Preparation method of perovskite layer, laminated solar cell and preparation method of laminated solar cell

Through magnetron sputtering technology, the problem of poor deposition effect of perovskite layer on suede crystal silicon substrate is solved, the formation of high-quality perovskite layer is achieved, and the light absorption rate of solar cells is improved. and stability.

CN118922040APending Publication Date: 2024-11-08SHENZHEN HIKING PV TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410932018.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-12
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing perovskite layer has poor deposition effect on suede crystal silicon substrate, resulting in large absorption loss, poor stability and easy short circuit in solar cells.

Method used

Magneto-controlled sputtering process instead of the traditional two-step drying method, and sputter ammonium salt film on the surface of lead iodide/cesium bromide mixed film through a high-vacuum magnetron sputtering machine to increase the contact surface area and form high-quality and low defect density Conformal perovskite layer.

Benefits of technology

The light absorption and stability of stacked solar cells are improved, lead iodide residues are reduced, and the quality of the perovskite layer and the overall performance of the solar cell are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118922040A_ABST
    Figure CN118922040A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of a perovskite layer, a laminated solar cell and a preparation method of the laminated solar cell, and belongs to the field of perovskite laminated solar cells. The co-evaporation method and the magnetron sputtering method are combined, the lead iodide / cesium bromide mixed film is prepared through the co-evaporation method, the ammonium salt film is deposited on the lead iodide / cesium bromide mixed film through the magnetron sputtering method, and due to the fact that the energy of the magnetron sputtering method is high, the ammonium salt film can be effectively deposited on the lead iodide / cesium bromide mixed film; therefore, the prepared laminated solar cell has excellent light absorption performance and attenuation rate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a perovskite tandem solar cell, and in particular to a method for preparing a perovskite layer and a tandem solar cell and a preparation method thereof. Background Art

[0002] Solar cells are environmentally friendly and renewable, with long service life and low maintenance costs. They are suitable for applications in a variety of fields, including but not limited to household and industrial electricity, communication technology, petroleum and solar energy architecture. Solar cells are devices that directly convert light energy into electrical energy through photoelectric effect or photochemical effect. In physics, it is called solar photovoltaic. The working principle of solar cells is based on the photovoltaic effect of semiconductor PN junction. When sunlight or other light irradiates the PN junction of a semiconductor, a voltage appears on both sides of the PN junction, namely the photovoltage. This effect is caused by the electron-hole pairs generated by light irradiating the PN junction. Under the action of the internal electric field, the electrons and holes flow to the N region and the P region respectively, thereby generating an electromotive force between the N region and the P region.

[0003] Crystalline silicon solar cells are currently widely used solar energy conversion technologies. Crystalline silicon solar cells have high conversion efficiency, good stability and low cost. Among them, perovskite / crystalline silicon stacking technology has become one of the research hotspots in the field of photovoltaic technology and has attracted widespread attention. The development of this technology is of great significance to improving the photoelectric conversion efficiency of solar cells and reducing manufacturing costs, thereby promoting the further development and application of solar power generation technology. The theoretical effective photoelectric conversion efficiency of crystalline silicon / perovskite stacked solar cells is as high as more than 40%, which is much higher than that of crystalline silicon solar cells. The basic principle of perovskite / crystalline silicon stacking technology is to stack perovskite materials and crystalline silicon materials together to form a heterojunction, and use the wide band gap, high absorption coefficient and high carrier mobility of perovskite materials and the stability and good electron transmission performance of crystalline silicon materials to improve the photoelectric conversion efficiency of solar cells.

[0004] The crystalline silicon in crystalline silicon solar cells can be polished crystalline silicon or textured crystalline silicon, of which polished crystalline silicon is more commonly used, but the light absorption loss of polished crystalline silicon / perovskite tandem solar cells is large and the short-circuit current density is low. Therefore, the method of using textured crystalline silicon to replace polished crystalline silicon has been commercialized on a large scale. Textured crystalline silicon can greatly reduce the reflection of incident light by the device, improve light absorption, and reduce light absorption loss. However, the current preparation method for textured crystalline silicon / perovskite tandem solar cells is still based on polished crystalline silicon, and its preparation method is mainly a solution wet method or a two-step dry method. In the textured crystalline silicon / perovskite tandem solar cell prepared by the solution wet method, due to the unevenness of the textured crystalline silicon substrate, the perovskite layer cannot be fully and conformally covered on the textured crystalline silicon substrate, thereby causing a short circuit in the device; and the two-step dry method generally uses an evaporation method to first prepare a lead iodide and cesium bromide mixed film of the perovskite stack, and then uses an evaporation method to prepare an ammonium salt film, and finally heats and deposits the ammonium salt film on the lead iodide and cesium bromide mixed film to form a conformal perovskite film, thereby improving the comprehensive coverage of the perovskite layer and the textured crystalline silicon.

[0005] However, in the traditional two-step dry method, during the heating deposition of the ammonium salt film and the lead iodide-cesium bromide mixed film, the lead iodide near the buried bottom surface in the lead iodide-cesium bromide mixed film is difficult to react completely because it does not directly contact the ammonium salt film, and eventually a large amount of lead iodide residue is formed in the lower layer of the perovskite film. These free lead iodides will form a large number of defects in the perovskite film, resulting in low quality of the formed perovskite film, thus affecting device performance.

[0006] In summary, in order to improve the light absorption rate, polished crystalline silicon is replaced by velvet crystalline silicon. However, due to the unevenness of velvet crystalline silicon, the existing perovskite film cannot be completely conformally covered. Therefore, a two-step dry method for preparing polished crystalline silicon / perovskite stacked solar cells is proposed. However, the deposition effect of the perovskite layer in this method is poor, resulting in a large amount of lead iodide residue, which causes a large number of defects in the perovskite layer and poor battery performance, which is still a problem that needs to be solved urgently. Summary of the invention

[0007] The purpose of the present invention is to overcome the problem that the deposition effect of ammonium salt on the surface of lead iodide / cesium bromide mixed film in the existing perovskite layer is poor, resulting in large light absorption loss, poor stability and easy short circuit of the stacked solar cell. A preparation method of a perovskite layer and a stacked solar cell are proposed. In the method, a magnetron sputtering process is used to replace the second step evaporation method in the traditional two-step dry method for preparing the perovskite layer. The ammonium salt has higher energy when deposited on the lead iodide / cesium bromide mixed film through the magnetron sputtering process. The ammonium salt can be embedded in the lead iodide / cesium bromide mixed film to increase the contact surface area, form a high-quality and low-defect density conformal perovskite layer, and improve the performance of the stacked solar cell.

[0008] To achieve the above object, the specific scheme provided by the present invention is as follows.

[0009] A method for preparing a perovskite layer comprises the following steps:

[0010] Step 1, preparing a lead iodide / cesium bromide mixed film on a substrate material by co-evaporation of lead iodide and cesium bromide;

[0011] Step 2, placing the lead iodide / cesium bromide mixed film in a vacuum chamber of a high vacuum magnetron sputtering machine, grinding formamidine iodide (FAI) and formamidine bromide (FABr) into powder to prepare a target material, and using a high vacuum magnetron sputtering machine to sputter the target material on the surface of the lead iodide / cesium bromide mixed film to obtain an ammonium salt film;

[0012] Step 3: After the ammonium salt film is sputtered, the lead iodide / cesium bromide mixed film is heated to obtain a perovskite layer.

[0013] Furthermore, the base material in step 1 is a velvet base; the velvet base includes a velvet crystalline silicon layer, a tunneling layer and a hole transport layer sequentially arranged on one surface of the velvet crystalline silicon layer, and a first conductive transparent layer and a first metal electrode layer arranged on another surface of the velvet crystalline silicon layer, and the perovskite layer is arranged on the hole transport layer.

[0014] Furthermore, in the co-evaporation method in step 1, the evaporation rate ratio of lead iodide to cesium bromide is (2:1)-(10:1).

[0015] Furthermore, in the step 1, the evaporation rate of lead iodide in the co-evaporation method is 1-10 A / s, and the evaporation rate of cesium bromide in the co-evaporation method is 0.1-10 A / s.

[0016] Furthermore, the total evaporation time of the co-evaporation method in step 1 is 1-10000s.

[0017] Furthermore, the thickness of the lead iodide / cesium bromide mixed film in step 1 is 200-800 nm.

[0018] Furthermore, in step 2, the mass ratio of formamidine iodide to formamidine bromide is (1:10)-(10:1).

[0019] Furthermore, the vacuum degree of the high vacuum magnetron sputtering machine in step 2 is 5×10 -5 -2×10 -4 Pa.

[0020] Furthermore, the power of the high vacuum magnetron sputtering machine in step 2 is 30-200W.

[0021] Furthermore, the thickness of the ammonium salt film in step 2 is 100-800 nm.

[0022] Furthermore, in step 3, the heating temperature is 80-200° C., and the heating time is 1-60 min.

[0023] The present invention also provides a stacked solar cell, which is prepared by the preparation method of the perovskite layer; the stacked solar cell comprises, from bottom to top, a first metal electrode layer, a first transparent electrode layer, a P-type base doping layer, a base passivation layer, a velvet crystalline silicon substrate, a base surface passivation layer, an N-type base doping layer, a tunneling layer, a hole transport layer, a perovskite layer, a passivation layer, an electron transport layer, a buffer layer, a second transparent electrode layer, a second metal electrode layer and an anti-reflection layer.

[0024] Furthermore, the method for preparing the stacked solar cell is as follows: providing a textured crystalline silicon substrate, preparing the base passivation layer on the back of the textured crystalline silicon substrate, preparing the P-type base doping layer on the surface of the base passivation layer, preparing the first transparent electrode layer on the surface of the P-type base doping layer, and preparing the first metal electrode layer on the surface of the first transparent electrode layer;

[0025] Furthermore, the base surface passivation layer is prepared on the surface of the textured crystalline silicon substrate, an N-type base doping layer is prepared on the surface of the base surface passivation layer, the tunneling layer is prepared on the surface of the N-type base doping layer, the hole transport layer is prepared on the surface of the tunneling layer, the perovskite layer is prepared on the surface of the hole transport layer, the passivation layer is prepared on the surface of the perovskite layer, the electron transport layer is prepared on the surface of the passivation layer, the buffer layer is prepared on the surface of the electron transport layer, the second transparent electrode layer is prepared on the surface of the buffer layer, the second metal electrode layer is prepared on the surface of the second transparent electrode layer, and the anti-reflection layer is prepared on the surface of the second metal electrode layer.

[0026] Specifically, the method for preparing the stacked solar cell comprises the following steps:

[0027] Step 1, preparing a base passivation layer on the back of a textured silicon substrate, and diffusing a phosphorus source into the base passivation layer to form a P-type base doping layer; preparing a base surface passivation layer on the surface of the textured silicon substrate, and diffusing a nitrogen source into the base surface passivation layer to form an N-type base doping layer, and finally obtaining a sample 1;

[0028] Step 2: Preparation of the first transparent electrode layer:

[0029] Sample 1 is placed in a vacuum chamber of a high vacuum magnetron sputtering machine, an indium tin oxide (ITO) target is set, and a first transparent electrode layer with a thickness of 10-200 nm is prepared on the surface of the P-type base doping layer in sample 1 by magnetron sputtering to obtain sample 2; wherein the power of the high vacuum magnetron sputtering machine is 50-200 W, and the operating time is 0.5-2 h;

[0030] Step 3: Preparation of the first metal electrode layer:

[0031] Sample 2 was placed on a mask plate, and a first metal electrode layer with a thickness of 10-200 nm was prepared by evaporation to obtain sample 3. The vacuum degree of the evaporation method was 5×10 -5 -2×10 -4 Pa, temperature is 500-2000℃, evaporation rate is 0.1-5Å / S;

[0032] Step 4: Preparation of tunneling layer:

[0033] Place the sample three on a mask plate and then place it in a vacuum chamber of a high vacuum magnetron sputtering machine, and use a magnetron sputtering method to prepare a tunneling layer with a thickness of 10-200nm on the surface of the N-type base doping layer of the sample three to obtain a sample four; the power of the magnetron sputtering equipment is 50-100W, and the operating time is 0.5-2h;

[0034] Step 5: Preparation of hole transport layer:

[0035] Clean sample 4 with an ultraviolet ozone cleaner (UV-Ozone) for 5-50 minutes, apply the hole transport layer dispersion liquid to the surface of the tunnel layer of sample 4 evenly after ultrasonic treatment for 5-20 minutes, prepare a hole transport layer with a thickness of 10-200 nm by spin coating, and after the spin coating is completed, perform annealing operation to obtain sample 5; the spin coating speed of the spin coating method is 1000-5000 rpm, the spin coating time is 10-100 s, the amount of the spin coating solution is 10-100 ul, the annealing temperature is 300-600°C, and the annealing time is 10-50 min;

[0036] Step 6: Preparation of perovskite layer:

[0037] Lead iodide and cesium bromide are co-evaporated to prepare a lead iodide / cesium bromide mixed film with a thickness of 200-800 nm on the surface of the hole transport layer in sample five, and then the sample five after the co-evaporation of the lead iodide / cesium bromide mixed film is placed in the vacuum chamber of a high vacuum magnetron sputtering machine, and formamidine iodide (FAI) and formamidine bromide (FABr) are ground into powder to prepare a target material, and an ammonium salt film with a thickness of 200-800 nm is sputtered on the surface of the lead iodide / cesium bromide mixed film by a high vacuum magnetron sputtering machine, and the lead iodide / cesium bromide mixed film after the ammonium salt film is sputtered is heated to obtain a sample six with a perovskite layer deposited thereon;

[0038] The evaporation rate of lead iodide is 0-10A / s, the evaporation rate of cesium bromide is 0-10A / s, the evaporation rate ratio of lead iodide to cesium bromide in the co-evaporation method is (2:1)-(10:1), the total evaporation time of the co-evaporation method is 1-10000s, the mass ratio of formamidine iodide to formamidine bromide is (1:10)-(10:1), the vacuum degree of the high vacuum magnetron sputtering machine is 5×10 -5 -2×10 -4 Pa, the power of the high vacuum magnetron sputtering machine is 30-200W, the thickness of the ammonium salt film is 100-800nm, the heating temperature is 80-200℃, and the heating time is 1-60min;

[0039] Step 7: Preparation of passivation layer:

[0040] Sample 6 is placed on a mask, and 1-5 mg of propylene diamine iodide is evaporated onto the surface of the perovskite layer of the sample 6 by evaporation to obtain a passivation layer with a thickness of 1-20 nm. After the evaporation is completed, annealing operation is performed to obtain sample 7; the evaporation vacuum degree is (1-5)×10 -4 Pa, evaporation temperature is 50-400℃, evaporation rate is 0.05-1Å / S, annealing temperature is 0-150℃, and annealing time is 0-30min;

[0041] The passivation layer can also be prepared by a spin coating method, specifically: dissolving propylene diamine iodide in an organic solvent, ultrasonically dissolving it until it is completely dissolved, and then spin coating it on the surface of the perovskite layer of the sample six to obtain a passivation layer with a thickness of 1-20nm. After the spin coating is completed, annealing operation is performed to obtain sample seven; the concentration of propylene diamine iodine is 0.1-6mg / mL, the organic solvent is one or more of methanol, ethanol or isopropanol, the ultrasonic time is 0-30min, the spin coating speed is 1000-7000rpm, the spin coating time is 20-120s, the annealing temperature is 40-160℃, and the annealing time is 5-40min;

[0042] The passivation layer can also be prepared by a spraying method, specifically: spraying a propylene diamine iodine dispersion on the surface of the perovskite layer of the sample six to obtain a passivation layer with a thickness of 1-20 nm, and after the spin coating is completed, performing an annealing operation to obtain a sample seven; the spraying rate is 0-100 cm / s, the annealing temperature is 20-170° C., and the annealing time is 0-30 min;

[0043] Step 8: Preparation of electron transport layer:

[0044] The electron transport layer material is evenly coated on the surface of the passivation layer of the sample 7 to obtain the sample 8 coated with the electron transport layer with a thickness of 10-100 nm; the spin coating speed is 500-4000 rpm, and the spin coating time is 10-80 s;

[0045] The electron transport layer can also be prepared by evaporation, specifically: evaporating the electron transport layer material onto the surface of the passivation layer of sample 7 to obtain sample 8 coated with an electron transport layer with a thickness of 10-100 nm; the vacuum degree of the evaporation is 5×10 -5 -5×10 -4 Pa, the evaporation temperature is 100-400℃, and the evaporation rate is 0.05-1Å / S;

[0046] Step 9: Preparation of buffer layer:

[0047] The buffer layer material is deposited onto the surface of the electron transport layer of the sample eight by atomic accumulation deposition using an atomic accumulation deposition device to obtain a sample nine having a buffer layer with a thickness of 10-100 nm; the deposition vacuum degree is (0-1)×10 4 Pa, the deposition pipeline temperature is between 50-150°C, and the deposition chamber temperature is 40-150°C;

[0048] The buffer layer can also be prepared by evaporation, specifically: evaporating the buffer layer material onto the surface of the electron transport layer of sample eight to obtain sample nine with a buffer layer deposited with a thickness of 10-100 nm; the evaporation vacuum degree is 6×10 -5 -4×10 -4 Pa, the evaporation temperature is 100-500℃, and the evaporation rate is 0.05-1Å / S;

[0049] Step 10: Preparation of the second transparent electrode layer:

[0050] The transparent electrode material is sputtered onto the surface of the buffer layer of the sample nine by using a magnetron sputtering method, and an indium zinc oxide (IZO) target is set to obtain a sample ten with a second transparent electrode layer having a thickness of 10-200 nm. The power of the magnetron sputtering method is 30-200 W, and the operation time is 0.5-2 hours.

[0051] The second transparent electrode layer can also be prepared by an evaporation method, specifically: evaporating the transparent electrode material onto the surface of the buffer layer of sample nine to obtain sample ten sputtered with a second transparent electrode layer having a thickness of 10-200 nm; the evaporation vacuum degree of the evaporation method is 1×10 -5 -5×10 -4 Pa, the evaporation temperature is 1000-2000℃, and the evaporation rate is 0.05-3Å / S;

[0052] Step 11: Preparation of the second metal electrode layer:

[0053] Sample 10 was placed on a mask plate, and a second metal electrode layer with a thickness of 10-200 nm was prepared by evaporation to obtain sample 11. The vacuum degree of the evaporation was 5×10 -5 -2×10 -4 Pa, temperature is 500-2000℃, evaporation rate is 0.1-5Å / S;

[0054] Step 12: Preparation of anti-reflection layer:

[0055] The anti-reflection layer material is sputtered onto the surface of the second metal electrode layer of the sample eleven by a magnetron sputtering method to obtain a laminated solar cell with an anti-reflection layer sputtered with a thickness of 10-200 nm; the power of the magnetron sputtering method is 30-200 W;

[0056] The anti-reflection layer can also be prepared by evaporation, specifically: placing the sample 11 on a mask, evaporating to the surface of the second metal electrode layer of the sample 11 by evaporation to obtain an anti-reflection layer with a thickness of 10-200nm, and after evaporation, performing annealing to obtain a stacked solar cell; the evaporation vacuum degree is (1-5)×10 -4 Pa, the evaporation temperature is 50-400℃, the evaporation rate is 0-5Å / S, the annealing temperature is 0-150℃, and the annealing time is 0-30min.

[0057] Furthermore, the hole transport layer dispersion in step 5 is one or more of poly[bis(4-phenyl)(2,4,6-trimethylphenyl)amine] (PTAA), poly-3-hexylthiophene (P3HT), nickel oxide (NiOx), molybdenum trioxide (MoO3), cuprous iodide (CuI), and cuprous thiocyanate (CuSCN), the solvent of the hole transport layer dispersion is ultrapure water, and the concentration of the hole transport layer dispersion is 0.05 mol / mL.

[0058] Furthermore, the composition of the perovskite layer in step 6 may be an ABX3 structure, wherein:

[0059] A position is an organic cation, including CH3NH3 +(MA+), NH2CH=NH2 + (FA+), CH3CH2NH3 + or Cs + One or more of the following;

[0060] The B position is a metal cation, including Pb 2+ Sn 2+ One or more of the following;

[0061] The X position is a halogen anion, including F - , Cl - Br - ,I - One or more of the .

[0062] Furthermore, the components of the passivation layer in step 7 include one or more of propylenediamine iodide, propylenediamine bromide (PDADBr), butylammonium chloride (BACl), butylammonium bromide (BABr), butylammonium iodide (BAI), N,N-dimethyl-1,3-propylenediamine hydrochloride (DMePDADCl), dodecanediaminium bromide (DDDADBr), magnesium fluoride, lithium fluoride (LiF), and sodium fluoride (NaF).

[0063] Furthermore, the components of the electron transport layer material in step 8 are zinc oxide (ZnO), tin dioxide (SnO2), titanium dioxide (TiO2), [6,6]-phenyl C 61 Methyl butyrate (PC 61 BM), carbon 60 (C 60 ), 2,9-dimethyl-4,7-diphenyl-1,10-phenanthroline (BCP) or more thereof.

[0064] Furthermore, the buffer layer material in step 9 is tin oxide (SnO2).

[0065] Furthermore, the component of the transparent electrode material of the buffer layer in step 10 is one or more of zinc oxide (ZnO), tin dioxide (SnO2), and titanium dioxide (TiO2).

[0066] Furthermore, in the step 11, the second metal electrode layer is composed of one or more of silver (Ag), gold (Au), copper (Cu), aluminum (Al), and carbon (C).

[0067] Furthermore, the anti-reflection layer in step 12 is composed of one or more of magnesium fluoride, lithium fluoride (LiF), sodium fluoride (NaF), and silicon oxide (SiO2).

[0068] The traditional method for preparing the perovskite layer is a two-step co-evaporation method, in which a lead iodide film is prepared by co-evaporation in the first step, and an ammonium salt film is deposited on the surface of the lead iodide film by co-evaporation in the second step, but the deposition effect of the co-evaporation method is poor, which will affect the performance of the stacked solar cell. The present invention combines the co-evaporation method with the magnetron sputtering method, firstly preparing a lead iodide / cesium bromide mixed film by co-evaporation, and then depositing the ammonium salt film on the lead iodide / cesium bromide mixed film by magnetron sputtering. Due to the high energy of the magnetron sputtering method, the ammonium salt film can be effectively deposited on the lead iodide / cesium bromide mixed film, and the stacked solar cell prepared thereby has excellent light absorption performance and attenuation rate. BRIEF DESCRIPTION OF THE DRAWINGS

[0069] Figure 1 This is a process diagram for preparing the perovskite layer of the stacked solar cell described in Examples 1-3;

[0070] Figure 2 This is a process diagram for preparing the perovskite layer of the stacked solar cell described in Comparative Example 1. DETAILED DESCRIPTION

[0071] The technical solutions in the embodiments of the present invention will be described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.

[0072] In the description of the present invention, unless otherwise specified, "multiple" means two or more; the terms "center", "longitudinal", "lateral", "up", "down", "left", "right", "inside", "outside", "front end", "rear end", "head", "tail", "vertical", "horizontal", "top", "bottom", "inside", "outside" and the like indicate the orientation or position relationship based on the orientation or position relationship shown in the drawings, which is only for the convenience of describing the present invention and simplifying the description, and does not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operate in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, the terms "first", "second", "third" and the like are used for descriptive purposes only and cannot be understood as indicating or implying relative importance.

[0073] Example 1

[0074] The present embodiment provides a stacked solar cell, which is prepared by the preparation method of the perovskite layer; the stacked solar cell comprises, from bottom to top, a first metal electrode layer, a first transparent electrode layer, a P-type base doping layer, a base passivation layer, a velvet crystalline silicon substrate, a base surface passivation layer, an N-type base doping layer, a tunneling layer, a hole transport layer, a perovskite layer, a passivation layer, an electron transport layer, a buffer layer, a second transparent electrode layer, a second metal electrode layer and an anti-reflection layer.

[0075] Furthermore, the preparation order of the stacked solar cell is: preparing the base passivation layer on the back of the textured crystalline silicon substrate, preparing the P-type base doping layer on the surface of the base passivation layer, preparing the first transparent electrode layer on the surface of the P-type base doping layer, and preparing the first metal electrode layer on the surface of the first transparent electrode layer;

[0076] The substrate surface passivation layer is prepared on the surface of the textured crystalline silicon substrate, an N-type substrate doping layer is prepared on the surface of the substrate surface passivation layer, the tunneling layer is prepared on the surface of the N-type substrate doping layer, the hole transport layer is prepared on the surface of the tunneling layer, the perovskite layer is prepared on the surface of the hole transport layer, the passivation layer is prepared on the surface of the perovskite layer, the electron transport layer is prepared on the surface of the passivation layer, the buffer layer is prepared on the surface of the electron transport layer, the second transparent electrode layer is prepared on the surface of the buffer layer, the second metal electrode layer is prepared on the surface of the second transparent electrode layer, and the anti-reflection layer is prepared on the surface of the second metal electrode layer.

[0077] Furthermore, the method for preparing the stacked solar cell comprises the following steps:

[0078] Step 1, preparing a base passivation layer on the back of a textured silicon substrate, and diffusing a phosphorus source into the base passivation layer to form a P-type base doping layer; preparing a base surface passivation layer on the surface of the textured silicon substrate, and diffusing a nitrogen source into the base surface passivation layer to form an N-type base doping layer, and finally obtaining a sample 1;

[0079] Step 2: Preparation of the first transparent electrode layer:

[0080] Sample 1 is placed in a vacuum chamber of a high vacuum magnetron sputtering machine, an indium tin oxide (ITO) target is set, and a first transparent electrode layer with a thickness of 100 nm is prepared on the surface of the P-type base doping layer in sample 1 by magnetron sputtering to obtain sample 2; wherein the power of the high vacuum magnetron sputtering machine is 60 W, and the operating time is 1.5 h;

[0081] Step 3: Preparation of the first metal electrode layer:

[0082] Sample 2 was placed on a mask plate, and a first metal electrode layer with a thickness of 200 nm was prepared by evaporation to obtain sample 3. The vacuum degree of the evaporation method was 2×10 -4 Pa, temperature is 800°C, evaporation rate is 2.5Å / S;

[0083] Step 4: Preparation of tunneling layer:

[0084] Sample 3 was placed on a mask plate and then placed in a vacuum chamber of a high vacuum magnetron sputtering machine, and a tunneling layer with a thickness of 40 nm was prepared on the surface of the N-type base doping layer of the sample 3 by magnetron sputtering to obtain sample 4; the power of the magnetron sputtering equipment was 60 W, and the operation time was 1 hour;

[0085] Step 5: Preparation of hole transport layer:

[0086] Sample 4 was cleaned with an ultraviolet ozone cleaner (UV-Ozone) for 15 minutes, and the hole transport layer dispersion was evenly coated on the surface of the tunnel layer of the sample 4 after ultrasonic treatment for 20 minutes, and a hole transport layer with a thickness of 20 nm was prepared by spin coating. After the spin coating was completed, annealing was performed to obtain sample 5; the spin coating speed of the spin coating method was 2000 rpm, the spin coating time was 40 s, the spin coating solution amount was 100 ul, the annealing temperature was 450°C, and the annealing time was 30 min;

[0087] Step 6: Preparation of perovskite layer:

[0088] Lead iodide and cesium bromide are co-evaporated to prepare a lead iodide / cesium bromide mixed film with a thickness of 440 nm on the surface of the hole transport layer in sample five, and then the sample five after the co-evaporation of the lead iodide / cesium bromide mixed film is placed in the vacuum chamber of a high vacuum magnetron sputtering machine, and formamidine iodide (FAI) and formamidine bromide (FABr) are ground into powder to prepare a target material, and an ammonium salt film with a thickness of 400 nm is sputtered on the surface of the lead iodide / cesium bromide mixed film by a high vacuum magnetron sputtering machine, and the lead iodide / cesium bromide mixed film after the ammonium salt film is sputtered is heated to obtain a sample six with a perovskite layer deposited thereon;

[0089] The evaporation rate of lead iodide is 8A / s, the evaporation rate of cesium bromide is 0.8A / s, the evaporation rate ratio of lead iodide to cesium bromide in the co-evaporation method is 10:1, the total evaporation time of the co-evaporation method is 1000s, the thickness of the lead iodide / cesium bromide mixed film is 440nm, the mass ratio of formamidine iodide to formamidine bromide is 4.7:1, the vacuum degree of the high vacuum magnetron sputtering machine is 5×10 -5 Pa, the power of the high vacuum magnetron sputtering machine is 30W, the thickness of the ammonium salt film is 400nm, the heating temperature is 150°C, and the heating time is 30min;

[0090] Step 7: Preparation of passivation layer:

[0091] Sample 6 was placed on a mask, and 3 mg of propylene diamine iodide was evaporated onto the surface of the perovskite layer of the sample 6 by evaporation to obtain a passivation layer with a thickness of 4 nm. After the evaporation was completed, annealing was performed to obtain sample 7. The evaporation vacuum degree was 2×10 -4Pa, evaporation temperature is 80℃, evaporation rate is 0.1Å / S, annealing temperature is 100℃, and annealing time is 8min;

[0092] Step 8: Preparation of electron transport layer:

[0093] The electron transport layer material was evaporated onto the surface of the passivation layer of the sample 7 to obtain the sample 8 coated with an electron transport layer with a thickness of 20 nm; the vacuum degree of the evaporation was 1×10 -4 Pa, the evaporation temperature is 200 °C, and the evaporation rate is 0.1 Å / S;

[0094] Step 9: Preparation of buffer layer:

[0095] The buffer layer material was deposited onto the surface of the electron transport layer of sample eight by atomic accumulation deposition using an atomic accumulation deposition device to obtain sample nine with a buffer layer having a thickness of 15 nm. The deposition vacuum degree was 0.5×10 4 Pa, the deposition pipeline temperature is between 70°C and the deposition chamber temperature is 60°C;

[0096] Step 10: Preparation of the second transparent electrode layer:

[0097] The transparent electrode material is sputtered onto the surface of the buffer layer of sample nine by using a magnetron sputtering method, and an indium zinc oxide (IZO) target is set to obtain sample ten with a second transparent electrode layer having a thickness of 100 nm. The power of the magnetron sputtering method is 50 W, and the operation time is 1 hour.

[0098] Step 11: Preparation of the second metal electrode layer:

[0099] Sample 10 was placed on a mask plate, and a second metal electrode layer with a thickness of 100 nm was prepared by evaporation to obtain sample 11. The vacuum degree of the evaporation was 2×10 -4 Pa, temperature is 800°C, evaporation rate is 0.1Å / S;

[0100] Step 12: Preparation of anti-reflection layer:

[0101] Sample 11 was placed on a mask plate, and the second metal electrode layer of the sample 11 was evaporated by evaporation to obtain an anti-reflection layer with a thickness of 100 nm. After the evaporation was completed, an annealing operation was performed to obtain a stacked solar cell. The evaporation vacuum degree was 2×10 -4 Pa, the evaporation temperature is 80℃, the evaporation rate is 2Å / S, the annealing temperature is 100℃, and the annealing time is 8min.

[0102] Example 2

[0103] The present embodiment provides a stacked solar cell, which is prepared from the perovskite layer; the stacked solar cell comprises, from bottom to top, a first metal electrode layer, a first transparent electrode layer, a P-type base doping layer, a base passivation layer, a velvet crystalline silicon substrate, a base surface passivation layer, an N-type base doping layer, a tunneling layer, a hole transport layer, a perovskite layer, a passivation layer, an electron transport layer, a buffer layer, a second transparent electrode layer, a second metal electrode layer and an anti-reflection layer.

[0104] Furthermore, the preparation order of the stacked solar cell is: preparing the base passivation layer on the back of the textured crystalline silicon substrate, preparing the P-type base doping layer on the surface of the base passivation layer, preparing the first transparent electrode layer on the surface of the P-type base doping layer, and preparing the first metal electrode layer on the surface of the first transparent electrode layer;

[0105] The substrate surface passivation layer is prepared on the surface of the textured crystalline silicon substrate, an N-type substrate doping layer is prepared on the surface of the substrate surface passivation layer, the tunneling layer is prepared on the surface of the N-type substrate doping layer, the hole transport layer is prepared on the surface of the tunneling layer, the perovskite layer is prepared on the surface of the hole transport layer, the passivation layer is prepared on the surface of the perovskite layer, the electron transport layer is prepared on the surface of the passivation layer, the buffer layer is prepared on the surface of the electron transport layer, the second transparent electrode layer is prepared on the surface of the buffer layer, the second metal electrode layer is prepared on the surface of the second transparent electrode layer, and the anti-reflection layer is prepared on the surface of the second metal electrode layer.

[0106] Furthermore, the method for preparing the stacked solar cell comprises the following steps:

[0107] Step 1, preparing a base passivation layer on the back of a textured silicon substrate, and diffusing a phosphorus source into the base passivation layer to form a P-type base doping layer; preparing a base surface passivation layer on the surface of the textured silicon substrate, and diffusing a nitrogen source into the base surface passivation layer to form an N-type base doping layer, and finally obtaining a sample 1;

[0108] Step 2: Preparation of the first transparent electrode layer:

[0109] Sample 1 is placed in a vacuum chamber of a high vacuum magnetron sputtering machine, an indium tin oxide (ITO) target is set, and a first transparent electrode layer with a thickness of 100 nm is prepared on the surface of the P-type base doping layer in sample 1 by magnetron sputtering to obtain sample 2; wherein the power of the high vacuum magnetron sputtering machine is 60 W, and the operating time is 1.5 h;

[0110] Step 3: Preparation of the first metal electrode layer:

[0111] Sample 2 was placed on a mask plate, and a first metal electrode layer with a thickness of 200 nm was prepared by evaporation to obtain sample 3. The vacuum degree of the evaporation method was 2×10 -4 Pa, temperature is 800°C, evaporation rate is 2.5Å / S;

[0112] Step 4: Preparation of tunneling layer:

[0113] Sample 3 was placed on a mask plate and then placed in a vacuum chamber of a high vacuum magnetron sputtering machine, and a tunneling layer with a thickness of 40 nm was prepared on the surface of the N-type base doping layer of the sample 3 by magnetron sputtering to obtain sample 4; the power of the magnetron sputtering equipment was 60 W, and the operation time was 1 hour;

[0114] Step 5: Preparation of hole transport layer:

[0115] Sample 4 was cleaned with an ultraviolet ozone cleaner (UV-Ozone) for 15 minutes, and the hole transport layer dispersion was evenly coated on the surface of the tunnel layer of the sample 4 after ultrasonic treatment for 20 minutes, and a hole transport layer with a thickness of 20 nm was prepared by spin coating. After the spin coating was completed, annealing was performed to obtain sample 5; the spin coating speed of the spin coating method was 2000 rpm, the spin coating time was 40 s, the spin coating solution amount was 100 ul, the annealing temperature was 450°C, and the annealing time was 30 min;

[0116] Step 6: Preparation of perovskite layer:

[0117] Lead iodide and cesium bromide are co-evaporated to prepare a lead iodide / cesium bromide mixed film with a thickness of 440 nm on the surface of the hole transport layer in sample five, and then the sample five after the co-evaporation of the lead iodide / cesium bromide mixed film is placed in the vacuum chamber of a high vacuum magnetron sputtering machine, and formamidine iodide (FAI) and formamidine bromide (FABr) are ground into powder to prepare a target material, and an ammonium salt film with a thickness of 400 nm is sputtered on the surface of the lead iodide / cesium bromide mixed film by a high vacuum magnetron sputtering machine, and the lead iodide / cesium bromide mixed film after the ammonium salt film is sputtered is heated to obtain a sample six with a perovskite layer deposited thereon;

[0118] The evaporation rate of lead iodide is 8A / s, the evaporation rate of cesium bromide is 0.8A / s, the evaporation rate ratio of lead iodide to cesium bromide in the co-evaporation method is 10:1, the total evaporation time of the co-evaporation method is 1000s, the thickness of the lead iodide / cesium bromide mixed film is 440nm, the mass ratio of formamidine iodide to formamidine bromide is 10:1, the vacuum degree of the high vacuum magnetron sputtering machine is 5×10 -5 Pa, the power of the high vacuum magnetron sputtering machine is 60W, the thickness of the ammonium salt film is 400nm, the heating temperature is 150°C, and the heating time is 30min;

[0119] Step 7: Preparation of passivation layer:

[0120] Sample 6 was placed on a mask, and 3 mg of propylene diamine iodide was evaporated onto the surface of the perovskite layer of the sample 6 by evaporation to obtain a passivation layer with a thickness of 4 nm. After the evaporation was completed, annealing was performed to obtain sample 7. The evaporation vacuum degree was 2×10 -4 Pa, evaporation temperature is 80℃, evaporation rate is 0.1Å / S, annealing temperature is 100℃, and annealing time is 8min;

[0121] Step 8: Preparation of electron transport layer:

[0122] The electron transport layer material was evaporated onto the surface of the passivation layer of the sample 7 to obtain the sample 8 coated with an electron transport layer with a thickness of 20 nm; the vacuum degree of the evaporation was 1×10 -4 Pa, the evaporation temperature is 200 °C, and the evaporation rate is 0.1 Å / S;

[0123] Step 9: Preparation of buffer layer:

[0124] The buffer layer material was deposited onto the surface of the electron transport layer of sample eight by atomic accumulation deposition using an atomic accumulation deposition device to obtain sample nine with a buffer layer having a thickness of 15 nm. The deposition vacuum degree was 0.5×10 4 Pa, the deposition pipeline temperature is between 70°C and the deposition chamber temperature is 60°C;

[0125] Step 10: Preparation of the second transparent electrode layer:

[0126] The transparent electrode material is sputtered onto the surface of the buffer layer of sample nine by using a magnetron sputtering method, and an indium zinc oxide (IZO) target is set to obtain sample ten with a second transparent electrode layer having a thickness of 100 nm. The power of the magnetron sputtering method is 50 W, and the operation time is 1 hour.

[0127] Step 11: Preparation of the second metal electrode layer:

[0128] Sample 10 was placed on a mask plate, and a second metal electrode layer with a thickness of 100 nm was prepared by evaporation to obtain sample 11. The vacuum degree of the evaporation was 2×10 -4 Pa, temperature is 800°C, evaporation rate is 0.1Å / S;

[0129] Step 12: Preparation of anti-reflection layer:

[0130] Sample 11 was placed on a mask plate, and the second metal electrode layer of the sample 11 was evaporated by evaporation to obtain an anti-reflection layer with a thickness of 100 nm. After the evaporation was completed, an annealing operation was performed to obtain a stacked solar cell. The evaporation vacuum degree was 2×10-4 Pa, the evaporation temperature is 80℃, the evaporation rate is 2Å / S, the annealing temperature is 100℃, and the annealing time is 8min.

[0131] Example 3

[0132] The present embodiment provides a stacked solar cell, which is prepared from the perovskite layer; the stacked solar cell comprises, from bottom to top, a first metal electrode layer, a first transparent electrode layer, a P-type base doping layer, a base passivation layer, a velvet crystalline silicon substrate, a base surface passivation layer, an N-type base doping layer, a tunneling layer, a hole transport layer, a perovskite layer, a passivation layer, an electron transport layer, a buffer layer, a second transparent electrode layer, a second metal electrode layer and an anti-reflection layer.

[0133] Furthermore, the preparation order of the stacked solar cell is: preparing the base passivation layer on the back of the textured crystalline silicon substrate, preparing the P-type base doping layer on the surface of the base passivation layer, preparing the first transparent electrode layer on the surface of the P-type base doping layer, and preparing the first metal electrode layer on the surface of the first transparent electrode layer;

[0134] The substrate surface passivation layer is prepared on the surface of the textured crystalline silicon substrate, an N-type substrate doping layer is prepared on the surface of the substrate surface passivation layer, the tunneling layer is prepared on the surface of the N-type substrate doping layer, the hole transport layer is prepared on the surface of the tunneling layer, the perovskite layer is prepared on the surface of the hole transport layer, the passivation layer is prepared on the surface of the perovskite layer, the electron transport layer is prepared on the surface of the passivation layer, the buffer layer is prepared on the surface of the electron transport layer, the second transparent electrode layer is prepared on the surface of the buffer layer, the second metal electrode layer is prepared on the surface of the second transparent electrode layer, and the anti-reflection layer is prepared on the surface of the second metal electrode layer.

[0135] Furthermore, the method for preparing the stacked solar cell comprises the following steps:

[0136] Step 1, preparing a base passivation layer on the back of a textured silicon substrate, and diffusing a phosphorus source into the base passivation layer to form a P-type base doping layer; preparing a base surface passivation layer on the surface of the textured silicon substrate, and diffusing a nitrogen source into the base surface passivation layer to form an N-type base doping layer, and finally obtaining a sample 1;

[0137] Step 2: Preparation of the first transparent electrode layer:

[0138] Sample 1 is placed in a vacuum chamber of a high vacuum magnetron sputtering machine, an indium tin oxide (ITO) target is set, and a first transparent electrode layer with a thickness of 100 nm is prepared on the surface of the P-type base doping layer in sample 1 by magnetron sputtering to obtain sample 2; wherein the power of the high vacuum magnetron sputtering machine is 60 W, and the operating time is 1.5 h;

[0139] Step 3: Preparation of the first metal electrode layer:

[0140] Sample 2 was placed on a mask plate, and a first metal electrode layer with a thickness of 200 nm was prepared by evaporation to obtain sample 3. The vacuum degree of the evaporation method was 2×10 -4 Pa, temperature is 800°C, evaporation rate is 2.5Å / S;

[0141] Step 4: Preparation of tunneling layer:

[0142] Sample 3 was placed on a mask plate and then placed in a vacuum chamber of a high vacuum magnetron sputtering machine, and a tunneling layer with a thickness of 40 nm was prepared on the surface of the N-type base doping layer of the sample 3 by magnetron sputtering to obtain sample 4; the power of the magnetron sputtering equipment was 60 W, and the operation time was 1 hour;

[0143] Step 5: Preparation of hole transport layer:

[0144] Sample 4 was cleaned with an ultraviolet ozone cleaner (UV-Ozone) for 15 minutes, and the hole transport layer dispersion was evenly coated on the surface of the tunnel layer of the sample 4 after ultrasonic treatment for 20 minutes, and a hole transport layer with a thickness of 20 nm was prepared by spin coating. After the spin coating was completed, annealing was performed to obtain sample 5; the spin coating speed of the spin coating method was 2000 rpm, the spin coating time was 40 s, the spin coating solution amount was 100 ul, the annealing temperature was 450°C, and the annealing time was 30 min;

[0145] Step 6: Preparation of perovskite layer:

[0146] Lead iodide and cesium bromide are co-evaporated to prepare a lead iodide / cesium bromide mixed film with a thickness of 440 nm on the surface of the hole transport layer in sample five, and then the sample five after the co-evaporation of the lead iodide / cesium bromide mixed film is placed in the vacuum chamber of a high vacuum magnetron sputtering machine, and formamidine iodide (FAI) and formamidine bromide (FABr) are ground into powder to prepare a target material, and an ammonium salt film with a thickness of 400 nm is sputtered on the surface of the lead iodide / cesium bromide mixed film by a high vacuum magnetron sputtering machine, and the lead iodide / cesium bromide mixed film after the ammonium salt film is sputtered is heated to obtain a sample six with a perovskite layer deposited thereon;

[0147] The evaporation rate of lead iodide is 8A / s, the evaporation rate of cesium bromide is 0.8A / s, the evaporation rate ratio of lead iodide to cesium bromide in the co-evaporation method is 10:1, the total evaporation time of the co-evaporation method is 1000s, the thickness of the lead iodide / cesium bromide mixed film is 440nm, the mass ratio of formamidine iodide to formamidine bromide is 10:1, the vacuum degree of the high vacuum magnetron sputtering machine is 5×10 -5 Pa, the power of the high vacuum magnetron sputtering machine is 90W, the thickness of the ammonium salt film is 400nm, the heating temperature is 150°C, and the heating time is 30min;

[0148] Step 7: Preparation of passivation layer:

[0149] Sample 6 was placed on a mask, and 3 mg of propylene diamine iodide was evaporated onto the surface of the perovskite layer of the sample 6 by evaporation to obtain a passivation layer with a thickness of 4 nm. After the evaporation was completed, annealing was performed to obtain sample 7. The evaporation vacuum degree was 2×10 -4 Pa, evaporation temperature is 80℃, evaporation rate is 0.1Å / S, annealing temperature is 100℃, and annealing time is 8min;

[0150] Step 8: Preparation of electron transport layer:

[0151] The electron transport layer material was evaporated onto the surface of the passivation layer of the sample 7 to obtain the sample 8 coated with an electron transport layer with a thickness of 20 nm; the vacuum degree of the evaporation was 1×10 -4 Pa, the evaporation temperature is 200 °C, and the evaporation rate is 0.1 Å / S;

[0152] Step 9: Preparation of buffer layer:

[0153] The buffer layer material was deposited onto the surface of the electron transport layer of sample eight by atomic accumulation deposition using an atomic accumulation deposition device to obtain sample nine with a buffer layer having a thickness of 15 nm. The deposition vacuum degree was 0.5×10 4 Pa, the deposition pipeline temperature is between 70°C and the deposition chamber temperature is 60°C;

[0154] Step 10: Preparation of the second transparent electrode layer:

[0155] The transparent electrode material is sputtered onto the surface of the buffer layer of sample nine by using a magnetron sputtering method, and an indium zinc oxide (IZO) target is set to obtain sample ten with a second transparent electrode layer having a thickness of 100 nm. The power of the magnetron sputtering method is 50 W, and the operation time is 1 hour.

[0156] Step 11: Preparation of the second metal electrode layer:

[0157] Sample 10 was placed on a mask plate, and a second metal electrode layer with a thickness of 100 nm was prepared by evaporation to obtain sample 11. The vacuum degree of the evaporation was 2×10 -4 Pa, temperature is 800°C, evaporation rate is 0.1Å / S;

[0158] Step 12: Preparation of anti-reflection layer:

[0159] Sample 11 was placed on a mask plate, and the second metal electrode layer of the sample 11 was evaporated by evaporation to obtain an anti-reflection layer with a thickness of 100 nm. After the evaporation was completed, an annealing operation was performed to obtain a stacked solar cell. The evaporation vacuum degree was 2×10 -4 Pa, the evaporation temperature is 80℃, the evaporation rate is 2Å / S, the annealing temperature is 100℃, and the annealing time is 8min.

[0160] Comparative Example 1

[0161] The present comparative example provides a stacked solar cell, which comprises, from bottom to top, a first metal electrode layer, a first transparent electrode layer, a P-type base doping layer, a base passivation layer, a velvet crystalline silicon substrate, a base surface passivation layer, an N-type base doping layer, a tunneling layer, a hole transport layer, a perovskite layer, a passivation layer, an electron transport layer, a buffer layer, a second transparent electrode layer, a second metal electrode layer and an anti-reflection layer.

[0162] Furthermore, the preparation order of the stacked solar cell is: preparing the base passivation layer on the back of the textured crystalline silicon substrate, preparing the P-type base doping layer on the surface of the base passivation layer, preparing the first transparent electrode layer on the surface of the P-type base doping layer, and preparing the first metal electrode layer on the surface of the first transparent electrode layer;

[0163] The substrate surface passivation layer is prepared on the surface of the textured crystalline silicon substrate, an N-type substrate doping layer is prepared on the surface of the substrate surface passivation layer, the tunneling layer is prepared on the surface of the N-type substrate doping layer, the hole transport layer is prepared on the surface of the tunneling layer, the perovskite layer is prepared on the surface of the hole transport layer, the passivation layer is prepared on the surface of the perovskite layer, the electron transport layer is prepared on the surface of the passivation layer, the buffer layer is prepared on the surface of the electron transport layer, the second transparent electrode layer is prepared on the surface of the buffer layer, the second metal electrode layer is prepared on the surface of the second transparent electrode layer, and the anti-reflection layer is prepared on the surface of the second metal electrode layer.

[0164] Furthermore, the method for preparing the stacked solar cell comprises the following steps:

[0165] Step 1, preparing a base passivation layer on the back of a textured silicon substrate, and diffusing a phosphorus source into the base passivation layer to form a P-type base doping layer; preparing a base surface passivation layer on the surface of the textured silicon substrate, and diffusing a nitrogen source into the base surface passivation layer to form an N-type base doping layer, and finally obtaining a sample 1;

[0166] Step 2: Preparation of the first transparent electrode layer:

[0167] Sample 1 is placed in a vacuum chamber of a high vacuum magnetron sputtering machine, an indium tin oxide (ITO) target is set, and a first transparent electrode layer with a thickness of 100 nm is prepared on the surface of the P-type base doping layer in sample 1 by magnetron sputtering to obtain sample 2; wherein the power of the high vacuum magnetron sputtering machine is 60 W, and the operating time is 1.5 h;

[0168] Step 3: Preparation of the first metal electrode layer:

[0169] Sample 2 was placed on a mask plate, and a first metal electrode layer with a thickness of 200 nm was prepared by evaporation to obtain sample 3. The vacuum degree of the evaporation method was 2×10 -4 Pa, temperature is 800°C, evaporation rate is 2.5Å / S;

[0170] Step 4: Preparation of tunneling layer:

[0171] Sample 3 was placed on a mask plate and then placed in a vacuum chamber of a high vacuum magnetron sputtering machine, and a tunneling layer with a thickness of 40 nm was prepared on the surface of the N-type base doping layer of the sample 3 by magnetron sputtering to obtain sample 4; the power of the magnetron sputtering equipment was 60 W, and the operation time was 1 hour;

[0172] Step 5: Preparation of hole transport layer:

[0173] Sample 4 was cleaned with an ultraviolet ozone cleaner (UV-Ozone) for 15 minutes, and the hole transport layer dispersion was evenly coated on the surface of the tunnel layer of the sample 4 after ultrasonic treatment for 20 minutes, and a hole transport layer with a thickness of 20 nm was prepared by spin coating. After the spin coating was completed, annealing was performed to obtain sample 5; the spin coating speed of the spin coating method was 2000 rpm, the spin coating time was 40 s, the spin coating solution amount was 100 ul, the annealing temperature was 450°C, and the annealing time was 30 min;

[0174] Step 6: Preparation of perovskite layer:

[0175] Lead iodide and cesium bromide are co-evaporated to prepare a lead iodide / cesium bromide mixed film with a thickness of 440 nm on the surface of the hole transport layer in sample 5, the evaporation rate of lead iodide is 8 A / s, the evaporation rate of cesium bromide is 0.8 A / s, the evaporation rate ratio of lead iodide to cesium bromide in the co-evaporation method is 10:1, the total evaporation time of the co-evaporation method is 1000 s, and the mass ratio of formamidine iodide to formamidine bromide is 10:1;

[0176] Co-evaporating formamidine iodide and formamidine bromide on the lead iodide / cesium bromide mixed film again by the second step co-evaporation method to obtain an ammonium salt film with a thickness of 400 nm. After the two-step co-evaporation, the two layers of the film are heated to 150° C. for 30 minutes to form sample 6 with a perovskite layer. The evaporation rate of the formamidine iodide is 4.7 A / s, and the evaporation rate of the formamidine bromide is 1 A / s. The evaporation rate ratio of formamidine iodide to formamidine bromide in the co-evaporation method is 10:1, and the total evaporation time of the co-evaporation method is 700 s.

[0177] Step 7: Preparation of passivation layer:

[0178] Sample 6 was placed on a mask, and 3 mg of propylene diamine iodide was evaporated onto the surface of the perovskite layer of the sample 6 by evaporation to obtain a passivation layer with a thickness of 4 nm. After the evaporation was completed, annealing was performed to obtain sample 7. The evaporation vacuum degree was 2×10 -4 Pa, evaporation temperature is 80℃, evaporation rate is 0.1Å / S, annealing temperature is 100℃, and annealing time is 8min;

[0179] Step 8: Preparation of electron transport layer:

[0180] The electron transport layer material was evaporated onto the surface of the passivation layer of the sample 7 to obtain the sample 8 coated with an electron transport layer with a thickness of 20 nm; the vacuum degree of the evaporation was 1×10 -4 Pa, the evaporation temperature is 200 °C, and the evaporation rate is 0.1 Å / S;

[0181] Step 9: Preparation of buffer layer:

[0182] The buffer layer material was deposited onto the surface of the electron transport layer of sample eight by atomic accumulation deposition using an atomic accumulation deposition device to obtain sample nine with a buffer layer having a thickness of 15 nm. The deposition vacuum degree was 0.5×10 4 Pa, the deposition pipeline temperature is between 70°C and the deposition chamber temperature is 60°C;

[0183] Step 10: Preparation of the second transparent electrode layer:

[0184] The transparent electrode material is sputtered onto the surface of the buffer layer of sample nine by using a magnetron sputtering method, and an indium zinc oxide (IZO) target is set to obtain sample ten with a second transparent electrode layer having a thickness of 100 nm. The power of the magnetron sputtering method is 50 W, and the operation time is 1 hour.

[0185] Step 11: Preparation of the second metal electrode layer:

[0186] Sample 10 was placed on a mask plate, and a second metal electrode layer with a thickness of 100 nm was prepared by evaporation to obtain sample 11. The vacuum degree of the evaporation was 2×10 -4 Pa, temperature is 800°C, evaporation rate is 0.1Å / S;

[0187] Step 12: Preparation of anti-reflection layer:

[0188] Sample 11 was placed on a mask plate, and the second metal electrode layer of the sample 11 was evaporated by evaporation to obtain an anti-reflection layer with a thickness of 100 nm. After the evaporation was completed, an annealing operation was performed to obtain a stacked solar cell. The evaporation vacuum degree was 2×10 -4 Pa, the evaporation temperature is 80℃, the evaporation rate is 2Å / S, the annealing temperature is 100℃, and the annealing time is 8min.

[0189] The test conditions of the stacked solar cell in the present invention are: using a solar simulator, a standard solar intensity calibration is performed, and an area of ​​1.0 cm 2 The device of the embodiment is subjected to long-term IV test, with the starting voltage set to 1.95V, the cut-off voltage set to 0V, the range set to 100mA, and the result is rounded to two decimal places. The test results are shown in the following table:

[0190] Photoelectric conversion efficiency (%) Open circuit voltage (V) <![CDATA[Short-circuit current density (mA / cm 2 ).]]> Decay rate (% / year) Example 1 30.6 1.94 21.3 0.8 Example 2 31.5 1.98 21.5 0.6 Example 3 30.3 1.94 21.2 0.6 Comparative Example 1 26.9 1.81 18.2 7.4

[0191] like Figure 1 The perovskite layer preparation process diagram of the laminated solar cell described in the present embodiment 1-3, the first step of the lead iodide / cesium bromide mixed film processed by the process of the present invention, because the second step ammonium salt particles have higher energy, they can be embedded in the lead iodide film, with a larger reaction surface area. The ammonium salt film can also react better with the lead iodide / cesium bromide mixed film inside and at the bottom. The perovskite film prepared by the process of the present invention has no lead iodide residue inside, and the film quality is high.

[0192] like Figure 2The perovskite layer preparation process diagram of the stacked solar cell described in Comparative Example 1 is based on the perovskite film prepared by the traditional method, because the first step film and the second ammonium salt film react incompletely. The ammonium salt film is difficult to react with the bottom of the film prepared in the first step, and a large amount of lead iodide remains inside and at the bottom of the formed perovskite film, and the film quality is low.

[0193] The laminated solar cell prepared by the method for preparing the perovskite layer of the present invention has high photoelectric conversion efficiency and low attenuation rate.

Claims

1. A method for preparing a perovskite layer, characterized in that: The following steps are involved: Step 1, preparing a lead iodide / cesium bromide mixed film on a substrate material by co-evaporation of lead iodide and cesium bromide; Step 2, placing the lead iodide / cesium bromide mixed film in a vacuum chamber of a high vacuum magnetron sputtering machine, grinding formamidine iodide (FAI) and formamidine bromide (FABr) into powder to prepare a target material, and using a high vacuum magnetron sputtering machine to sputter the target material on the surface of the lead iodide / cesium bromide mixed film to obtain an ammonium salt film; Step 3: After the ammonium salt film is sputtered, the lead iodide / cesium bromide mixed film is heated to obtain a perovskite layer.

2. The preparation method according to claim 1, characterized in that: The vacuum degree of the high vacuum magnetron sputtering machine in step 2 is 5×10 -5 -2×10 -4 Pa, the power of the high vacuum magnetron sputtering machine is 30-200W.

3. The preparation method according to claim 2, characterized in that: The evaporation rate ratio of lead iodide to cesium bromide in the co-evaporation method in step 1 is (2:1)-(10:1).

4. The preparation method according to claim 2, characterized in that: The evaporation rate of lead iodide in the co-evaporation method in step 1 is 1-10 A / s, and the evaporation rate of cesium bromide in the co-evaporation method is 0.1-10 A / s.

5. The preparation method according to claim 2, characterized in that: The total evaporation time of the co-evaporation method in step 1 is 1-10000s.

6. The preparation method according to claim 2, characterized in that: The mass ratio of formamidine iodide to formamidine bromide in step 2 is (1:10)-(10:1).

7. The preparation method according to claim 2, characterized in that: The thickness of the lead iodide / cesium bromide mixed film in step 1 is 200-800nm.

8. The preparation method according to claim 2, characterized in that: The thickness of the ammonium salt film in step 2 is 100-800 nm.

9. The preparation method according to claim 2, characterized in that: The heating temperature in step 3 is 80-200° C., and the heating time is 1-60 min.

10. A stacked solar cell, characterized in that: The stacked solar cell is prepared by the preparation method of the perovskite layer according to any one of claims 1 to 9, and the stacked solar cell comprises, from bottom to top, a first metal electrode layer, a first transparent electrode layer, a P-type base doping layer, a base passivation layer, a suede crystalline silicon substrate, a base surface passivation layer, an N-type base doping layer, a tunneling layer, a hole transport layer, a perovskite layer, a passivation layer, an electron transport layer, a buffer layer, a second transparent electrode layer, a second metal electrode layer and an anti-reflection layer.

11. The method for preparing laminated solar energy according to claim 10, characterized in that: The invention comprises the following steps: providing a textured crystalline silicon substrate, preparing the base passivation layer on the back of the textured crystalline silicon substrate, preparing the P-type base doping layer on the surface of the base passivation layer, preparing the first transparent electrode layer on the surface of the P-type base doping layer, preparing the first metal electrode layer on the surface of the first transparent electrode layer, preparing the base surface passivation layer on the surface of the textured crystalline silicon substrate, preparing the N-type base doping layer on the surface of the base surface passivation layer, preparing the tunneling layer on the surface of the N-type base doping layer, preparing the hole transport layer on the surface of the tunneling layer, preparing the perovskite layer on the surface of the hole transport layer, preparing the passivation layer on the surface of the perovskite layer, preparing the electron transport layer on the surface of the passivation layer, preparing the buffer layer on the surface of the electron transport layer, preparing the second transparent electrode layer on the surface of the buffer layer, preparing the second metal electrode layer on the surface of the second transparent electrode layer, and preparing an anti-reflection layer on the surface of the second metal electrode layer.