand for 2 min, and then placed at 10 -2 Perform vacuum drying treatment under MPa environment to solidify into a film, thereby obtaining a first auxiliary functional layer;

[0172] S1.7, in a nitrogen environment at room temperature and pressure, spin-coat a 6 mg / mL LiAlH4-ethanol solution on the side of the first auxiliary functional layer away from the first electron transport layer, then adjust the ambient pressure to 35 KPa, let it stand for 2 minutes, and then place it at 10 -2 Perform vacuum drying treatment under MPa environment to solidify into a film, thereby obtaining a first nucleophilic functional layer;

[0173] S1.8. In a nitrogen environment at room temperature and pressure, a 3 mg / mL 7-aminocoumarin-ethanol solution was spin-coated on the side of the first nucleophilic functional layer away from the first auxiliary functional layer, and then the ambient pressure was adjusted to 35 KPa, and the mixture was allowed to stand for 2 minutes, and then placed at 10 -2 Perform vacuum drying treatment under MPa environment to solidify into a film, thereby obtaining a second auxiliary functional layer;

[0174] S1.9, in a nitrogen environment at room temperature and pressure, spin-coat a 30 mg / mL nano ZnO-ethanol solution on the side of the second auxiliary functional layer away from the first nucleophilic functional layer, then adjust the ambient pressure to 35 KPa, let it stand for 2 minutes, and then place it at 10 -2 Perform vacuum drying treatment under MPa environment to solidify into a film, thereby obtaining a second electron transport layer;

[0175] S1.10. In a nitrogen environment at room temperature and pressure, a 3 mg / mL 7-aminocoumarin-ethanol solution was spin-coated on the side of the second electron transport layer away from the second auxiliary functional layer, and then the ambient pressure was adjusted to 35 KPa, and the mixture was allowed to stand for 2 minutes, and then placed at 10 -2 Perform vacuum drying treatment under MPa environment to solidify into a film, thereby obtaining a third auxiliary functional layer;

[0176] S1.11. In a nitrogen environment at room temperature and pressure, spin-coat a 6 mg / mL LiAlH4-ethanol solution on the side of the third auxiliary functional layer away from the second electron transport layer, then adjust the ambient pressure to 35 KPa, let it stand for 2 minutes, and then place it at 10 -2 MPa environment, vacuum drying treatment is performed to solidify the film to obtain a second nucleophilic functional layer;

[0177] S1.12. In a nitrogen environment at room temperature and pressure, a 3 mg / mL 7-aminocoumarin-ethanol solution was spin-coated on the side of the second nucleophilic functional layer away from the third auxiliary functional layer, and then the ambient pressure was adjusted to 35 KPa, and the mixture was allowed to stand for 2 minutes, and then placed at 10 -2 MPa environment, vacuum drying treatment is performed to solidify the film to obtain a fourth auxiliary functional layer;

[0178] S1.13, in a nitrogen environment at room temperature and pressure, spin-coat a 30 mg / mL nano ZnO-ethanol solution on the side of the fourth auxiliary functional layer away from the second nucleophilic functional layer, then adjust the ambient pressure to 35 KPa, let it stand for 2 minutes, and then place it at 10 -2 MPa environment, vacuum drying treatment is performed to solidify the film to obtain a third electron transport layer;

[0179] S1.14. In a nitrogen environment at room temperature and pressure, a 3 mg / mL 7-aminocoumarin-ethanol solution was spin-coated on the side of the third electron transport layer away from the fourth auxiliary functional layer, and then the ambient pressure was adjusted to 35 KPa, and the mixture was allowed to stand for 2 minutes, and then placed at 10 -2 MPa environment, vacuum drying treatment is performed to solidify the film to obtain the fifth auxiliary functional layer;

[0180] S1.15. In a nitrogen environment at room temperature and pressure, a 6 mg / mL LiAlH4-ethanol solution was spin-coated on the side of the fifth auxiliary functional layer away from the third electron transport layer, and then the ambient pressure was adjusted to 35 KPa, and the mixture was allowed to stand for 2 min, and then placed at 10 -2 MPa environment, vacuum drying treatment is performed to solidify the film to obtain a third nucleophilic functional layer;

[0181] S1.16, in a nitrogen environment at room temperature and pressure, spin-coat a 3 mg / mL 7-aminocoumarin-ethanol solution on the side of the third nucleophilic functional layer away from the fifth auxiliary functional layer, then adjust the ambient pressure to 35 KPa, let it stand for 2 minutes, and then place it at 10 -2 Perform vacuum drying treatment under MPa environment to solidify into a film, thereby obtaining a sixth auxiliary functional layer;

[0182] S1.17, in a nitrogen environment at room temperature and pressure, spin-coat a 30 mg / mL nano ZnO-ethanol solution on the side of the sixth auxiliary functional layer away from the third nucleophilic functional layer, then adjust the ambient pressure to 35 KPa, let it stand for 2 minutes, and then place it at 10 -2 MPa environment, vacuum drying treatment is performed to solidify the film to obtain a fourth electron transport layer;

[0183] S1.18, subjecting the prefabricated device having completed S1.17 to ultraviolet light treatment, so as to cause at least part of the 7-aminocoumarin in the first auxiliary functional layer to the sixth auxiliary functional layer to undergo self-crosslinking reaction to form a crosslinked compound, wherein the process parameters of the ultraviolet light treatment are: the wavelength of the light is 365 nm, the pulse width of the ultraviolet laser is 22 ns, the power is 5 W, the frequency is 1.2 Hz, and the time is 90 s;

[0184] S1.19, vacuum degree not higher than 3×10 -4 In the evaporation chamber of Pa, Ag is evaporated on the side of the fourth electron transport layer away from the sixth auxiliary functional layer to obtain a cathode, which is then encapsulated with epoxy resin to obtain a photoelectric device.

[0185] Example 2

[0186] This embodiment provides a photoelectric device and a method for preparing the same. Compared with the photoelectric device in Embodiment 1, the difference of the photoelectric device in this embodiment is that the materials of the first nucleophilic functional layer to the third nucleophilic functional layer are respectively replaced with "CH3-Mg-Br".

[0187] The preparation method of the optoelectronic device in this embodiment is carried out with reference to that in Embodiment 1.

[0188] Example 3

[0189] This embodiment provides a photoelectric device and a preparation method thereof. Compared with the photoelectric device in Example 1, the difference of the photoelectric device in this embodiment is that the materials of the first nucleophilic functional layer to the third nucleophilic functional layer are respectively replaced with "trioctylamine (CAS No. 1116-76-3)".

[0190] The preparation method of the optoelectronic device in this embodiment is carried out with reference to that in Embodiment 1.

[0191] Example 4

[0192] This embodiment provides a photoelectric device and a method for preparing the same. Compared with the photoelectric device in Embodiment 1, the difference of the photoelectric device in this embodiment is that the materials of the first nucleophilic functional layer to the third nucleophilic functional layer are respectively replaced with "dimethyl copper lithium (CAS No. 15681-48-8)".

[0193] The preparation method of the optoelectronic device in this embodiment is carried out with reference to that in Embodiment 1.

[0194] Example 5

[0195] This embodiment provides a photoelectric device and a method for preparing the same. The structure and composition of the photoelectric device in this embodiment are the same as those in Embodiment 1.

[0196] Compared with the method for preparing the optoelectronic device in Example 1, the difference in the method for preparing the optoelectronic device in this embodiment is that the process of "then adjusting the ambient pressure to 35 Kpa and standing for 2 minutes" in steps S1.6 to S1.17 is omitted.

[0197] Example 6

[0198] This embodiment provides a photoelectric device and a method for preparing the same. Compared with the photoelectric device in Embodiment 1, Figure 4 As shown, the difference of the optoelectronic device in this embodiment is that the first to sixth auxiliary functional layers are omitted.

[0199] Compared with the method for preparing the optoelectronic device in Example 1, the method for preparing the optoelectronic device in this embodiment is different in that the steps of preparing the first to sixth auxiliary functional layers are omitted.

[0200] Example 7

[0201] This embodiment provides a photoelectric device and a method for preparing the same. Compared with the photoelectric device in Embodiment 1, the difference of the photoelectric device in this embodiment is that the first to sixth auxiliary functional layers are omitted, and the materials of the first to third nucleophilic functional layers are respectively replaced with 7-aminocoumarin.

[0202] Compared with the preparation method of the photoelectric device in Example 1, the difference of the preparation method of the photoelectric device in this embodiment is that: the preparation steps of the first auxiliary functional layer to the sixth auxiliary functional layer are omitted, and the "LiAlH4-ethanol solution" in step S1.7, step S1.11 and step S1.15 are replaced with "7-aminocoumarin-ethanol solution" respectively, and step S1.18 is omitted.

[0203] Example 8

[0204] This embodiment provides a photoelectric device and a method for preparing the same. Figure 5 As shown, compared with the optoelectronic device in Example 1, the difference of the optoelectronic device in this embodiment is that the electronic functional layer 14 includes a first electron transport layer 141-1, a nucleophilic functional layer 142 and a second electron transport layer 141-2 which are stacked in sequence. Among them, the materials of the first electron transport layer 141-1 and the second electron transport layer 141-2 are nano ZnO (average particle size is 5nm), and the thickness of the first electron transport layer 141-1 and the second electron transport layer 141-2 are 30nm respectively. The material of the nucleophilic functional layer 142 is LiAlH4, and the thickness of the nucleophilic functional layer 142 is 21nm.

[0205] The method for preparing the optoelectronic device in this embodiment comprises the following steps:

[0206] S8.1, refer to step S1.1;

[0207] S8.2, refer to step S1.2;

[0208] S8.3, refer to step S1.3;

[0209] S8.4, refer to step S1.4;

[0210] S8.5, refer to step S1.5;

[0211] S8.6. In a nitrogen environment at room temperature and pressure, a 6 mg / mL LiAlH4-ethanol solution was spin-coated on the side of the first electron transport layer away from the light-emitting layer, and then the ambient pressure was adjusted to 35 KPa, and the mixture was allowed to stand for 2 min, and then placed at 10 -2 The vacuum drying treatment is carried out under MPa environment to solidify the film and obtain the nucleophilic functional layer;

[0212] S8.7, in a nitrogen environment at room temperature and pressure, spin-coat a 30 mg / mL nano ZnO-ethanol solution on the side of the nucleophilic functional layer away from the first electron transport layer, then adjust the ambient pressure to 35 KPa, let it stand for 2 minutes, and then place it at 10 -2 Perform vacuum drying treatment under MPa environment to solidify into a film, thereby obtaining a second electron transport layer;

[0213] S8.8, vacuum degree not higher than 3×10 -4 In the Pa evaporation chamber, Ag is evaporated on the side of the second electron transport layer away from the nucleophilic functional layer to obtain a cathode, which is then encapsulated with epoxy resin to obtain a photoelectric device.

[0214] Example 9

[0215] This embodiment provides a photoelectric device and a method for preparing the same. Figure 6As shown, compared with the optoelectronic device in Example 1, the difference of the optoelectronic device in this embodiment is that: the electronic functional layer 14 includes a first electron transport layer 141-1, a first auxiliary functional layer 143-1, a first nucleophilic functional layer 142-1, a second auxiliary functional layer 143-2, a second nucleophilic functional layer 142-2, a third auxiliary functional layer 143-3, a third nucleophilic functional layer 142-3, a fourth auxiliary functional layer 143-4 and a second electron transport layer 141-2, wherein the materials of the first electron transport layer 141-1 and the second electron transport layer 141-2 are respectively nano ZnO (average particle size is 5nm), and the thickness of the first electron transport layer 141-1 and the second electron transport layer 141-2 is 30nm respectively. The materials and thicknesses of the first nucleophilic functional layer 142-1 to the third nucleophilic functional layer 142-3 are consistent with those in Example 1. The materials of the first to fourth auxiliary functional layers 143 - 1 to 143 - 4 respectively include cross-linked compounds formed by self-cross-linking reaction of 7-aminocoumarin, and the thicknesses of the first to fourth auxiliary functional layers 143 - 1 to 143 - 4 are respectively 7 nm.

[0216] The method for preparing the optoelectronic device in this embodiment comprises the following steps:

[0217] S9.1, refer to step S1.1;

[0218] S9.2, refer to step S1.2;

[0219] S9.3, refer to step S1.3;

[0220] S9.4, refer to step S1.4;

[0221] S9.5, refer to step S1.5;

[0222] S9.6, refer to step S1.6;

[0223] S9.7, refer to step S1.7;

[0224] S9.8, refer to step S1.8;

[0225] S9.9. In a nitrogen environment at room temperature and pressure, a 6 mg / mL LiAlH4-ethanol solution was spin-coated on the side of the second auxiliary functional layer away from the first nucleophilic functional layer, and then the ambient pressure was adjusted to 35 KPa, and the mixture was allowed to stand for 2 minutes, and then placed at 10 -2 MPa environment, vacuum drying treatment is performed to solidify the film to obtain a second nucleophilic functional layer;

[0226] S9.10. In a nitrogen environment at room temperature and pressure, a 3 mg / mL 7-aminocoumarin-ethanol solution was spin-coated on the side of the third nucleophilic functional layer away from the second auxiliary functional layer, and then the ambient pressure was adjusted to 35 KPa, and the mixture was allowed to stand for 2 minutes, and then placed at 10 -2 Perform vacuum drying treatment under MPa environment to solidify into a film, thereby obtaining a third auxiliary functional layer;

[0227] S9.11. In a nitrogen environment at room temperature and pressure, a 6 mg / mL LiAlH4-ethanol solution was spin-coated on the side of the third auxiliary functional layer away from the second nucleophilic functional layer, and then the ambient pressure was adjusted to 35 KPa, and the mixture was allowed to stand for 2 minutes, and then placed at 10 -2 MPa environment, vacuum drying treatment is performed to solidify the film to obtain a third nucleophilic functional layer;

[0228] S9.12. In a nitrogen environment at room temperature and pressure, a 3 mg / mL 7-aminocoumarin-ethanol solution was spin-coated on the side of the third nucleophilic functional layer away from the third auxiliary functional layer, and then the ambient pressure was adjusted to 35 KPa, and the mixture was allowed to stand for 2 minutes, and then placed at 10 -2 MPa environment, vacuum drying treatment is performed to solidify the film to obtain a fourth auxiliary functional layer;

[0229] S9.13, in a nitrogen environment at room temperature and pressure, spin-coat a 30 mg / mL nano ZnO-ethanol solution on the side of the fourth auxiliary functional layer away from the third nucleophilic functional layer, then adjust the ambient pressure to 35 KPa, let it stand for 2 minutes, and then place it at 10 -2 Perform vacuum drying treatment under MPa environment to solidify into a film, thereby obtaining a second electron transport layer;

[0230] S9.14, subjecting the prefabricated device after S9.13 to ultraviolet light treatment, so as to cause at least part of the 7-aminocoumarin in the first auxiliary functional layer to the fourth auxiliary functional layer to undergo self-crosslinking reaction to form a crosslinked compound, wherein the process parameters of the ultraviolet light treatment are: the wavelength of the light is 365 nm, the pulse width of the ultraviolet laser is 22 ns, the power is 5 W, the frequency is 1.2 Hz, and the time is 90 s;

[0231] S9.15, vacuum degree not higher than 3×10 -4 In the evaporation chamber of Pa, Ag is evaporated on the side of the second electron transport layer away from the fourth auxiliary functional layer to obtain a cathode, which is then encapsulated with epoxy resin to obtain a photoelectric device.

[0232] Comparative Example 1

[0233] This comparative example provides a photoelectric device and a preparation method thereof. Compared with the photoelectric device in Example 1, the difference between the photoelectric device in this comparative example is that: Figure 7 As shown, the electronic functional layer 14 is a single-layer structure, the material of the electronic functional layer 14 is nano ZnO (with an average particle size of 5 nm), and the thickness of the electronic functional layer 14 is 60 nm.

[0234] Compared with the preparation method of the optoelectronic device in Example 1, the difference of the preparation method of the optoelectronic device in this comparative example is that step S1.5 is replaced by "under a nitrogen environment at room temperature and pressure, spin-coating a 30 mg / mL nano ZnO-ethanol solution on the side of the light-emitting layer away from the hole transport layer, and then placing it at 10 -2 MPa environment to perform vacuum drying treatment to solidify into a film to obtain an electronic functional layer", and steps S1.6 to S1.18 are omitted.

[0235] Comparative Example 2

[0236] This comparative example provides a photoelectric device and a preparation method thereof. Compared with the photoelectric device in Example 1, the difference between the photoelectric device in this comparative example is that: Figure 8 As shown, the electronic functional layer 14 is composed of a stacked electron transport layer 141 and a nucleophilic functional layer 142, and the nucleophilic functional layer 142 is closer to the cathode 12 than the electronic functional layer 14. The material of the electron transport layer 141 is nano ZnO (average particle size is 5nm), and the thickness of the electron transport layer 141 is 60nm; the material of the nucleophilic functional layer 142 is LiAlH4, and the thickness of the nucleophilic functional layer 142 is 21nm.

[0237] Compared with the preparation method of the optoelectronic device in Example 1, the difference of the preparation method of the optoelectronic device in this comparative example is that step S1.5 is replaced by "under a nitrogen environment at room temperature and pressure, spin-coating a 30 mg / mL nano ZnO-ethanol solution on the side of the light-emitting layer away from the hole transport layer, and then placing it at 10 -2 MPa environment, vacuum drying treatment to solidify the film to obtain an electron transport layer", and replace step S1.6 with "under a nitrogen environment at room temperature and pressure, spin-coat a 6 mg / mL LiAlH4-ethanol solution on the side of the electron transport layer away from the light-emitting layer, and then place it at 10 -2 MPa environment to perform vacuum drying to solidify the film and obtain a nucleophilic functional layer", and omit steps S1.7 to S1.18.

[0238] Experimental Example 1

[0239] A stress tester (Puyun PY-H608 MIT) was used to test the mechanical stress of the electronic functional layer in the optoelectronic devices of Examples 1 to 9, Comparative Example 1 and Comparative Example 2. During the preparation of the optoelectronic devices in Examples 1 to 9, Comparative Example 1 and Comparative Example 2, the mechanical stress test was performed after the preparation of the electronic functional layer. The test results are shown in Table 1 below:

[0240] Table 1 Summary of mechanical stress of electronic functional layers in optoelectronic devices of Examples 1 to 9, Comparative Examples 1 and 2

[0241]

[0242]

[0243] It can be seen from Table 1 that compared with the mechanical stress of the electronic functional layer in the optoelectronic devices of Comparative Examples 1 and 2, the mechanical stress of the electronic functional layer in the optoelectronic devices of Examples 1 to 9 is better, especially the mechanical stress of the electronic functional layer in the optoelectronic devices of Examples 1 to 4 and 9 is significantly better than the mechanical stress of the electronic functional layer in the optoelectronic devices of Comparative Examples 1 and 2. The reason may be that: except for Example 5, the adjacent film layers are dissolved in each other during the preparation of the electronic functional layers in other embodiments, which can improve the overall mechanical stress of the electronic functional layer; the electronic functional layer in the optoelectronic devices of Examples 1 to 4 and 9 also includes an auxiliary functional layer with an adhesion effect, which further improves the overall mechanical stress of the electronic functional layer; in addition, since the electronic functional layer of the optoelectronic device in Example 5 includes an auxiliary functional layer with an adhesion effect, the mechanical stress of the electronic functional layer of the optoelectronic device in Example 5 is better than the mechanical stress of the electronic functional layer of the optoelectronic device in Comparative Examples 1 and 2.

[0244] Experimental Example 2

[0245] The performance of the encapsulated optoelectronic devices in Examples 1 to 9, Comparative Examples 1 and 2 was tested, and the FPD optical property measurement equipment (including Ocean Optics USB2000, LabView controlled QE-PRO spectrometer, Keithley 2400, high-precision digital source meter Keithley 6485, an optical fiber with an inner diameter of 50 μm, a device test probe and a fixture, various related connecting wires and data cards, an efficiency test cassette and a data acquisition system and other components to build an efficiency test system) was used to detect and obtain the parameters such as the start-up voltage, current, brightness, and luminescence spectrum of each optoelectronic device, and then the key parameters such as the external quantum efficiency and power efficiency were calculated, and the service life of each of the above-mentioned optoelectronic devices was tested using a life test equipment.

[0246] The current efficiency test method is: set the luminous area to 2mm×2mm=4mm 2 , intermittently collect the brightness value of the photoelectric device in the range of 0V to 6V. The initial voltage value of the brightness is 3V, and the brightness is collected every 0.2V. The brightness value collected each time is divided by the corresponding current density to obtain the current efficiency of the photoelectric device under the collection conditions, and the maximum current efficiency (CE max ,cd / A).

[0247] The test method for service life is as follows: under the drive of constant current (2mA), a 128-channel QLED life test system is used to perform electroluminescent life analysis on each optoelectronic device, and the time required for each optoelectronic device to decay from the maximum brightness to 95% (T95, h) is recorded. The time required for the brightness of each optoelectronic device to decay from 100% to 95% at a brightness of 1000nit is calculated through the attenuation fitting formula (T95@1000nit, h).

[0248] The performance test data of each optoelectronic device at 25°C is shown in Table 2 below:

[0249] Table 2 Performance test data of the optoelectronic devices in Examples 1 to 9, Comparative Examples 1 and 2 at 25°C

[0250]

[0251] As shown in Table 1, compared with the comprehensive performance of the optoelectronic devices in Comparative Examples 1 and 2, the comprehensive performance of the optoelectronic devices in Examples 1 to 9 is more advantageous, specifically, the optoelectronic performance of the optoelectronic devices in Examples 1 to 9 is better, and the device life of the optoelectronic devices in Examples 1 to 9 is longer. Taking the optoelectronic devices in Example 1 and Comparative Example 1 as an example, the L max is the L of the optoelectronic device in Comparative Example 1 max The T95 of the optoelectronic device in Example 1 is 1.2 times that of the T95 of the optoelectronic device in Comparative Example 1, the T95@1000nit of the optoelectronic device in Example 1 is 1.1 times that of the T95 of the optoelectronic device in Comparative Example 1, the T95@1000nit of the optoelectronic device in Example 1 is 1.5 times that of the T95@1000nit of the optoelectronic device in Comparative Example 1, and the CE of the optoelectronic device in Example 1 is 1.5 times that of the T95@1000nit of the optoelectronic device in Comparative Example 1. max is the CE of the optoelectronic device in Comparative Example 1 max 1.2 times of that.

[0252] It can be seen from the performance test data of the optoelectronic devices in Examples 1 to 9 and Comparative Example 1 that the introduction of a nucleophilic functional layer into the electronic functional layer can effectively improve the optoelectronic performance and device life of the optoelectronic device. The reason is that the nucleophilic functional layer attracts holes, thereby improving the hole injection level, effectively improving the problem of the electron injection level of QLED being much greater than the hole injection level, promoting the electron-hole transfer balance, and is beneficial to improving the comprehensive performance of the optoelectronic device.

[0253] It can be seen from the performance test data of the optoelectronic devices in Examples 1 to 9 and Comparative Example 2 that, compared with setting a nucleophilic functional layer between the electron transport layer and the cathode, configuring the electron transport layer as a multi-layer structure with intervals and setting the nucleophilic functional layer between two adjacent electron transport layers can further improve the comprehensive performance of the optoelectronic device. The reason is that: it will not adversely affect the interface state between the electron transport layer and the cathode, and can effectively improve the hole injection level of the optoelectronic device without affecting the electron injection level and reducing the risk of quantum dot quenching.

[0254] The above is a detailed introduction to an optoelectronic device, a method for preparing an optoelectronic device, and an electronic device provided in the embodiments of the present application. Specific examples are used herein to illustrate the principles and implementation methods of the present application. The description of the above embodiments is only used to help understand the technical solutions and core ideas of the present application; ordinary technicians in this field should understand that they can still modify the technical solutions recorded in the aforementioned embodiments, or replace some of the technical features therein by equivalents; and these modifications or replacements do not make the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present application.

Claims

1. A photoelectric device, characterized in that: The optoelectronic device comprises: an anode and a cathode disposed opposite to each other; and An electronic functional layer, disposed between the cathode and the anode; Among them, the electronic functional layer includes N electron transport layers spaced between the anode and the cathode, and N is a positive integer greater than or equal to 2; the electronic functional layer also includes a nucleophilic functional layer, which is arranged between two adjacent electron transport layers, and the material of the nucleophilic functional layer includes a nucleophilic compound.

2. The optoelectronic device according to claim 1, characterized in that: At least one nucleophilic functional layer is disposed between any two adjacent electron transport layers; and / or The nucleophilic compound is selected from one or more of NaNH2, Grignard reagent, Gilman reagent, organic lithium reagent, NaBH4, LiAlH4, amino-substituted coumarin, a first compound and a second compound, wherein the first compound has a structure shown in the following general formula (I): The second compound has a structure shown in the following general formula (II): wherein R1 to R6 are independently selected from aliphatic hydrocarbon groups or aromatic hydrocarbon groups; and / or The material of the electron transport layer includes a first metal oxide, which is selected from one or more of zinc oxide, titanium oxide, tin oxide, barium oxide, tantalum oxide, aluminum oxide, zirconium oxide, magnesium zinc oxide, calcium zinc oxide, zirconium oxide, gallium zinc oxide, aluminum zinc oxide, lithium zinc oxide, titanium zinc oxide, yttrium zinc oxide, indium tin oxide and lithium titanium oxide.

3. The optoelectronic device according to claim 2, characterized in that: The carbon number of the aliphatic hydrocarbon group is 1 to 10, and optionally, the aliphatic hydrocarbon group is selected from pentyl, hexyl, heptyl or octyl; the carbon number of the aromatic hydrocarbon group is 6 to 20, and optionally, the aromatic hydrocarbon group is selected from phenyl, naphthyl or biphenyl; and / or When there are at least two nucleophilic functional layers, the nucleophilic compounds in each nucleophilic functional layer are independently selected from one or more of NaNH2, Grignard reagent, Gilman reagent, organic lithium reagent, NaBH4, LiAlH4, amino-substituted coumarin, the first compound and the second compound.

4. The optoelectronic device according to claim 1, characterized in that: The total thickness of the electronic functional layer is 40nm to 200nm; and / or The thickness of each electron transport layer is 7nm to 15nm; and / or The total thickness of the N electron transport layers is 30 nm to 80 nm; and / or When there are at least two nucleophilic functional layers, the total thickness of the nucleophilic functional layers is 7 nm to 40 nm, and / or the thickness of each nucleophilic functional layer is 7 nm to 15 nm.

5. The optoelectronic device according to claim 1, characterized in that: The electronic functional layer further comprises at least one auxiliary functional layer, wherein the auxiliary functional layer is disposed between the adjacent electron transport layer and the nucleophilic functional layer, and / or the auxiliary functional layer is disposed between two adjacent nucleophilic functional layers; the material of the auxiliary functional layer comprises a cross-linking compound, wherein the cross-linking compound is a compound formed by a self-cross-linking reaction of a third compound; Wherein, the third compound has a structure shown by the following general formula (III): In the general formula (III), each occurrence of R7 is independently selected from hydrogen atom, -NH2, carboxyl group, hydrocarbon group or -X, X is halogen, and y is a positive integer of 1 to 4.

6. The optoelectronic device according to claim 5, characterized in that: The thickness of the auxiliary functional layer is 7nm to 15nm; and / or The hydrocarbon group has 1 to 10 carbon atoms, and optionally, the hydrocarbon group is selected from methyl, ethyl or propyl; and / or The material of the nucleophilic functional layer does not contain coumarin and / or coumarin derivatives.

7. The optoelectronic device according to claim 1, characterized in that: The optoelectronic device further comprises a light-emitting layer, which is disposed between the anode and the electronic functional layer; the material of the light-emitting layer comprises one or more of an organic light-emitting material and a quantum dot; Wherein, the organic light-emitting material is selected from one or more of 4,4'-bis(N-carbazole)-1,1'-biphenyl:tri[2-(p-tolyl)pyridine iridium(III), 4,4',4"-tri(carbazole-9-yl)triphenylamine:tri[2-(p-tolyl)pyridine iridium, diaromatic anthracene derivatives, distilbene aromatic derivatives, pyrene derivatives, fluorene derivatives, TBPe fluorescent materials, TTPX fluorescent materials, TBRb fluorescent materials, DBP fluorescent materials, delayed fluorescent materials, TTA materials, thermally activated delayed materials, polymers containing BN covalent bonds, hybrid localized charge transfer excited state materials and exciplex light-emitting materials; the quantum dots are selected from one or more of single component quantum dots, core-shell structure quantum dots, inorganic perovskite quantum dots, organic perovskite quantum dots and organic-inorganic hybrid perovskite quantum dots; and / or The material of the single-component quantum dot, the material of the core of the core-shell structure quantum dot, and the material of the shell of the core-shell structure quantum dot are independently selected from at least one of a II-VI group compound, a III-V group compound, a IV-VI group compound, or a I-III-VI group compound, wherein the II-VI group compound is selected from CdS, CdSe, CdTe, ZnS, ZnSe, ZnTe, ZnO, HgS, HgSe, HgTe, CdSeS, CdSeTe, CdSTe, ZnSeS, ZnSeTe, ZnSTe, HgSeS, HgSeT e, HgSTe, CdZnS, CdZnSe, CdZnTe, CdHgS, CdHgSe, CdHgTe, HgZnS, HgZnSe, HgZnTe, CdZnSeS, CdZnSeTe, CdZnSTe, CdHgSeS, CdHgSeTe, CdHgSTe, HgZnSeS, HgZnSeTe and HgZnSTe, and the III-V group compound is selected from GaN, GaP, GaAs, GaSb, AlN, AlP, AlAs, AlSb, InN, InP, InA s, InSb, GaNP, GaNAs, GaNSb, GaPAs, GaPSb, AlNP, AlNAs, AlNSb, AlPAs, AlPSb, InNP, InNAs, InNSb, InPAs, InPSb, GaAlNP, GaAl NAs, GaAlNSb, GaAlPAs, GaAlPSb, GaInNP, GaInNAs, GaInNSb, GaInPAs, GaInPSb, InAlNP, InAlNAs, InAlNSb, InAlPAs and InAlPS b, the IV-VI group compound is selected from one or more of SnS, SnSe, SnTe, PbS, PbSe, PbTe, SnSeS, SnSeTe, SnSTe, PbSeS, PbSeTe, PbSTe, SnPbS, SnPbSe, SnPbTe, SnPbSSe, SnPbSeTe and SnPbSTe, the I-III-VI group compound is selected from one or more of CuInS, CuInSe and AgInS; the general structural formula of the inorganic perovskite quantum dot is AMX3, wherein A is Cs + ion, M is a divalent metal cation, M is selected from Pb 2+ Sn 2+ , Cu 2+ 、Ni 2+ 、Cd 2+ Cr 2 + , Mn 2+ 、Co 2+ , Fe 2+ ,Ge 2+ , Yb 2+ and Eu 2+ One or more of, X is a halogen anion; the general structural formula of the organic perovskite quantum dot is CMX3, C is a carboxamidine group; the general structural formula of the organic-inorganic hybrid perovskite quantum dot is BMX3, B is selected from an organic amine cation; and / or The materials of the anode and the cathode are independently selected from one or more of a metal, a carbon material and a second metal oxide, the metal is selected from one or more of Al, Ag, Cu, Mo, Au, Ba, Pt, Ca, Ir, Ni and Mg, the carbon material is selected from one or more of graphite, carbon nanotubes, graphene and carbon fibers, and the third metal oxide is selected from one or more of indium-doped tin oxide, fluorine-doped tin oxide, antimony-doped tin oxide, aluminum-doped zinc oxide, gallium-doped zinc oxide, indium-doped zinc oxide, magnesium-doped zinc oxide, aluminum-doped magnesium oxide, SnO2, ZnO and In2O3; and / or The photoelectric device also includes a hole functional layer arranged between the anode and the electronic functional layer, and the material of the hole functional layer includes poly (3,4-ethylenedioxythiophene): poly (styrene sulfonic acid), copper phthalocyanine, titanium phthalocyanine, 2,3,5,6-tetrafluoro-7,7',8,8'-tetracyanodimethyl-p-benzoquinone, 2,3,6,7,10,11-hexycyano-1,4,5,8,9,12-hexaazatriphenylene, 3-hexyl substituted polythiophene, poly (9-vinyl carbazole), 4,4'-bis (9-carbazole) biphenyl, poly [bis (4-phenyl) (4-butylphenyl) amine], 4, 4'-cyclohexylbis[N,N-di(4-methylphenyl)aniline], poly[(9,9-dioctylfluorenyl-2,7-diyl)-co-(4,4'-(N-(4-sec-butylphenyl)diphenylamine)], poly[(9,9-dioctylfluorenyl-2,7-diyl)-co-(4,4'-(N-(p-butylphenyl))diphenylamine)], poly(N,N'-di(4-butylphenyl)-N,N'-diphenyl-1,4-phenylenediamine-co-9,9-dioctylfluorene), 4,4',4'-tri(N-3-methylphenyl-N-phenylamino)triphenylamine, 4,4',4"-tri (Carbazole-9-yl) triphenylamine, 4,4',4'-tri(2-naphthylphenylamino) triphenylamine, N,N'-diphenyl-N,N'-(1-naphthyl)-1,1'-biphenyl-4,4'-diamine, N,N'-diphenyl-N,N'-di(3-methylphenyl)-1,1'-biphenyl-4,4'-diamine, N,N'-bis[4-(diphenylamino)phenyl]-N,N'-diphenylbenzidine, N,N'-bis(3-methylphenyl)-N,N'-diphenyl-9,9-spirobifluorene-2,7-diamine, N2,N7-di-1-naphthyl-N2,N7-diphenyl One or more of 9,9'-spirobi[9H-fluorene]-2,7-diamine, poly[bis(4-phenyl)(2,4,6-trimethylphenyl)amine], 2,2',7,7'-tetrakis[N,N-di(4-methoxyphenyl)amino]-9,9'-spirobifluorene, doped or undoped graphene, C60, doped or undoped nickel oxide, doped or undoped molybdenum oxide, doped or undoped tungsten oxide, doped or undoped vanadium oxide, doped or undoped P-type gallium nitride, doped or undoped chromium oxide, doped or undoped copper oxide, transition metal sulfide and transition metal selenide.

8. A method for preparing a photoelectric device, characterized in that: The steps include: providing a bottom electrode, and forming an electronic functional layer on one side of the bottom electrode; and forming a top electrode on a side of the electronic functional layer away from the bottom electrode; Among them, one of the bottom electrode and the top electrode is an anode, and the other is a cathode; the electronic functional layer includes N electron transport layers spaced between the anode and the cathode, and N is a positive integer greater than or equal to 2; the electronic functional layer also includes a nucleophilic functional layer, which is arranged between two adjacent electron transport layers, and the material of the nucleophilic functional layer includes a nucleophilic compound.

9. The preparation method according to claim 8, characterized in that: At least one nucleophilic functional layer is formed between any two adjacent electron transport layers; and / or The nucleophilic compound is selected from one or more of NaNH2, Grignard reagent, Gilman reagent, organic lithium reagent, NaBH4, LiAlH4, amino-substituted coumarin, a first compound and a second compound, wherein the first compound has a structure shown in the following general formula (I): The second compound has a structure shown in the following general formula (II): wherein R1 to R6 are independently selected from aliphatic hydrocarbon groups or aromatic hydrocarbon groups; and / or The method for forming the electron transport layer comprises the steps of: depositing a first solution comprising a first metal oxide; and performing a first drying process on the deposited first solution to obtain the electron transport layer; Wherein, the first metal oxide is selected from one or more of zinc oxide, titanium oxide, tin oxide, barium oxide, tantalum oxide, aluminum oxide, zirconium oxide, magnesium zinc oxide, calcium zinc oxide, zirconium zinc oxide, gallium zinc oxide, aluminum zinc oxide, lithium zinc oxide, titanium zinc oxide, yttrium zinc oxide, indium tin oxide and lithium titanium oxide; and / or The method for forming the nucleophilic functional layer comprises the steps of: depositing a second solution comprising a nucleophilic compound; and The deposited second solution is subjected to a second drying process to obtain the nucleophilic functional layer.

10. The preparation method according to claim 9, characterized in that: Before the step of performing a first drying treatment on the deposited first solution, the method for forming an electron transport layer further comprises the steps of: placing the deposited first solution in an inert gas atmosphere and allowing it to stand; and / or Before the step of performing a second drying treatment on the deposited second solution, the method for forming a nucleophilic functional layer further comprises the step of placing the deposited second solution in an inert gas atmosphere and allowing it to stand.

11. The preparation method according to any one of claims 8 to 10, characterized in that: The electronic functional layer further comprises at least one auxiliary functional layer, wherein the auxiliary functional layer is formed between the adjacent electron transport layer and the nucleophilic functional layer, and / or the auxiliary functional layer is formed between two adjacent nucleophilic functional layers; The method for forming the auxiliary functional layer comprises the steps of: depositing a third solution comprising a third compound; Performing a third drying process on the deposited third solution to obtain a solidified film layer whose material is the third compound; as well as Performing light treatment on the cured film layer to cause at least a portion of the third compound to undergo a self-crosslinking reaction to form a crosslinked compound, thereby obtaining the auxiliary functional layer; Wherein, the third compound has a structure shown by the following general formula (III): In the general formula (III), each occurrence of R7 is independently selected from hydrogen atom, -NH2, carboxyl group, hydrocarbon group or -X, X is halogen, and y is a positive integer of 1 to 4.

12. The preparation method according to claim 11, characterized in that: Before the step of performing a third drying process on the deposited third solution, the method for forming the auxiliary functional layer further comprises the step of placing the deposited third solution in an inert gas atmosphere and allowing it to stand.

13. An electronic device, characterized in that: The electronic device comprises the optoelectronic device as claimed in any one of claims 1 to 7, or the electronic device comprises the optoelectronic device manufactured by the manufacturing method as claimed in any one of claims 8 to 12.