Method for preparing CsPbBr3 perovskite thin film battery through cesium bromide pre-doping and battery thereof
Pre-doping method of cesium bromide predoping method to prepare a mesoporous CsPbBr3 film in inorganic perovskite solar cells, which solves the charge recombination and defect problems, improves the grain size and purity of the film, and achieves efficient and stable perovskite Solar cells improve photovoltaic efficiency and environmental stability.
Patent Information
- Application Number
- CN202410959122.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-11-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Due to the limited absorption range and serious charge recombination problems, existing inorganic perovskite solar cells have low efficiency and shortened service life, especially the charge recombination and defect problems caused by grain boundaries in CsPbBr3 perovskite films are difficult to solve.
When preparing CsPbBr3 perovskite films, a mesoporous Cs-Pb-Br film was formed by dropping the cesium bromide/methanol solution during the spin coating of lead bromide, and the Cs-Pb-Br film was used. Low boiling point methanol accelerates solvent vaporization, promotes the full reaction between CsBr and PbBr2, reduces the formation of CsPb2Br5 heterophase, and improves the purity and grain size of CsPbBr3 phase.
Through the predoping method of cesium bromide, the charge recombination and defect density are significantly reduced, the grain size and charge extraction efficiency are improved, and the efficient and stable preparation of CsPbBr3 perovskite thin film batteries is achieved, which improves photovoltaic efficiency and environmental stability. .
Smart Images

Figure CN118922036A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of solar cells, and in particular relates to a method for preparing a CsPbBr3 perovskite thin film cell by pre-doping cesium bromide and a cell thereof. Background Art
[0002] In the past decade, organic-inorganic hybrid perovskite solar cells (PSCs) have made significant breakthroughs, with their efficiency increasing from 3.8% in 2009 to 26.1% at present. However, this type of solar cell is composed of MA + or FA + The instability leads to the degradation of battery performance and shortened service life, which seriously hinders the commercialization of perovskite solar cells. Therefore, people are interested in using highly stable inorganic cations (such as Cs + ) instead of volatile organic cations (MA + and FA + ) all-inorganic PSCs are gaining more and more attention. Among various inorganic PSCs, CsPbBr3PSC has a high open circuit voltage (V OC ), excellent wet and thermal stability and shows great potential for photovoltaic applications.
[0003] The limited absorption range and severe charge recombination pose a major challenge to improving the PCE of CsPbBr3. Most of the charge recombination occurs at the grain boundaries of the perovskite film, because the grain boundaries lead to shallow states near the edge of the perovskite valence band (VB), which restricts the diffusion of holes and provides sites for many non-coordinated ion defects. Therefore, how to fabricate high-quality perovskite films with large grain size and low grain boundaries is the key to reducing charge recombination to improve the photovoltaic performance of the device. Summary of the invention
[0004] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a method for preparing CsPbBr3 perovskite thin film battery by pre-doping cesium bromide and a battery thereof, which solves the problems in the above-mentioned background technology.
[0005] The technical solution adopted by the present invention to solve the technical problem is: a method for preparing CsPbBr3 perovskite thin film battery by cesium bromide pre-doping is provided, comprising the following steps:
[0006] 1) Pretreatment of conductive transparent substrate;
[0007] 2) Preparation of electron transport layer: Spin coating SnO2 thin film on the surface of conductive transparent substrate to form electron transport layer;
[0008] 3) Pre-doping with cesium bromide: Spin-coating a PbBr2 solution on the surface of the electron transport layer, while dropping a CsBr methanol solution, and annealing in an ambient atmosphere to form a pre-doped film;
[0009] 4) Preparing a perovskite layer: spin coating a methanol solution of CsBr on the surface of the pre-doped film to form a perovskite layer;
[0010] 5) Preparing electrodes: forming electrodes on the surface of the perovskite layer.
[0011] In the present invention, 2) preparing the electron transport layer: diluting the SnO2 dispersant and deionized water in a volume ratio of 1:4, and then spin coating the diluted SnO2 dispersant on the substrate at a speed of 3500 rpm, and annealing at 150°C for 30 minutes after spin coating to obtain the electron transport layer.
[0012] In the present invention, 3) pre-doping cesium bromide: spin-coating the PbBr2 solution at a speed of 2000 rpm on the surface of the deposited electron transport layer for 30 seconds, and then annealing on a hot plate at 100°C for 30 minutes. During the spin-coating process of the PbBr2 solution, a methanol solution of CsBr is added dropwise to obtain a pre-doped film. The concentration of the PbBr2 is 1.0 M, the concentration of CsBr in the methanol solution of CsBr is 0.07 M, and the amount of the methanol solution of CsBr is 120 μL.
[0013] In the present invention, 4) preparing the perovskite layer: after cooling to room temperature, spin coating the CsBr methanol solution on the surface of the pre-doped film at a speed of 2000 rpm, with a loading time of 30 seconds, and then continuously heating at 250° C. for 5 minutes to obtain the perovskite layer. The concentration of CsBr in the CsBr methanol solution is 0.07 M. The number of spin coatings is 7 times.
[0014] In the present invention, 5) preparing electrodes: using a screen to print carbon paste on the surface of the perovskite layer to form a carbon electrode, thereby completing the production of the perovskite thin film battery.
[0015] In the present invention, the conductive transparent substrate in step 1) is an ITO conductive glass substrate, and the pretreatment includes cleaning and the like.
[0016] The present invention also provides a CsPbBr3 perovskite thin film battery, which is prepared by the above method and includes a conductive transparent substrate, an electron transport layer, a perovskite layer and a counter electrode arranged in sequence.
[0017] Compared with the background technology, this technical solution has the following advantages:
[0018] 1. The preparation method of the present invention uses pre-doped cesium bromide, that is, the cesium bromide / methanol solution of the first spin coating is introduced into the spin coating process of lead bromide, and the preparation is completed with the assistance of a low-boiling point methanol anti-solvent, thereby successfully obtaining a Cs-Pb-Br film with a mesoporous structure;
[0019] 2. The present invention selects low-boiling-point methanol as an anti-solvent, utilizes the solubility characteristics of CsBr, accelerates the vaporization of the solvent during the spin coating process, and prepares a Cs-Pb-Br film with a mesoporous structure, which is beneficial to the subsequent full reaction of CsBr and PbBr2, significantly reduces the CsPb2Br5 impurity phase generated by insufficient reaction, and improves the purity of the CsPbBr3 phase;
[0020] 3. The pre-doping of cesium bromide in the present invention increases the density of nucleation sites of the Cs-Pb-Br film, so that the CsPb2Br5 grain size generated by pre-crystallization is smaller and the nucleation sites are denser;
[0021] 4. The CsPbBr3 thin film battery prepared by spin coating of the present invention finally has a larger grain size and a lower defect density, achieves the suppression of charge recombination and the enhancement of charge extraction, and finally obtains a highly efficient and stable CsPbBr3 perovskite thin film battery through the above-mentioned synergistic effect. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 Flow chart of the preparation of CsPbBr3 perovskite thin films of the embodiment (top) and the comparative example (bottom);
[0023] Figure 2 The top view SEM images and the statistical distribution diagram of the grain size of Examples 1 to 4 and the comparative example;
[0024] Figure 3 UV-Vis absorption spectra of the devices of Example 3 and Comparative Example;
[0025] Figure 4 PL spectra of the devices of Example 3 and Comparative Example;
[0026] Figure 5 JV curves of the devices of Examples 1 to 4 and the comparative example;
[0027] Figure 6 3 are the steady-state power output curves of Example 3 and the comparative example;
[0028] Figure 7 3 are TPC curves of the devices of Example 3 and the comparative example;
[0029] Figure 8 3 are TPV curves of the devices of Example 3 and the comparative example;
[0030] Fig. 9 3 are Tafel curves of the devices of Example 3 and Comparative Example;
[0031] Fig.10 The dependence of the current on the light intensity of the devices of Example 3 and the comparative example;
[0032] Fig.11 The dependence of the voltage on the light intensity of the devices of Example 3 and the comparative example;
[0033] Fig.12 SCLC curves of the devices of Example 3 and Comparative Example;
[0034] Fig.13 3 are EIS curves of the devices of Example 3 and Comparative Example;
[0035] Fig.14 3 are the MS curves of the devices of Example 3 and the comparative example;
[0036] Fig.15 tDOS curves of the devices of Example 3 and Comparative Example;
[0037] Fig.16 This is a 30-day stability test of the devices of Example 3 and the comparative example in an atmospheric environment. DETAILED DESCRIPTION
[0038] Example 1
[0039] The present embodiment provides a method for preparing a CsPbBr3 perovskite thin film battery by pre-doping cesium bromide, comprising the following steps:
[0040] S1. Cleaning of ITO conductive glass substrate: The etched ITO conductive glass substrate was ultrasonically cleaned in a beaker with detergent, deionized water, acetone and ethanol in sequence for 20 minutes, then treated with O3 / ultraviolet light for 15 minutes, and plasma cleaned for 6 minutes.
[0041] Preparation of S2, SnO2 electron transport layer (ETL): dilute the tin dioxide dispersant and deionized water in a ratio of 1:4, and then spin-coat 100 μL of the diluted tin dioxide dispersant on the substrate at a speed of 3500 rpm. After spin coating, anneal on a hot plate at 150°C for 30 minutes to obtain an electron transport layer.
[0042] S3, preparation of CsBr pre-doped film: prepare 1M PbBr2 DMF solution and 0.07M CsBr methanol solution, filter with nylon-66 filter plug in advance. Spin-coat the PbBr2 (1.0M) solution on the deposited ETL surface at 2000rpm, load for 30s, then anneal on a hot plate at 100℃ for 30min. During the spin coating of lead bromide, drop 120μL cesium bromide / methanol solution for 5s to obtain CsBr pre-doped film.
[0043] S4. The preparation method of the perovskite layer is as follows: after cooling to room temperature, spin-coating a CsBr methanol solution (0.07 M) on the CsBr pre-doped film at a speed of 2000 rpm for 30 s, and then continuously heating at 250°C for 5 min, repeating 7 times to obtain a perovskite layer.
[0044] S5. Preparation of the counter electrode: Using a screen to print the carbon paste on the formed CsPbBr3 film to complete the production of PSCs. Figure 1 The efficient and stable CsPbBr3 perovskite thin film battery prepared in this embodiment includes an ITO conductive glass substrate, a conductive transparent substrate, an electron transport layer, a perovskite layer and a counter electrode stacked in sequence.
[0045] Example 2
[0046] The difference between Example 2 and Example 1 is that:
[0047] S3, Preparation of CsBr pre-doped film: Prepare 1M PbBr2 DMF solution and 0.07M CsBr methanol solution, and filter with nylon-66 filter plug in advance. Spin-coat the PbBr2 (1.0M) solution on the deposited ETL surface at 2000rpm, load for 30s, and then anneal on a hot plate at 100℃ for 30min. During the spin coating of lead bromide, drop 120μL cesium bromide / methanol solution for 10s to obtain CsBr pre-doped film.
[0048] Example 3
[0049] The difference between Example 3 and Example 1 is that:
[0050] S3, Preparation of CsBr pre-doped film: Prepare 1M PbBr2 DMF solution and 0.07M CsBr methanol solution, and filter with nylon-66 filter plug in advance. Spin-coat the PbBr2 (1.0M) DMF solution on the deposited ETL surface at 2000rpm, load for 30s, and then anneal on a hot plate at 100℃ for 30min. During the spin coating of lead bromide, drop 120μL cesium bromide / methanol solution for 15s to obtain CsBr pre-doped film.
[0051] Example 4
[0052] The difference between Example 4 and Example 1 is that:
[0053] S3, preparation of CsBr pre-doped film: prepare 1M PbBr2 DMF solution and 0.07M CsBr methanol solution, filter with nylon-66 filter plug in advance. Spin-coat the PbBr2 (1.0M) solution on the deposited ETL surface at 2000rpm, load for 30s, then anneal on a hot plate at 100℃ for 30min. During the spin coating of lead bromide, drop 120μL cesium bromide / methanol solution for 20s to obtain CsBr pre-doped film.
[0054] Comparative Example
[0055] like Figure 1 The difference between the comparative example and Example 1 is that: step S3 is omitted, and the preparation of the CsBr pre-doped film is not performed. The perovskite layer is prepared directly in S4 after S2: after cooling to room temperature, a methanol solution of CsBr (0.07 M) is spin-coated on the surface of the PbBr2 film at a speed of 2000 rpm for 30 s, and then heated at 250°C for 5 min, which is repeated 8 times to obtain a perovskite layer.
[0056] The performance of the perovskite solar cell devices obtained in Examples 1 to 4 and the comparative example was tested.
[0057] refer to Figure 2 , multiple holes can be observed in the comparative CsPbBr3 film, indicating that there are obvious defects in the perovskite film. These defects can lead to a large amount of charge recombination, resulting in a decrease in device performance. In contrast, due to the comprehensive penetration of CsBr and the effective regulation of nucleation sites, the CsPbBr3 films of Examples 1-4 are smoother, and the roughness shows a larger grain size and surface smoothness. The cross-sectional SEM images also show that the target perovskite film has a larger grain size and grows in the form of a single layer vertical distribution.
[0058] refer to Figure 3 Compared with Example 3, the comparative example has a higher absorbance and the bandgap width remains basically unchanged, which is mainly due to the enhanced crystallinity and coverage of the perovskite film.
[0059] refer to Figure 4 In both CsPbBr3 films, an obvious PL emission peak appears, with the center position at about 530nm. The intensity of the CsPbBr3 perovskite film of Example 3 is significantly stronger than that of the comparative example CsPbBr3 perovskite film, indicating that the defect sites inside the perovskite are suppressed.
[0060] refer to Figure 5 The photocurrent-voltage (JV) curves of the CsPbBr3 PSCs of Examples 1 to 4 were measured under the condition of light intensity of AM 1.5G. It is worth noting that when the drop-adding interval is 15 seconds, the device efficiency is as high as 10.08%.
[0061] refer to Figure 6 , the efficiency of the device in Example 3 is 9.8%, J SC 7.54 mA cm –2 , and presents a stable output within 400 seconds. In addition, when a 1.3V bias voltage is applied to the comparative device, the maximum values of current density and PCE can be reached faster due to the improvement of charge extraction efficiency and the reduction of interfacial charge accumulation.
[0062] refer to Figure 7 , the charge extraction lifetime of the CsPbBr3 device of Example 3 is 53.25 μs, which is smaller than that of the comparative example (230.29 μs), indicating that the charge transfer process is improved.
[0063] refer to Figure 8 , compared with the comparative example, the device in Example 3 (2.609ms) achieves an extended charge recombination lifetime. This extended charge recombination lifetime indicates that the cesium bromide pre-doping method effectively alleviates charge recombination. It can be inferred that the improvement in photovoltaic efficiency is due to more efficient charge extraction and reduced carrier recombination.
[0064] refer to Fig. 9 , compared with the comparative example, the current leakage of the device in Example 3 is significantly reduced, which means that the charge carrier recombination is significantly weakened. Through the pre-doping of cesium bromide, the crystallinity and purity of the perovskite layer are improved, which plays an important role in improving the optoelectronic performance of the device.
[0065] refer to Fig.10 , the device in Example 3 shows a more favorable value (1.03) compared to the value of the comparative example (1.06). This indicates that the bimolecular recombination within the perovskite film is effectively suppressed, which is consistent with its higher FF and J SC The value remains consistent.
[0066] refer to Fig.11 In Example 3, the device exhibited a steep slope of 1.84 KT / q, while the comparative example exhibited a slope of 1.32 KT / q, indicating that the trap-assisted recombination in the device was reduced, thereby resulting in a reduction in the photovoltage loss of the device.
[0067] refer to Fig.12 , the trap state density was further determined. By calculating the trap filling limit voltage, the trap state density of Example 3 was obtained from 11.02×1015cm -3Reduced to 9.65×1015cm -3 , thereby improving the carrier transfer efficiency.
[0068] refer to Fig.13 , from the Nyquist plot of the device under dark conditions, it is obvious that the series resistance (Rs) of Example 3 is reduced to 12Ω, and the composite resistance (Rrec) is increased to 4876Ω, which indicates that the electron extraction efficiency is higher and the charge recombination is reduced, which helps to improve the FF and V OC .
[0069] refer to Fig.14 By Mott-Schottky (MS) analysis and using the Mott-Schottky equation to calculate the built-in potential, the CsPbBr3 PSC of Example 3 has a higher V than that of the comparative example. bi (1.24V), showing a stronger driving force on carrier separation and mobility, thereby improving the V OC .
[0070] refer to Fig.15 , the analysis shows that, compared with the comparative example, Example 3 has lower tDOS in the entire trap depth region, including the deeper trap region (0.40 to 0.55 eV) associated with film surface defects, and the shallower trap region (0.30 to 0.40 eV) associated with film surface defects. The smaller tDOS value confirms that the higher Voc in Example 3 is caused by fewer defects, because surface charge traps have been shown to be the main cause of Voc loss in solar cells.
[0071] refer to Fig.16 After storing the unpackaged device at room temperature and relative humidity of about 45% for 720 hours, the degradation of Example 3 was negligible. The enhanced environmental stability of PSCs is mainly attributed to the high-quality, pinhole-free, purer phase, and less defective CsPbBr3 perovskite film.
[0072] The device performance tests of Examples 1 to 4 and the comparative example are shown in the following table: Voc is the open circuit voltage, Jsc is the short circuit current density, FF is the fill factor, and PCE is the photoelectric conversion efficiency. Compared with the comparative example, the above performances of Examples 1 to 4 have been effectively improved. It is worth noting that the device efficiency of Example 3 is as high as 10.08%, with a Voc of 1.62V and a Jsc of 7.96mA cm -2 , FF is 78.11%.
[0073]
[0074] The present invention adopts the method of dripping cesium bromide / methanol solution during the lead bromide spin coating process to prepare a Cs-Pb-Br film with a mesoporous structure to promote the subsequent sufficient reaction of CsBr and PbBr2, which is beneficial to improve the purity of the CsPbBr3 phase. In addition, due to the pre-doping of cesium bromide, the CsPb2Br5 crystal size generated by pre-crystallization is smaller and the nucleation sites are denser, which is beneficial to obtain a perovskite thin film battery with a larger grain size and fewer defects.
[0075] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some or all of the technical features thereof may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. Preparation of CsPbBr by CsB pre-doping 3 Perovskite thin film battery method, Features: The steps include: 1) Pretreatment of conductive transparent substrate; 2) Preparation of electron transport layer: Spin coating SnO on the surface of conductive transparent substrate 2 thin film, forming an electron transport layer; 3) Pre-doping with cesium bromide: Spin coating PbBr on the surface of the electron transport layer 2 solution, and at the same time, dropwise add CsBr methanol solution, and anneal in ambient atmosphere to form a pre-doped film; 4) Preparing a perovskite layer: spin coating a methanol solution of CsBr on the surface of the pre-doped film to form a perovskite layer; 5) Preparing electrodes: forming electrodes on the surface of the perovskite layer.
2. Preparation of CsPbBr by cesium bromide pre-doping according to claim 1 3 Perovskite thin film battery method, Features: 2) Preparation of electron transport layer: SnO 2 The dispersant and deionized water were diluted in a volume ratio of 1:4, and then the diluted SnO 2 The dispersant was spin-coated on the substrate at a speed of 3500 rpm, and then annealed at 150° C. for 30 min to obtain an electron transport layer.
3. Preparation of CsPbBr by cesium bromide pre-doping according to claim 1 3 Perovskite thin film battery method, Features: 3) Pre-doping with cesium bromide: PbBr 2 The solution was spin-coated on the surface of the deposited electron transport layer at a speed of 2000 rpm for 30 s, and then annealed on a hot plate at 100 °C for 30 min. 2 During the spin coating process of the solution, a methanol solution of CsBr was added dropwise to obtain a pre-doped film.
4. The method for preparing CsPbBr by cesium bromide pre-doping according to claim 3 3 Perovskite thin film battery method, Features: In step 3), the PbBr 2 The concentration of CsBr is 1.0 M, the concentration of CsBr in the methanol solution of CsBr is 0.07 M, and the dosage is 120 μL.
5. The method for preparing CsPbBr by cesium bromide pre-doping according to claim 3 3 Perovskite thin film battery method, Features: 4) Preparation of perovskite layer: After cooling to room temperature, CsBr methanol solution was spin coated on the surface of the pre-doped film at a speed of 2000 rpm for 30 s, and then heated at 250° C. for 5 min to obtain the perovskite layer.
6. The method for preparing CsPbBr by cesium bromide pre-doping according to claim 5 3 Perovskite thin film battery method, Features: In step 4), the concentration of CsBr in the methanol solution of CsBr is 0.07M.
7. The method for preparing CsPbBr by cesium bromide pre-doping according to claim 5 3 Perovskite thin film battery method, Features: In step 4), the spin coating is performed 7 times.
8. The method for preparing CsPbBr by cesium bromide pre-doping according to claim 1 3 Perovskite thin film battery method, Features: 5) Electrode preparation: Use a screen to print carbon paste on the surface of the perovskite layer to form a carbon electrode, completing the production of the perovskite thin film battery.
9. The method for preparing CsPbBr by cesium bromide pre-doping according to claim 1 3 Perovskite thin film battery method, Features: In step 1), the conductive transparent substrate is an ITO conductive glass substrate. 10.CsPbBr 3 Perovskite thin film battery, Features: The method according to any one of claims 1 to 9 is used to prepare the conductive transparent substrate, the electron transport layer, the perovskite layer and the counter electrode, which are arranged in sequence.
Citation Information
Patent Citations
Preparation method of high-quality CsPbI2Br inorganic perovskite film
CN109638162A
All-inorganic CsPbBr3 perovskite solar cell based on PbBr2 micropore regulation and control and preparation method and application thereof
CN110289327A
CsPbBr3 perovskite thin film and preparation method and application thereof
CN117623373A