MnZn-based ferrite
By adjusting the content of the main and secondary components of MnZn-based ferrites and the sintering process, MnZn-based ferrites with low core loss over a wide temperature range were prepared, solving the problem of difficult core loss reduction in existing technologies and achieving high efficiency and miniaturization of transformers.
Patent Information
- Application Number
- CN202380029249.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-23
- Filing Date
- 2023-03-16
- Publication Date
- 2024-11-08
AI Technical Summary
The core loss of existing MnZn ferrites is difficult to further reduce over a wide temperature range, which affects the miniaturization and efficiency of transformers.
By adjusting the contents of the main components Fe2O3, ZnO, and MnO in MnZn-based ferrites, and controlling the contents of the secondary components CaO, SiO2, Nb2O5, ZrO2, Co3O4, and SnO2 within a specific range, the sintering process was optimized to prepare MnZn-based ferrites.
Significantly reduce core losses over a wide temperature range of 25℃ to 120℃ while maintaining high saturation flux density, achieving high efficiency and miniaturization of the transformer.
Smart Images

Figure BDA0005052793370000081 
Figure BDA0005052793370000082
Abstract
Description
Technical Field
[0001] The present invention relates to a MnZn ferrite used as a transformer material for a switching power supply, and more particularly to a MnZn ferrite with a small temperature dependence of magnetic core loss. Background Art
[0002] MnZn ferrites have the characteristics of low core loss and high saturation flux density, so they are widely used as transformer materials for switching power supplies. 2 O 3 , ZnO and Mn are the main components, and CaO, SiO 2 and Nb 2 O 5 Such MnZn ferrites are required to have high saturation magnetic flux density, and also require low core loss in a wide temperature range in consideration of the operating environment of power supplies, and various MnZn ferrites with low temperature dependence of core loss have been proposed.
[0003] As a conventional MnZn ferrite, for example, Patent Document 1 discloses a MnZn ferrite containing Fe 2 O 3 The main components are 53.2 to 54.5 mol% of iron oxide in terms of ZnO, 7.5 to 11.5 mol% of zinc oxide in terms of ZnO, and the balance of manganese oxide (MnO). 3 O 4 Calculated as 2000-4500ppm of cobalt oxide, SiO 2 60-140 ppm of silicon oxide, 300-700 ppm of calcium oxide, and 300-700 ppm of NbO2. 2 O 5 This is calculated as 100 to 350 ppm of niobium oxide. Thus, a MnZn-based ferrite having reduced core loss in a wide temperature range can be obtained.
[0004] In addition, Patent Document 2 discloses a MnZn-based ferrite containing Fe 2 O 3 , ZnO, and MnO as main components, and SiO is contained relative to 100 parts by mass of the total amount of the main components calculated as the oxides. 2 Conversion of greater than 0.001 mass parts and less than or equal to 0.015 mass parts of Si, CaCO 3 The amount of Ca, Co, and 3 O 40.4 parts by mass (excluding 0) of Co, Ta 2 O 5 0.1 parts by mass (including 0) or less of Ta, ZrO 2 Converted to less than or equal to 0.1 mass part (including 0) of Zr, Nb 2 O 5 0.05 parts by mass or less (including 0) of Nb is converted into a minor component. Prior art literature Patent Literature
[0005] Patent document: Japanese Patent Application Publication No. 2002-231520 Patent document: International Publication No. 2017 / 164350 Summary of the invention -Problems to be solved by the invention-
[0006] The MnZn ferrite described in Patent Documents 1 and 2 can relatively reduce the core loss by setting the content of each component of the MnZn ferrite within a specified range. However, in order to make the transformer smaller and more efficient, it is necessary to further reduce the core loss within a wide temperature range. To this end, it is necessary to set the content of each component of the MnZn ferrite that contributes to reducing the core loss within a more appropriate range.
[0007] The present invention has been made in view of the above-mentioned problems, and an object of the present invention is to provide a MnZn-based ferrite capable of reducing core loss in a wide temperature range of 25°C to 120°C. -Solutions to solve the problem-
[0008] In order to achieve the above-mentioned object, in the present invention, the content of each component of the MnZn-based ferrite is set within the prescribed range shown below.
[0009] Specifically, the MnZn ferrite of the present invention is characterized in that the MnZn ferrite contains 50 mol% to 53 mol% of Fe in terms of oxide. 2 O 3 , 8 mol% to 10 mol% ZnO, and 37 mol% to 42 mol% MnO as main components, and contains 100 ppm to 300 ppm CaO and 120 ppm or less SiO in terms of oxides. 2 , 100ppm~500ppm Nb 2 O 5 , 0ppm~200ppm ZrO 2 , 2000ppm~4000ppm Co 3 O 4, and 0ppm~1500ppm SnO 2 As a secondary ingredient.
[0010] According to the MnZn ferrite of the present invention, the core loss can be reduced by setting the contents of the components of the MnZn ferrite within the above-mentioned specified range. In particular, the MnZn ferrite of the present invention contains 50 mol% to 53 mol% of Fe in terms of oxide. 2 O 3 , 8mol% to 10mol% ZnO, and 37mol% to 42mol% MnO as main components, so that a high saturation magnetic flux density can be obtained and the effect of reducing the magnetic core loss can be obtained. Furthermore, in the MnZn-based ferrite of the present invention, the CaO, SiO 2 , Nb 2 O 5 、ZrO 2 、Co 3 O 4 and SnO 2 As a secondary component, it is possible to reduce the core loss in a wide temperature range. 2 If the content of CaO exceeds the above range, abnormal grain growth of crystals is likely to occur during sintering, which may increase the core loss. If the content of CaO does not meet the above range, high-resistance grain boundaries cannot be fully formed, which may increase the core loss. 3 O 4 and Nb 2 O 5 If the above range is not met, the effect of reducing core loss may be reduced. 3 O 4 and Nb 2 O 5 If the above range is exceeded, the core loss may increase. 2 and SnO 2 If the temperature exceeds the above range, the core loss may increase. In combination with these characteristics, the MnZn ferrite according to the present invention can reduce the core loss in a wide temperature range of 25°C to 120°C.
[0011] In addition, the MnZn-based ferrite of the present invention preferably contains 150 ppm to 250 ppm of CaO and 50 ppm to 150 ppm of ZrO in terms of oxide. 2 , 2000ppm~3000ppm Co 3 O 4 , and 500ppm~1000ppm SnO 2As the auxiliary component.
[0012] By setting the content of the auxiliary component of the MnZn-based ferrite within a more appropriate range as described above, the core loss can be effectively reduced in a wide temperature range. -Effects of the Invention-
[0013] According to the MnZn-based ferrite of the present invention, the core loss can be reduced in a wide temperature range of 25°C to 120°C. DETAILED DESCRIPTION
[0014] The following description of the preferred embodiments is merely illustrative in nature and is not intended to limit the present invention, the methods of application of the present invention, or the uses of the present invention.
[0015] First, a MnZn-based ferrite according to an embodiment of the present invention will be described.
[0016] The MnZn-based ferrite according to the present embodiment contains 50 mol% to 53 mol% of Fe in terms of oxide. 2 O 3 , 8mol% to 10mol% ZnO, and 37mol% to 42mol% MnO as the main components. 2 O 3 , ZnO and MnO exceed the above content range, the core loss may increase.
[0017] Furthermore, the MnZn-based ferrite according to the present embodiment contains 100 ppm to 300 ppm of CaO and 120 ppm or less of SiO in terms of oxide. 2 , 100ppm~500ppm Nb 2 O 5 , 0ppm~200ppm ZrO 2 , 2000ppm~4000ppm Co 3 O 4 , and 0ppm~1500ppm SnO 2 As a secondary ingredient.
[0018] In the above-mentioned auxiliary component content range, if CaO is less than 100ppm, the core loss may increase, and if CaO exceeds 300ppm, abnormal grain growth of crystals is likely to occur during sintering, resulting in an increase in core loss. The CaO content is preferably 185ppm to 280ppm, and the CaO content is more preferably 220ppm to 280ppm.
[0019] Within the above-mentioned range of the content of the secondary components, if SiO 2If the content exceeds 120 ppm, abnormal grain growth of the crystals is likely to occur during firing, resulting in an increase in core loss. 2 The content is more preferably 117 ppm or less.
[0020] Within the above-mentioned range of the content of the secondary components, if Nb 2 O 5 If Nb is less than 100ppm, the effect of reducing core loss may be reduced. 2 O 5 If the content exceeds 500 ppm, abnormal grain growth of the crystals is likely to occur during firing, which may increase the core loss. 2 O 5 The content of is preferably 300ppm to 400ppm.
[0021] Within the above-mentioned range of the content of the secondary components, if Co 3 O 4 If the Co 3 O 4 If the concentration exceeds 4000ppm, the core loss may increase. 3 O 4 The content of is preferably 2650ppm to 3100ppm.
[0022] Within the above-mentioned range of the content of the secondary components, if SnO 2 and ZrO 2 If the content exceeds the above range, the core loss may increase. 2 The content of ZrO is preferably 0ppm to 1000ppm. 2 The content of is preferably 0 ppm to 110 ppm.
[0023] Furthermore, in this embodiment, it is preferable that 150 ppm to 250 ppm of CaO and 50 ppm to 150 ppm of ZrO are contained in terms of oxides. 2 , 2000ppm~3000ppm Co 3 O 4 , and 500ppm~1000ppm SnO 2 As the above-mentioned auxiliary component. Thus, a MnZn-based ferrite capable of more effectively reducing the core loss in a wide temperature range of 25°C to 120°C can be obtained. More preferably, the content of CaO is 185ppm to 215ppm, and the content of ZrO is 100ppm to 210ppm. 2 The content of Co is 90ppm~110ppm, 3 O 4 The content of SnO is 2650ppm~2750ppm,2 The content is 900ppm~1000ppm.
[0024] In addition, in this embodiment, preferably, as the auxiliary component, Nb 2 O 5 Ratio of Nb to CaO 2 O 5 / CaO) is 1.0 to 2.5. 2 O 5 By setting the ratio to CaO within the above range, the temperature dependency of the core loss can be reduced.
[0025] In addition, in this embodiment, preferably, TiO is substantially not contained. 2 、V 2 O 5 、MoO 3 、Bi 2 O 3 As a secondary ingredient.
[0026] Next, a preferred method for producing the MnZn-based ferrite according to one embodiment of the present invention will be described.
[0027] First, the raw materials of each main component (Fe 2 O 3 , ZnO, MnO) powders are wet mixed, pre-sintered and pulverized at a predetermined temperature in the range of 800°C to 900°C. Then, a predetermined amount of the raw materials of the auxiliary components (CaO, SiO 2 , Nb 2 O 5 、ZrO 2 、Co 3 O 4 SnO 2 ) to obtain a mixed powder.
[0028] The mixed powder composed of the main component and the auxiliary component obtained as above is first granulated into particles in order to be formed into a desired shape. For this purpose, a small amount of polyvinyl alcohol as a suitable binder is added to the mixed powder, and the mixed powder is spray-dried.
[0029] The obtained particles are formed into a desired shape, and the formed body is used for a sintering process. The sintering process is divided into a heating process, a maintaining process and a cooling process. In particular, in the maintaining process, the maintaining temperature is 1200°C to 1300°C, and is maintained for 2 hours to 5 hours. At this time, the atmospheric oxygen concentration is adjusted to between 1% and 5%, and the equilibrium oxygen partial pressure (equilibrium oxygen partial pressure) formula is used for adjustment in the cooling process. As described above, MnZn-based ferrite formed into a desired shape can be prepared. [Example]
[0030] Hereinafter, examples and comparative examples to which the present invention is applied will be described. The examples are examples of the present invention and are not intended to limit the scope of the present invention.
[0031] (Sample production) First, samples of MnZn ferrite of Examples 1 and 2 and Comparative Examples 1 to 4 were prepared by the following method. Specifically, for each sample of Example and Comparative Example, the raw material of the main component (Fe 2 O 3 , MnO, ZnO) to achieve the composition shown in Table 1, and then wet mixing. The slurry obtained by wet mixing is dried, pre-sintered at 800°C to 900°C, and then pulverized. Then, appropriate amounts of CaO, NbO, and other auxiliary components are added and mixed into the pre-sintered powder obtained. 2 O 5 、Co 3 O 4 、ZrO 2 SnO 2 、TaO 2 The mixture is mixed to obtain the composition shown in Table 1, and then finely ground with a binder and spray-dried. The obtained particles are formed into a predetermined shape and then calcined.
[0032] The above-mentioned sintering process is divided into a heating process, a maintaining process and a cooling process. In the heating process, the temperature is raised to 600°C to 800°C in the atmosphere, and the temperature is raised from the subsequent temperature to the maintaining temperature in a reducing atmosphere. At this time, the heating rate is 150°C / h to 250°C / h. The temperature of the maintaining process is 1200°C to 1300°C, and it is maintained for 2 hours to 5 hours. At this time, the atmospheric oxygen concentration is adjusted to between 1% and 5%. In the cooling process, cooling is carried out at a cooling rate of 60°C / h to 100°C / h, and the atmospheric oxygen concentration is adjusted using the balanced oxygen partial pressure formula. Through the above sintering process, a sample with an outer diameter of 25mm, an inner diameter of 17mm, and a height of 11mm is obtained.
[0033] Next, the core loss, saturation magnetic flux density, and magnetic permeability of each of the obtained samples were evaluated in the following manner.
[0034] (Temperature dependence of core loss) The core loss was evaluated in the following manner: using an SY-8217 analyzer from IWATSU ELECTRIC CO., LTD., the primary and secondary windings were each wound three times on the samples of each embodiment and comparative example obtained, and the evaluation was performed at a frequency of 100 kHz, a maximum magnetic flux density of 200 mT, and a temperature range of 25°C to 140°C.
[0035] (Saturation flux density) The saturation magnetic flux density was evaluated in the following manner: using an SY-8217 analyzer produced by IWATSU ELECTRIC CO., LTD., the primary and secondary windings were respectively wound 18 times on the samples of each embodiment and comparative example, and the evaluation was performed under the conditions of 1 kHz 1194 A / m, 25°C, and 100°C.
[0036] (Magnetic Permeability) The magnetic permeability was evaluated as follows: using an E4990A analyzer from Keysight Technologies, a winding was wound 10 times on the obtained samples of each embodiment and comparative example, and the evaluation was performed under the conditions of 1 kHz, 1 V, and room temperature.
[0037] Table 2 shows the evaluation results of the core loss, saturation magnetic flux density, and magnetic permeability of each sample.
[0038] [Table 1]
[0039] [Table 2]
[0040] As shown in Table 2, it is shown that the MnZn ferrite of the examples satisfying the composition range of the present invention has higher magnetic permeability, particularly high saturation magnetic flux density and small core loss in the temperature range of 25°C to 120°C, compared with the MnZn ferrite of the comparative example not satisfying the composition range of the present invention. Therefore, by using the MnZn ferrite of each example, it is possible to obtain a MnZn ferrite capable of reducing the core loss in the temperature range of 25°C to 120°C.
[0041] As can be seen from the above, the Fe content is 50 mol% to 53 mol% in terms of oxide. 2 O 3 , 8 mol% to 10 mol% ZnO, and 37 mol% to 42 mol% MnO as main components, and contains 100 ppm to 300 ppm CaO and 120 ppm or less SiO in terms of oxides. 2 , 100ppm~500ppm Nb 2 O 5 , 0ppm~200ppm ZrO 2 , 2000ppm~4000ppm Co 3 O 4 , and 0ppm~1500ppm SnO 2The MnZn-based ferrite of the present invention as a minor component can reduce core loss in a wide temperature range of 25° C. to 120° C., and is very useful.
Claims
1. A MnZn ferrite, characterized in that: The MnZn-based ferrite contains 50 mol% to 53 mol% of Fe2O3, 8 mol% to 10 mol% of ZnO, and 37 mol% to 42 mol% of MnO as main components in terms of oxide. The MnZn-based ferrite contains 100ppm to 300ppm of CaO, 120ppm or less of SiO2, 100ppm to 500ppm of Nb2O5, 0ppm to 200ppm of ZrO2, 2000ppm to 4000ppm of Co3O4, and 0ppm to 1500ppm of SnO2 as auxiliary components in terms of oxides.
2. The MnZn ferrite according to claim 1, characterized in that: The MnZn-based ferrite contains, as the auxiliary components, 150 ppm to 250 ppm of CaO, 50 ppm to 150 ppm of ZrO 2 , 2000 ppm to 3000 ppm of Co 3 O 4 , and 500 ppm to 1000 ppm of SnO 2 in terms of oxides.
Citation Information
Patent Citations
Soft magnetic ferrite material and preparation process thereof
CN102194561A
High temperature and low loss MnZn ferrite core and preparation method thereof
CN102219486A
Soft magnetic ferrite material low in magnetic core loss
CN102924071A
High-frequency wide-temperature low-loss manganese-zinc ferrite and manufacturing technique thereof
CN103396111A
Low-loss manganese zinc ferrite material for temperature of 40 DEG C below zero to 160 DEG C and manufacturing method thereof