Modified perovskite thin film, perovskite composite film, preparation methods of modified perovskite thin film and perovskite composite film, and perovskite solar cell
By introducing the compound of formula I into perovskite solar cells, the problems of stability and repeatability of perovskite solar cells are solved, efficient preparation of perovskite films and improved device performance, and I0 defects in the prior art are solved The resulting performance degradation and cost problems.
Patent Information
- Application Number
- CN202410961305.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-17
AI Technical Summary
Perovskite solar cells face stability and repeatability challenges in the pursuit of high efficiency, especially performance degradation and insufficient life due to I0 defects. The existing reducing agent and redox agent strategies have a single function, high cost and efficiency. Reduced problem.
Introducing compounds of formula I, such as 3-amino-phthalidylhydrazide and derivatives thereof, inhibit the generation of defects in perovskite films by selective redox and reduction of I0 defects, and regulate the Fermi energy level to reduce charge accumulation, forming Modified perovskite film or composite film to improve device stability and efficiency.
It significantly improves the stability and photoelectric conversion efficiency of perovskite solar cells, extends the service life of the device, and reduces costs, achieving higher quality perovskite film preparation.
Smart Images

Figure BDA0004950599430000031 
Figure BDA0004950599430000032 
Figure BDA0004950599430000061
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of solar cells, and in particular to a modified perovskite film, a perovskite composite film, a preparation method thereof and a perovskite solar cell. Background Art
[0002] In the frontier exploration of optoelectronic technology, metal halide perovskite solar cells (PSCs) have become a shining star in the field of photovoltaic technology with their excellent performance and potential. In the past decade, PSCs have made significant breakthroughs in technology, and their efficiency-certified power conversion efficiency (PCE) has climbed to 26.7%, which is gradually approaching and approaching the peak level of industrial crystalline silicon and Cu(In,Ga)Se2 photovoltaic technology. However, just like the shadow behind the shining stars, PSCs, while pursuing high efficiency, also face severe challenges such as the stability and repeatability of perovskite-based electronic materials and devices.
[0003] However, despite the great progress made in efficiency of PSCs, the stability and repeatability of perovskite-based electronic materials and devices are still important issues that restrict their application. These challenges mainly stem from the oxidation of iodine and the reduction of lead under non-equilibrium conditions (such as light, heat, and electric fields), which not only affect their performance and lifespan, but also limit the in-depth understanding of their intrinsic properties and the exploration of their practical application potential. On the road of scientific research and production, the lack of repeatability makes each experiment and manufacturing full of unknowns and variables, which undoubtedly increases the complexity and uncertainty of R&D and production.
[0004] In particular, the perovskite light-absorbing layer has relatively weak intrinsic stability due to its ionic compound characteristics. At the interface with other semiconductor materials, ion migration (such as the migration of iodine and lead) becomes an insurmountable gap, which not only weakens the performance of PSCs, but also makes it difficult for its working life to meet the stringent standards of commercial applications (usually requiring a 25-year operating life to meet the IEC 61215 stability standard).
[0005] To this end, researchers have been exploring and proposing a variety of solutions. Among them, reducing agents and redox couples have become the two major strategies. Reducing agents such as benzylhydrazine hydrochloride (BHC), phenylhydrazine-4-sulfonic acid (PHPA), 3-hydrazinebenzoic acid (3-HBA), etc. can stabilize the precursor and inhibit the oxidation of iodine ions; while redox couples such as Eu 3+ / Eu 2+ (Science 2019, 363, 265-270.) and ferrocene (Fc, Angew. Chem. Int. Ed. 2021, 60, 25567-25574.), etc., can repair Pb 0 and I 0Defects and achieve self-regeneration.
[0006] However, these solutions are not perfect. For the reducing agent strategy, since the reducing agent has a relatively single function and is a consumable, it will become ineffective after a period of aging, and it is difficult to continuously restore defects during the long-term aging process. The design and development of reducing agents are often limited by existing chemical knowledge and technical conditions, which makes it difficult to integrate multiple functions on a single molecule. The reducing agents used in the prior art are often only used to repair specific chemical reactions or defects and lack versatility. This is mainly because the design of reducing agents is often based on specific redox reactions, which makes them unable to cope with complex reaction systems or multiple defects. When the reducing agent participates in the redox reaction, its own chemical structure will change, resulting in reduced or lost activity. In addition, environmental factors such as temperature and humidity may also accelerate the aging process of the reducing agent. The reducing agent will gradually be consumed during the reaction, and its effectiveness and performance will decrease with the increase of usage time, and eventually lose its effect. Although the redox pair strategy can inhibit the oxidation of iodide ions, it is relatively single in function. The existing redox pair strategy, first of all, Eu metal is a rare metal element, and its limited mining volume leads to its high price. In addition, the high purity requirement for Eu metal also increases its production cost, so the cost of using Eu is high. Secondly, the redox kinetics of Pb and I do not match, and the defect formation energy and migration energy of I are lower, resulting in a mismatch in the defect concentration change of I ions during the reaction, which in turn induces the formation of I defects, making these defects more likely to diffuse and accumulate in the material. These defects will reduce the performance and stability of the device. Thirdly, under actual working conditions, hole accumulation may occur at the upper interface of perovskite solar cells. Hole accumulation will lead to uneven charge distribution at the upper interface, which will in turn cause changes in the local electric field. These changes will promote the migration of I ions and I 0 The formation of defects will affect the performance and stability of the device.
[0007] Therefore, the development of multifunctional additives has become a hot topic of common concern in current scientific research and industry. This is not only the key to improving the stability and reproducibility of PSCs, but also an important driving force for its continuous advancement on the road to commercialization. Summary of the invention
[0008] In order to overcome the defects of the prior art, the purpose of the present invention is to provide a modified perovskite film, a perovskite composite film, a preparation method thereof and a solar cell. The modified perovskite film / perovskite composite film can improve the problems of poor repeatability and many defects of the perovskite film in the prior art, and is used to improve the efficiency and stability of the device.
[0009] The first aspect of the present invention provides a modified perovskite film, which comprises a perovskite material and a compound of formula I:
[0010]
[0011] Wherein, in the compound of formula I, R is selected from -H, -OCH3, -CH3, -F, -Cl, -COOH, -CF3, -SO2CF3.
[0012] A second aspect of the present invention provides a perovskite composite film, the perovskite composite film comprising a perovskite film formed of a perovskite material and a functional layer disposed on the perovskite film, wherein the functional layer comprises a compound of formula I:
[0013]
[0014] Wherein, in the compound of formula I, R is selected from -H, -OCH3, -CH3, -F, -Cl, -COOH, -CF3, -SO2CF3.
[0015] According to the modified perovskite film of the first aspect or the perovskite composite film of the second aspect, wherein the perovskite material has a general formula of ABX3, wherein A is one or more monovalent cations of an amine group, an amidine group, a guanidine group, a cesium group, and a rubidium group; B is Pb 2+ Sn 2+ One or more of; X is Cl - Br - ,I - 、SCN - 、CH3COO - One or more of; preferably, the molar fraction of lead ions in B is not less than 80%;
[0016] More preferably, in the modified perovskite film or perovskite composite film, the molar ratio of the perovskite material to the compound of formula I is 100:(0.1-1).
[0017] According to the modified perovskite film of the first aspect or the perovskite composite film of the second aspect, the compound of formula I is selected from one or more of 3-amino-phthalhydrazide, 4-aminophthalhydrazide, 3-amino-4-carboxylphthalhydrazide, 3-amino-4-fluorophthalhydrazide, and 3-amino-4-trifluoromethanesulfonic acid phthalhydrazide.
[0018] The third aspect of the present invention provides a method for preparing the modified perovskite film of the first aspect, comprising:
[0019] (1) preparing a perovskite precursor solution, and adding a compound of formula I to the perovskite precursor solution;
[0020] Preferably, in the perovskite precursor solution, the concentration of the compound of formula I is 0.01 to 3 mg / mL;
[0021] (2) depositing a perovskite precursor solution to form a wet film, and extracting the wet film using an anti-solvent to form a modified perovskite film.
[0022] The fourth aspect of the present invention provides a method for preparing the perovskite composite film of the second aspect, the method comprising:
[0023] (1) preparing a perovskite precursor solution;
[0024] (2) depositing a perovskite precursor solution to form a wet film, and extracting the wet film using an anti-solvent to which a compound of formula I is added to form the perovskite composite film;
[0025] Preferably, the concentration of the compound of formula I in the anti-solvent is 0.1-20 mg / mL.
[0026] The fifth aspect of the present invention provides a method for preparing the perovskite composite film of the second aspect, the method comprising:
[0027] (1) preparing a perovskite precursor solution;
[0028] (2) depositing a perovskite precursor solution to form a wet film, extracting the wet film using an anti-solvent, and drying to obtain a perovskite film;
[0029] (3) preparing a functional layer on the surface of the perovskite film obtained in step (2) using a surface modification solution containing the compound of formula I to form the perovskite composite film;
[0030] Preferably, in the surface modification solution, the concentration of the compound of formula I is 0.1 to 20 mg / mL; and / or
[0031] Preferably, the solvent of the surface modification solution is selected from one or more of methyl ether, isopropanol, m-xylene, toluene, 1,3,5-trimethylbenzene butanol, 1,2-dichlorobenzene, ethyl acrylate, chloroform, ethyl acetate, butyl acrylate, ethyl ether, chlorobenzene, and toluene;
[0032] More preferably, the doping method is immersion and / or deposition;
[0033] Further preferably, the immersing includes immersing the perovskite film in the surface modification solution for a immersion time of 5 to 600 seconds.
[0034] According to the method of the third to fifth aspects, in step (2), the anti-solvent is selected from one or more of anisole, isopropanol, m-xylene, toluene, 1,3,5-trimethylol, 1,2-dichlorobenzene, ethyl acrylate, chloroform, ethyl acetate, butyl acrylate, ether, chlorobenzene, and toluene;
[0035] Preferably, the extraction method is soaking and / or sedimentation;
[0036] More preferably, the soaking comprises soaking the wet film in an anti-solvent for a soaking time of 5 to 600 seconds; and / or
[0037] More preferably, the depositing comprises depositing an anti-solvent on the wet film surface.
[0038] A sixth aspect of the present invention provides a perovskite solar cell, wherein the perovskite layer of the perovskite solar cell comprises the modified perovskite film of the first aspect or the modified perovskite film prepared according to the method of the third aspect.
[0039] A seventh aspect of the present invention provides a perovskite solar cell, wherein the perovskite layer of the perovskite solar cell comprises the perovskite composite film of the second aspect or the perovskite composite film prepared according to the method of the fifth or sixth aspect;
[0040] Wherein, the functional layer of the perovskite composite film is arranged on one side of the hole transport layer of the perovskite solar cell.
[0041] The perovskite solar cell according to the sixth aspect or the seventh aspect comprises a conductive glass electrode layer, a first charge transport layer, a perovskite layer, a second charge transport layer, and a counter electrode layer; wherein when the first charge transport layer is an electron transport layer, the second charge transport layer is a hole transport layer; when the first charge transport layer is a hole transport layer, the second charge transport layer is an electron transport layer;
[0042] Preferably, the electron transport layer material is an N-type semiconductor, preferably selected from C 60 , BCP, PC 61 BM, PC 71 One or more of BM, TiO2, ZnO, SnO2, ZnTiO3, more preferably, the thickness of the electron transport layer is 5 to 120 nm;
[0043] Preferably, the hole transport layer material is a P-type semiconductor, preferably selected from one or more of nickel oxide, Spiro-OMeTAD, poly-TPD, copper phthalocyanine, nickel phthalocyanine, poly(triarylamine), poly(3-hexylthiophene), more preferably, the hole transport layer has a thickness of 50 to 150 nm; and / or;
[0044] Preferably, the material of the counter electrode layer is selected from one or more of gold, silver, copper and ITO, and the thickness of the counter electron layer is 60 to 300 nm.
[0045] The modified perovskite film / perovskite composite film of the present invention has but is not limited to the following beneficial effects:
[0046] The present invention introduces the compound of formula I into the perovskite, and utilizes the hydrazine group in its structure to selectively reduce I 0 , reducing the possibility of ion migration, thereby preventing performance degradation caused by ion migration. At the same time, it will participate in the nucleation and crystallization regulation of perovskite, and the O atoms with lone pairs of electrons contained in it can coordinate with Pb atoms, thereby delaying the crystallization process of the perovskite material to a certain extent, which helps to obtain high-quality perovskite films. The present invention also further regulates the Fermi level of the film through the design of substituents, reduces the charge accumulation on the heterogeneous interface, further improves the efficiency and working stability of the device, and shows great potential in improving the optoelectronic performance and stability of the device. DETAILED DESCRIPTION
[0047] The present invention is further described in detail below through examples. Through these examples, the features and advantages of the present invention will become clearer and more specific.
[0048] The word “exemplary” is used exclusively herein to mean “serving as an example, example, or illustration.” Any embodiment described herein as “exemplary” is not necessarily to be construed as preferred or advantageous over other embodiments.
[0049] In addition, the technical features involved in different embodiments of the present application described below can be combined with each other as long as they do not conflict with each other.
[0050] The present invention provides a modified perovskite film, which comprises a perovskite material and a compound of formula I:
[0051]
[0052] Wherein, in the compound of formula I, R is selected from -H, -OCH3, -CH3, -F, -Cl, -COOH, -CF3, -SO2CF3.
[0053] The present invention also provides a perovskite composite film, the perovskite composite film comprising a perovskite film formed of a perovskite material and a functional layer disposed on the perovskite film, wherein the functional layer comprises a compound of formula I:
[0054]
[0055] Wherein, in the compound of formula I, R is selected from -H, -OCH3, -CH3, -F, -Cl, -COOH, -CF3, -SO2CF3.
[0056] In the compound of formula I, -NH2 and R are substituents at any position on the benzene ring, wherein when R is -H, the compound of formula I is luminol or isoluminol.
[0057] The core purpose of the present invention is to solve the problem of the perovskite solar cell being 0 The stability problems caused by defects are solved, and the long-term reliability of the device is improved through innovative strategies. The present invention can achieve the following effects by modifying the perovskite film in the solar cell:
[0058] 1. Solve the I in the work process 0 Defect stability issues
[0059] During the operation of perovskite solar cells, I 0 The generation of defects is often a key factor leading to device performance degradation and insufficient stability. To this end, the present invention proposes using a compound containing a hydrazine group to selectively oxidize and reduce these defects to improve the stability and working efficiency of the device.
[0060] 2. Functional group design to suppress defects in thin films
[0061] In addition to repairing defects that have already occurred, the present invention can also introduce specific functional groups to suppress the generation of defects in perovskite films. These functional groups can form stable chemical bonds with key elements in perovskite materials, thereby preventing the generation of new defects during preparation and use. This strategy not only helps to improve the initial performance of the device, but also further extend its service life. When an electron-donating group is introduced, the electron-donating group will shift the Fermi level of the perovskite downward, making it more inclined to the P type, thereby better matching the energy level structure of the hole transport layer; when an electron-withdrawing group is introduced, the electron-withdrawing group will shift the Fermi level of the perovskite downward, making it more inclined to the N type, thereby better matching the energy level structure of the electron transport layer.
[0062] 3. Regulate the Fermi level of perovskite films to reduce charge accumulation at heterojunction interfaces
[0063] The Fermi level of perovskite film has an important influence on its performance. The present invention achieves precise regulation of the Fermi level of perovskite film by introducing substituents with different electron-pulling and electron-donating capabilities. This regulation can optimize the carrier dynamics of the device and reduce the charge accumulation at the heterogeneous interface, thereby further improving the performance and stability of the device.
[0064] In one embodiment, the perovskite material has a general formula of ABX3, wherein A is one or more monovalent cations of amine, amidine, guanidine, cesium, and rubidium; B is Pb 2+ Sn 2+ One or more of; X is Cl - Br - ,I - 、SCN - 、CH3COO -One or more of; preferably, the molar fraction of lead ions in B is not less than 80%;
[0065] More preferably, in the modified perovskite film or perovskite composite film, the molar ratio of the perovskite material to the compound of formula I is 100:(0.1-1).
[0066] The present invention uses a compound of formula I to modify the perovskite film, and the compound of formula I includes luminol, isoluminol, and derivatives thereof. When R is -H, the compound of formula I is luminol or isoluminol, and the hydrazine group in the structure is used to selectively reduce I 0 , reducing the possibility of ion migration, thereby preventing the performance degradation caused by ion migration. At the same time, it will participate in the nucleation and crystallization regulation of perovskite, and the O atoms with lone pairs of electrons contained can coordinate with Pb atoms, thereby delaying the crystallization process of perovskite materials to a certain extent, and helping to obtain high-quality perovskite films. The present invention can also further regulate the Fermi level of the film by the design of substituents, such as R can be selected from -OCH3, -CH3, -F, -Cl, (electron donating group, high Fermi level direction) and -COOH, -CF3, -SO2CF3 (electron withdrawing group, low Fermi level direction), reducing the charge accumulation on the heterogeneous interface, and further improving the efficiency and working stability of the device.
[0067] Luminol, isoluminol, and their derivatives are as follows:
[0068] Luminol (3-amino-phthaloyl hydrazide):
[0069]
[0070] Isoluminol (4-aminophthalhydrazide):
[0071]
[0072] R1 in the luminol derivative refers to -NH2, and R2 refers to one of -OCH3, -CH3, -F, -Cl (electron donating group, high Fermi level direction) and -COOH, -CF3, -SO2CF3 (electron withdrawing group, low Fermi level direction):
[0073]
[0074] R3 in the isoluminol derivative refers to -NH2, and R4 refers to one of -OCH3, -CH3, -F, -Cl (electron donating group, high Fermi level direction) and -COOH, -CF3, -SO2CF3 (electron withdrawing group, low Fermi level direction):
[0075]
[0076] In one embodiment, the compound of formula I is selected from one or more of 3-amino-phthalic acid hydrazide, 4-aminophthalic acid hydrazide, 3-amino-4-carboxyphthalic acid hydrazide, 3-amino-4-fluorophthalic acid hydrazide, and 3-amino-4-trifluoromethanesulfonic acid phthalic acid hydrazide.
[0077] The present invention also provides a method for preparing the modified perovskite film, comprising:
[0078] (1) preparing a perovskite precursor solution, and adding a compound of formula I to the perovskite precursor solution;
[0079] Preferably, in the perovskite precursor solution, the concentration of the compound of formula I is 0.01 to 3 mg / mL;
[0080] (2) depositing a perovskite precursor solution to form a wet film, and extracting the wet film using an anti-solvent to form a modified perovskite film.
[0081] Specifically, the precursor solution containing the compound of formula I is deposited on a substrate to form a perovskite layer containing the compound of formula I, so that the compound of formula I is directly doped in the perovskite and coated on the grain boundary surface.
[0082] The present invention also provides a method for preparing the perovskite composite film, comprising:
[0083] (1) preparing a perovskite precursor solution;
[0084] (2) depositing a perovskite precursor solution to form a wet film, and extracting the wet film using an anti-solvent to which a compound of formula I is added to form the perovskite composite film;
[0085] Preferably, the concentration of the compound of formula I in the anti-solvent is 0.1-20 mg / mL.
[0086] Specifically, a perovskite precursor solution is deposited on a substrate to form a wet film; and an anti-solvent containing a compound of formula I is used to extract the wet film to form a perovskite layer including the compound of formula I, thereby using the anti-solvent to introduce the compound of formula I into the perovskite and coat the grain boundaries and the surface of the perovskite layer.
[0087] The present invention also provides a method for preparing the perovskite composite film, comprising:
[0088] (1) preparing a perovskite precursor solution;
[0089] (2) depositing a perovskite precursor solution to form a wet film, extracting the wet film using an anti-solvent, and drying to obtain a perovskite film;
[0090] (3) preparing a functional layer on the surface of the perovskite film obtained in step (2) using a surface modification solution containing the compound of formula I to form the perovskite composite film;
[0091] Preferably, in the surface modification solution, the concentration of the compound of formula I is 0.1 to 20 mg / mL; and / or
[0092] Preferably, the solvent of the surface modification solution is selected from one or more of methyl ether, isopropanol, m-xylene, toluene, 1,3,5-trimethylbenzene butanol, 1,2-dichlorobenzene, ethyl acrylate, chloroform, ethyl acetate, ethanol, butyl acrylate, ethyl ether, chlorobenzene, and toluene;
[0093] More preferably, the doping method is immersion and / or deposition;
[0094] Further preferably, the immersing includes immersing the perovskite film in the surface modification solution for a immersion time of 5 to 600 seconds.
[0095] Specifically, a perovskite precursor solution is first deposited on a substrate, and after it is dried to form a film, the dry film is doped with the surface modification solution to form a perovskite layer coated with the compound of formula I.
[0096] The present invention relates to a method for preparing a high-stability modified perovskite film / perovskite composite film, comprising directly doping a compound of formula I into perovskite and coating the compound on the grain boundary surface, forming a surface modification solution prepared from the compound of formula I and coating the compound on the perovskite layer surface, or introducing an anti-solvent containing the compound of formula I into perovskite and coating the compound on the grain boundary and the perovskite layer surface.
[0097] The present invention utilizes an anti-solvent to extract the perovskite wet film, and through this method, double passivation of the perovskite surface and grain boundary by luminol and its derivatives is achieved in one step.
[0098] In a specific embodiment, in step (1), the perovskite precursor solution is prepared by the following method: PbI2, FAI (formamidine hydroiodide) and CsI are dissolved in a solvent to obtain a perovskite precursor solution, and the solvent is a mixed liquid of NMP (N-methylpyrrolidone) and DMF (N,N-dimethylformamide) in a volume ratio of 1:5.
[0099] In a specific embodiment, in step (2), the anti-solvent is selected from one or more of anisole, isopropanol, m-xylene, toluene, 1,3,5-trimethylol, 1,2-dichlorobenzene, ethyl acrylate, chloroform, ethyl acetate, ethanol, butyl acrylate, ether, chlorobenzene, and toluene;
[0100] Preferably, the extraction method is soaking and / or sedimentation;
[0101] More preferably, the soaking comprises soaking the wet film in an anti-solvent for a soaking time of 5 to 600 seconds; and / or
[0102] More preferably, the depositing comprises depositing an anti-solvent on the wet film surface.
[0103] The present invention also provides a perovskite solar cell, wherein the perovskite layer of the perovskite solar cell comprises the aforementioned modified perovskite film / perovskite composite film or the modified perovskite film / perovskite composite film prepared according to the aforementioned method;
[0104] Wherein, the functional layer of the perovskite composite film is arranged on one side of the hole transport layer of the perovskite solar cell.
[0105] In one embodiment, the perovskite solar cell comprises a conductive glass electrode layer, a first charge transport layer, a perovskite layer, a second charge transport layer, and a counter electrode layer; wherein, when the first charge transport layer is an electron transport layer, the second charge transport layer is a hole transport layer; when the first charge transport layer is a hole transport layer, the second charge transport layer is an electron transport layer;
[0106] Preferably, the electron transport layer material is an N-type semiconductor, preferably selected from C 60 , BCP, PC 61 BM, PC 71 One or more of BM, TiO2, ZnO, SnO2, ZnTiO3, more preferably, the thickness of the electron transport layer is 5 to 120 nm;
[0107] Preferably, the hole transport layer material is a P-type semiconductor, preferably selected from one or more of nickel oxide, Spiro-OMeTAD, poly-TPD, copper phthalocyanine, nickel phthalocyanine, poly(triarylamine), poly(3-hexylthiophene), more preferably, the hole transport layer has a thickness of 50 to 150 nm; and / or;
[0108] Preferably, the material of the counter electrode layer is selected from one or more of gold, silver, copper and ITO, and the thickness of the counter electron layer is 60 to 120 nm.
[0109] The modified perovskite film / perovskite composite film of the present invention can be used for an upright structure or an inverted structure solar cell. When the structure of the perovskite solar cell is an upright structure, it comprises a conductive glass electrode layer, an electron transport layer, a perovskite layer, a hole transport layer and a counter electrode from bottom to top; when the structure of the perovskite solar cell is an inverted structure, it comprises a conductive glass electrode layer, a hole transport layer, a perovskite layer, an electron transport layer and a counter electrode from bottom to top.
[0110] The present invention has no special restrictions on the sources of all raw materials. Unless otherwise specified, they are all conventional products that can be obtained commercially.
[0111] Example 1
[0112] This example is used to illustrate the modification of perovskite film by doping luminol with a precursor.
[0113] This embodiment provides a method for preparing a perovskite solar cell with an upright structure, comprising:
[0114] Step S1, preparing an electron transport layer: on a clean cathode (FTO glass), a titanium oxide layer is prepared by a spray pyrolysis method, the spraying temperature is 500°C, the number of spraying circles is 12 circles, annealing at 500°C for 45 minutes, and after natural cooling, a KCl aqueous solution is spin-coated at a speed of 3000 rpm, and annealing at 100°C for 10 minutes, so that a TiO2 electron transport layer with a film thickness of 30 nm is obtained on the FTO glass;
[0115] Step S2, including step S2-1 to step S2-2;
[0116] Step S2-1, preparing a perovskite precursor solution containing luminol: dissolving PbI2, FAI and CsI in a molar ratio of 1:0.95:0.05 in a solvent (a mixed liquid of NMP and DMF in a volume ratio of 1:5), adding 0.2 mg / mL of luminol, and shaking and mixing to obtain a precursor solution with a concentration of 1.5 mol / L;
[0117] Step S2-2, preparing a luminol material-doped perovskite layer: spin coating the precursor solution on the electron transport layer obtained in step S1, the spin coating condition is 6000 rpm, the spin coating time is 30 s, and chlorobenzene solution is added dropwise as an anti-solvent for extraction at the 25th second, annealing at 100° C. for 60 min, and cooling naturally to obtain a perovskite layer;
[0118] Step S3, including step S3-1 to step S3-2;
[0119] Step S3-1, preparing a chlorobenzene dispersion of Spiro-OMeTAD: weighing 72 mg of Spiro-OMeTAD, adding it to 1 mL of chlorobenzene, then adding 17.5 μL of Li-TFSI / ACN (520 mg / mL) and 28.8 μL of tBP, and ultrasonically dispersing for 10 minutes to prepare a chlorobenzene dispersion of Spiro-OMeTAD;
[0120] Step S3-2, preparing a hole transport layer: spin-coating the chlorobenzene dispersion of Spiro-OMeTAD on the perovskite layer by a solution method at a spin coating speed of 3500 rpm, and drying naturally to obtain a hole transport layer with a film thickness of 130 nm;
[0121] Step S4, preparing the anode: evaporating metallic silver on the hole transport layer to obtain an anode with a film thickness of 100 nm.
[0122] The upright perovskite solar cell provided in this embodiment is denoted as C-1.
[0123] Example 2
[0124] This example is used to illustrate the modification of perovskite film by doping luminol with an antisolvent.
[0125] The method of this embodiment differs from the method of embodiment 1 only in that:
[0126] Step S2, including step S2-1 to step S2-2;
[0127] Step S2-1, preparing a perovskite precursor solution: dissolving PbI2, FAI and CsI in a molar ratio of 1:0.95:0.05 in a solvent (a mixed liquid of NMP and DMF in a volume ratio of 1:5), shaking and mixing to obtain a precursor solution with a concentration of 1.5 mol / L;
[0128] Step S2-2, preparing a perovskite layer doped with an anti-solvent containing luminol: spin-coating 50 μL of the precursor solution on the electron transport layer obtained in step S1, the spin-coating condition is 6000 rpm, the spin-coating time is 30 s, and at the 25th second, 80 μL of chlorobenzene solution containing 0.5 mg / mL luminol is added as an anti-solvent for extraction, annealing at 100°C for 60 min, and naturally cooling to obtain a perovskite layer.
[0129] The upright perovskite solar cell provided in this embodiment is denoted as C-2.
[0130] Example 3
[0131] This example is used to illustrate the modification of perovskite film by interfacial modification luminol.
[0132] The method of this embodiment differs from the method of embodiment 1 only in that:
[0133] Step S2, including steps S2-1 to S2-3;
[0134] Step S2-1, preparing a perovskite precursor solution: dissolving PbI2, FAI and CsI in a molar ratio of 1:0.95:0.05 in a solvent (a mixed liquid of NMP and DMF in a volume ratio of 1:5), shaking and mixing to obtain a precursor solution with a concentration of 1.5 mol / L.
[0135] Step S2-2, preparing an unmodified perovskite layer: spin coating 50 μL of the perovskite precursor solution on the electron transport layer obtained in step S1, the spin coating condition is 6000 rpm, the spin coating time is 35 s, and chlorobenzene solution is added dropwise as an anti-solvent for extraction at the 28th second, annealing at 100° C. for 45 min, and naturally cooling to obtain a dry film (unmodified perovskite layer);
[0136] Step S2-3, preparing a luminol-modified perovskite layer: spin-coating 20 μL of a 0.3 mg / mL luminol isopropanol surface modification solution on the unmodified perovskite layer obtained in step S2-2, at a spin coating condition of 4000 rpm for 30 s, and cooling naturally to obtain a modified perovskite layer;
[0137] The upright perovskite solar cell provided in this embodiment is denoted as C-3.
[0138] Example 4
[0139] This example is used to illustrate the modification of the perovskite film by doping the precursor with a luminol derivative-electron withdrawing group (3-amino-4-trifluoromethanesulfonic acid phthaloyl hydrazide).
[0140] The method of this embodiment differs from the method of embodiment 1 only in that:
[0141] Step S2, including step S2-1 to step S2-2;
[0142] Step S2-1, preparing a perovskite precursor solution containing a luminol derivative: dissolving PbI2, FAI and CsI in a molar ratio of 1:0.95:0.05 in a solvent (a mixed liquid of NMP and DMF in a volume ratio of 1:5), adding 0.2 mg / mL of 3-amino-4-trifluoromethanesulfonic acid phthaloyl hydrazide, shaking and mixing, and obtaining a precursor solution with a concentration of 1.5 mol / L;
[0143] Step S2-2, preparing a luminol derivative-doped perovskite layer: spin-coating the precursor solution on the electron transport layer obtained in step S1, the spin-coating condition is 6000 rpm, the spin-coating time is 30 s, and chlorobenzene solution is added as an anti-solvent for extraction at 25 s, annealing at 100° C. for 60 min, and naturally cooling to obtain a perovskite layer.
[0144] The upright perovskite solar cell provided in this embodiment is denoted as C-4.
[0145] Example 5
[0146] This example is used to illustrate the modification of the perovskite film by doping the precursor with an isoluminol derivative-electron withdrawing group (5-amino-4-trifluoromethanesulfonic acid phthaloyl hydrazide).
[0147] The method of this embodiment differs from the method of embodiment 1 only in that:
[0148] Step S2, including step S2-1 to step S2-2;
[0149] Step S2-1, preparing a perovskite precursor solution containing a luminol derivative: dissolving PbI2, FAI and CsI in a molar ratio of 1:0.95:0.05 in a solvent (a mixed liquid of NMP and DMF in a volume ratio of 1:5), adding 0.2 mg / mL of 5-amino-4-trifluoromethanesulfonic acid phthaloyl hydrazide, shaking and mixing, and obtaining a precursor solution with a concentration of 1.5 mol / L;
[0150] Step S2-2, preparing an isoluminol derivative-doped perovskite layer: spin-coating the precursor solution on the electron transport layer obtained in step S1, the spin-coating condition is 6000 rpm, the spin-coating time is 30 s, and chlorobenzene solution is added dropwise as an anti-solvent for extraction at 25 s, annealing at 100° C. for 60 min, and naturally cooling to obtain a perovskite layer.
[0151] The upright perovskite solar cell provided in this embodiment is denoted as C-5.
[0152] Example 6
[0153] This example is used to illustrate the modification of the perovskite film by doping the precursor with a luminol derivative-electron donating group (3-amino-4-methylphthalhydrazide).
[0154] The method of this embodiment differs from the method of embodiment 1 only in that:
[0155] Step S2, including step S2-1 to step S2-2;
[0156] Step S2-1, preparing a perovskite precursor solution containing a luminol derivative: dissolving PbI2, FAI and CsI in a molar ratio of 1:0.95:0.05 in a solvent (a mixed liquid of NMP and DMF in a volume ratio of 1:5), adding 0.2 mg / mL of 3-amino-4-methylphthalic acid hydrazide, and shaking and mixing to obtain a precursor solution with a concentration of 1.5 mol / L;
[0157] Step S2-2, preparing a luminol derivative-doped perovskite layer: spin-coating the precursor solution on the electron transport layer obtained in step S1, the spin-coating condition is 6000 rpm, the spin-coating time is 30 s, and chlorobenzene solution is added as an anti-solvent for extraction at 25 s, annealing at 100° C. for 60 min, and naturally cooling to obtain a perovskite layer.
[0158] The upright perovskite solar cell provided in this embodiment is denoted as C-6.
[0159] Example 7
[0160] This example is used to illustrate the modification of perovskite film by doping isoluminol with a precursor.
[0161] The method of this embodiment differs from the method of embodiment 1 only in that:
[0162] Step S2, including step S2-1 to step S2-2;
[0163] Step S2-1, preparing a perovskite precursor solution containing isoluminol: dissolving PbI2, FAI and CsI in a molar ratio of 1:0.95:0.05 in a solvent (a mixed liquid of NMP and DMF in a volume ratio of 1:5), adding 0.2 mg / mL of isoluminol, and shaking and mixing to obtain a precursor solution with a concentration of 1.5 mol / L;
[0164] Step S2-2, preparing an isoluminol-doped perovskite layer: spin-coating the precursor solution on the electron transport layer obtained in step S1, the spin-coating condition is 6000 rpm, the spin-coating time is 30 s, and chlorobenzene solution is added dropwise as an anti-solvent for extraction at 25 s, annealing at 100° C. for 60 min, and naturally cooling to obtain a perovskite layer.
[0165] The upright perovskite solar cell provided in this embodiment is denoted as C-7.
[0166] Example 8
[0167] This example is used to illustrate the modification of perovskite film by doping the precursor with luminol derivative-electron withdrawing group (3-amino-4-carboxyphthalhydrazide).
[0168] The method of this embodiment differs from the method of embodiment 1 only in that:
[0169] Step S2, including step S2-1 to step S2-2;
[0170] Step S2-1, preparing a perovskite precursor solution containing a luminol derivative: dissolving PbI2, FAI and CsI in a molar ratio of 1:0.95:0.05 in a solvent (a mixed liquid of NMP and DMF in a volume ratio of 1:5), adding 0.2 mg / mL of 3-amino-4-carboxyphthalhydrazide, and shaking and mixing to obtain a precursor solution with a concentration of 1.5 mol / L;
[0171] Step S2-2, preparing a luminol derivative-doped perovskite layer: spin-coating the precursor solution on the electron transport layer obtained in step S1, the spin-coating condition is 6000 rpm, the spin-coating time is 30 s, and chlorobenzene solution is added as an anti-solvent for extraction at 25 s, annealing at 100° C. for 60 min, and naturally cooling to obtain a perovskite layer.
[0172] The upright perovskite solar cell provided in this embodiment is denoted as C-8.
[0173] Example 9
[0174] This example is used to illustrate the modification of the perovskite film by doping the precursor with a luminol derivative-electron donating group (3-amino-4-fluorophthalic acid hydrazide).
[0175] The method of this embodiment differs from the method of embodiment 1 only in that:
[0176] Step S2, including step S2-1 to step S2-2;
[0177] Step S2-1, preparing a perovskite precursor solution containing a luminol derivative: dissolving PbI2, FAI and CsI in a molar ratio of 1:0.95:0.05 in a solvent (a mixed liquid of NMP and DMF in a volume ratio of 1:5), adding 0.2 mg / mL of 3-amino-4-fluorophthalic acid hydrazide, and shaking and mixing to obtain a precursor solution with a concentration of 1.5 mol / L;
[0178] Step S2-2, preparing a luminol derivative-doped perovskite layer: spin-coating the precursor solution on the electron transport layer obtained in step S1, the spin-coating condition is 6000 rpm, the spin-coating time is 30 s, and chlorobenzene solution is added as an anti-solvent for extraction at 25 s, annealing at 100° C. for 60 min, and naturally cooling to obtain a perovskite layer.
[0179] The upright perovskite solar cell provided in this embodiment is denoted as C-9.
[0180] Comparative Example 1
[0181] This comparative example is used to illustrate a method for preparing a solar cell without modifying the perovskite film.
[0182] The difference between this comparative example method and the method of Example 1 is that:
[0183] Step S2, including step S2-1 to step S2-2;
[0184] Step S2-1, preparing a perovskite precursor solution: dissolving PbI2, FAI and CsI in a molar ratio of 1:0.95:0.05 in a solvent (a mixed liquid of NMP and DMF in a volume ratio of 1:5), shaking and mixing to obtain a precursor solution with a concentration of 1.5 mol / L.
[0185] Step S2-2, preparing an unmodified perovskite layer: spin coating the perovskite solution on the electron transport layer obtained in step S1, the spin coating condition is 6000 rpm, the spin coating time is 35 s, and chlorobenzene solution is added as an anti-solvent for extraction at 28 s, annealing at 100 ° C for 45 min, and naturally cooling to obtain a dry film (unmodified perovskite layer).
[0186] The upright perovskite solar cell provided in this comparative example is denoted as C-10.
[0187] The electrochemical properties of the perovskite solar cells prepared in the above embodiments and comparative examples were tested, and the results are shown in Table 1.
[0188] Table 1
[0189]
[0190]
[0191]
[0192] * The aging condition for the photoelectric conversion efficiency retention rate of the device after 1000h aging is 65℃ nitrogen atmosphere.
[0193] It can be seen from the data in Table 1 that compared with the device in Comparative Example 1 (i.e., no luminol material is added to the perovskite layer), the present invention significantly improves the photoelectric conversion efficiency and thermal stability of the device by introducing the luminol material into the perovskite layer. The modified perovskite films of Examples 1-9 all show beneficial stability, and the photoelectric conversion efficiency retention rate after 1000h aging is significantly improved compared with the unmodified Comparative Example 1. Further comparison of Example 1 (introducing luminol material using a precursor solution), Example 2 (introducing luminol material using an anti-solvent) and Example 3 (introducing luminol material through a surface modification solution) shows that the perovskite solar cell prepared by introducing the luminol material by means of a precursor solution exhibits more superior photoelectric performance, which is because the method of introducing the precursor solution can ensure the uniform distribution and high efficiency of the compound of Formula I in the perovskite layer. In addition, after comparing Example 1 with Examples 4 to 9, it can be observed that in the upright device structure, the luminol derivatives designed with electron-withdrawing functional groups (Examples 4, 5 and 8) show more optimized performance in terms of photoelectric performance and stability compared to the designs with electron-donating groups (Examples 6 and 9).
[0194] The present application has been described above in conjunction with preferred embodiments, but these embodiments are only exemplary and serve only as an illustration. On this basis, various replacements and improvements may be made to the present application, all of which fall within the scope of protection of the present application.
Claims
1. A modified perovskite film comprising a perovskite material and a compound of formula I: in, In the compound of formula I, R is selected from -H, -OCH3, -CH3, -F, -Cl, -COOH, -CF3, -SO2CF3.
2. A perovskite composite film, characterized in that: The perovskite composite film comprises a perovskite film formed of a perovskite material and a functional layer disposed on the perovskite film, wherein the functional layer comprises a compound of formula I: Wherein, in the compound of formula I, R is selected from -H, -OCH3, -CH3, -F, -Cl, -COOH, -CF3, -SO2CF3.
3. The modified perovskite film according to claim 1 or the perovskite composite film according to claim 2, characterized in that: The perovskite material has a general formula of ABX3, wherein A is one or more monovalent cations of amine, amidine, guanidine, cesium, and rubidium; B is Pb 2+ Sn 2+ One or more of; X is Cl - Br - ,I - 、SCN - 、CH3COO - One or more of; preferably, the molar fraction of lead ions in B is not less than 80%; More preferably, in the modified perovskite film or perovskite composite film, the molar ratio of the perovskite material to the compound of formula I is 100:(0.1-1).
4. The modified perovskite film according to claim 1 or the perovskite composite film according to claim 2, characterized in that: The compound of formula I is selected from one or more of 3-amino-phthalic acid hydrazide, 4-aminophthalic acid hydrazide, 3-amino-4-carboxyphthalic acid hydrazide, 3-amino-4-fluorophthalic acid hydrazide and 3-amino-4-trifluoromethanesulfonic acid phthalic acid hydrazide.
5. The method for preparing the modified perovskite film according to claim 1, 3 or 4, characterized in that: The method comprises: (1) preparing a perovskite precursor solution, and adding a compound of formula I to the perovskite precursor solution; Preferably, in the perovskite precursor solution, the concentration of the compound of formula I is 0.01 to 3 mg / mL; (2) depositing a perovskite precursor solution to form a wet film, and extracting the wet film using an anti-solvent to form a modified perovskite film.
6. The method for preparing a perovskite composite film according to any one of claims 2 to 4, characterized in that: The method comprises: (1) preparing a perovskite precursor solution; (2) depositing a perovskite precursor solution to form a wet film, and extracting the wet film using an anti-solvent to which a compound of formula I is added to form the perovskite composite film; Preferably, the concentration of the compound of formula I in the anti-solvent is 0.1-20 mg / mL.
7. The method for preparing a perovskite composite film according to any one of claims 2 to 4, characterized in that: The method comprises: (1) preparing a perovskite precursor solution; (2) depositing a perovskite precursor solution to form a wet film, extracting the wet film using an anti-solvent, and drying to obtain a perovskite film; (3) preparing a functional layer on the surface of the perovskite film obtained in step (2) using a surface modification solution containing the compound of formula I to form the perovskite composite film; Preferably, in the surface modification solution, the concentration of the compound of formula I is 0.1 to 20 mg / mL; and / or Preferably, the solvent of the surface modification solution is selected from one or more of methyl ether, isopropanol, m-xylene, toluene, 1,3,5-trimethylbenzene butanol, 1,2-dichlorobenzene, ethyl acrylate, chloroform, ethyl acetate, butyl acrylate, ethyl ether, chlorobenzene, and toluene; More preferably, the doping method is immersion and / or deposition; Further preferably, the immersing includes immersing the perovskite film in the surface modification solution for a immersion time of 5 to 600 seconds.
8. The method according to any one of claims 4 to 7, characterized in that In step (2), the anti-solvent is selected from one or more of anisole, isopropanol, m-xylene, toluene, 1,3,5-trimethylol, 1,2-dichlorobenzene, ethyl acrylate, chloroform, ethyl acetate, butyl acrylate, ether, chlorobenzene, and toluene; Preferably, the extraction method is soaking and / or sedimentation; More preferably, the soaking comprises soaking the wet film in an anti-solvent for a soaking time of 5 to 600 seconds; and / or More preferably, the depositing comprises depositing an anti-solvent on the wet film surface.
9. A perovskite solar cell, characterized in that: The perovskite layer of the perovskite solar cell comprises the modified perovskite film according to claim 1, 3 or 4 or the modified perovskite film prepared according to the method of claim 4 or 8.
10. A perovskite solar cell, characterized in that: The perovskite layer of the perovskite solar cell comprises the perovskite composite film according to any one of claims 2 to 4 or the perovskite composite film prepared according to the method according to any one of claims 5 to 8; Wherein, the functional layer of the perovskite composite film is arranged on one side of the hole transport layer of the perovskite solar cell.
11. The perovskite solar cell according to claim 9 or 10, characterized in that: The perovskite solar cell comprises a conductive glass electrode layer, a first charge transport layer, a perovskite layer, a second charge transport layer, and a counter electrode layer; wherein, when the first charge transport layer is an electron transport layer, the second charge transport layer is a hole transport layer; when the first charge transport layer is a hole transport layer, the second charge transport layer is an electron transport layer; Preferably, the electron transport layer material is an N-type semiconductor, preferably selected from C 60 , BCP, PC 61 BM, PC 71 One or more of BM, TiO2, ZnO, SnO2, ZnTiO3, more preferably, the thickness of the electron transport layer is 5 to 120 nm; Preferably, the hole transport layer material is a P-type semiconductor, preferably selected from one or more of nickel oxide, Spiro-OMeTAD, poly-TPD, copper phthalocyanine, nickel phthalocyanine, poly(triarylamine), poly(3-hexylthiophene), more preferably, the hole transport layer has a thickness of 50 to 150 nm; and / or; Preferably, the material of the counter electrode layer is selected from one or more of gold, silver, copper and ITO, and the thickness of the counter electron layer is 60 to 300 nm.
Citation Information
Patent Citations
Preparation method of perovskite thin film and preparation method of perovskite solar cell
CN114220923A
Perovskite solar cell doped with hydrazide passivator and preparation method thereof
CN115050891A
Multifunctional additive modified inverted perovskite solar cell
CN115697010A
Four-mode emission carbon nanodot / perovskite composite material and preparation method and application thereof
CN115926780A
Preparation method of tin-based perovskite solar cell
CN116322082A