Fiber-reinforced resin molding material and molded article
By using long-term and short-term fiber structure and thermoset resin adhesion technology in fiber reinforced thermoplastic resin molding materials, the problem of taking into account both the flowability and mechanical properties of fiber reinforced thermoplastic resin molding materials in small, thin-walled and complex moldings is achieved. Excellent molding performance and dimensional accuracy.
Patent Information
- Application Number
- CN202380029399.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-06-30
- Filing Date
- 2023-06-20
- Publication Date
- 2024-11-08
AI Technical Summary
Existing fiber-reinforced thermoplastic resin molding materials are difficult to take into account excellent fluidity, mechanical properties and dimensional accuracy in small, thin-walled and complex molding products. Long fibers lead to poor fluidity, while short fibers lead to reduced mechanical properties and dimensional accuracy.
A fiber reinforced resin molding material containing 1 to 30 parts by weight of reinforcing fibers and 70 to 99 parts by weight of thermoplastic resins is used. The reinforcing fibers contain unidirectional fibers with a length of 3 to 15 mm and bundled fibers with a length of 0.5 to 2.9 mm. The length direction is consistent, and the resin component is adhered to the surface of the bundled fibers, and a thermosetting resin is used to improve the bundled property.
It realizes excellent fluidity, mechanical properties and dimensional accuracy in small, thin-walled and complex molded products. It is suitable for a variety of molding methods, such as injection molding, stamping molding, etc., and is suitable for automotive parts, semiconductor parts and medical devices. field.
Smart Images

Figure CN118922480A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a molding material comprising reinforcing fibers and a thermoplastic resin, and a molded product comprising reinforcing fibers and a thermoplastic resin. Background Art
[0002] As molding materials using continuous reinforcing fibers and thermoplastic resins as a matrix, various forms such as thermoplastic prepregs, yarns, and glass mats (GMT) are known. Such molding materials are easy to mold due to the characteristics of thermoplastic resins, do not require storage loads like thermosetting resins, and have the characteristics of high toughness of the resulting molded products. In particular, molding materials processed into granules are suitable for molding methods with excellent economy and productivity such as injection molding or stamping molding, and are useful as industrial materials.
[0003] Patent Document 1 discloses that a molding material composed of reinforcing fibers and a thermoplastic resin and an injection molded product are crushed, and the obtained molding material combined with a fiber-reinforced thermoplastic resin molding material is injection molded to obtain a molded product having excellent mechanical properties and fluidity. In addition, Patent Documents 2 and 3 disclose that two types of reinforcing fibers, one having a long fiber length and one having a short fiber length, are combined with a thermoplastic resin and injection molded to obtain a molded product having excellent mechanical properties and appearance quality.
[0004] [Prior art literature]
[0005] [Patent Document]
[0006] [Patent Document 1] Japanese Patent Application Publication No. 2006-181776
[0007] [Patent Document 2] Japanese Patent Application Publication No. 2012-116917
[0008] [Patent Document 3] Japanese Patent Application Laid-Open No. 4-175108 Summary of the invention
[0009] [Problems to be solved by the invention]
[0010] However, in recent years, with the miniaturization, thin-walling and complexity of molded products, molding materials are required to have higher precision moldability, and a high degree of balance is required to take into account the excellent fluidity, mechanical properties and dimensional accuracy of small, thin-walled and complex molded products. In the past, thermoplastic resin molding materials containing reinforcing fibers had the problem of poor fluidity due to the length of the reinforcing fibers. On the other hand, when the length of the reinforcing fibers is short, although the fluidity is excellent, the reinforcing fibers will be damaged during injection molding, so there is a problem of reduced mechanical properties and dimensional accuracy of the molded products, which are difficult to take into account. Therefore, in the use of small, thin-walled and complex molded products, long reinforcing fibers with excellent mechanical properties and excellent fluidity must be included.
[0011] Therefore, in view of the above problems and needs, an object of the present invention is to provide a fiber-reinforced resin molding material and a fiber-reinforced resin molded product that can achieve excellent fluidity, mechanical properties, and dimensional accuracy.
[0012] [Methods to solve the problem]
[0013] In order to solve the above-mentioned problems, the present invention has the following configurations.
[0014] [1] A fiber-reinforced resin molding material comprising reinforcing fibers (A) and a thermoplastic resin (B),
[0015] The fiber-reinforced resin molding material comprises 1 to 30 parts by weight of reinforcing fiber (A) and 70 to 99 parts by weight of thermoplastic resin (B) based on 100 parts by weight of the total of (A) and (B).
[0016] The reinforcing fibers (A) include reinforcing fibers (A-1) and bundled reinforcing fibers (A-2).
[0017] The length of the reinforcing fiber (A-1) is 3 to 15 mm, and the reinforcing fiber (A-1) is aligned with the longitudinal direction of the molding material, and the length of the reinforcing fiber (A-1) is the same as the length of the longitudinal direction of the molding material.
[0018] The bundled reinforcing fibers (A-2) are composed of 10 or more single fibers each having a length of 0.5 to 2.9 mm.
[0019] [2] The fiber-reinforced resin molding material as described in [1],
[0020] The fiber-reinforced resin molding material comprises a fiber-reinforced resin molding material (X) and a fiber-reinforced resin molding material (Y),
[0021] The fiber-reinforced resin molding material (X) comprises reinforcing fibers (A-1) and a thermoplastic resin (B-1).
[0022] The longitudinal directions of the reinforcing fibers (A-1) and the fiber-reinforced resin molding material (X) are aligned.
[0023] The fiber-reinforced resin molding material (Y) contains bundled reinforcing fibers (A-2) and a thermoplastic resin (B-2).
[0024] [3] The fiber-reinforced resin molding material according to [1] or [2],
[0025] The fiber-reinforced resin molding material has a core-sheath structure.
[0026] The core structure of the core-sheath structure comprises reinforcing fibers (A-1), and the reinforcing fibers (A-1) are oriented in the same direction as the length direction of the molding material.
[0027] The sheath structure of the core-sheath structure is a fiber-reinforced resin composition (C) comprising bundled reinforcing fibers (A-2) and a thermoplastic resin (B),
[0028] The sheath structure covers the core structure.
[0029] [4] The fiber-reinforced resin molding material according to any one of [1] to [3], wherein the reinforcing fibers (A-1) and the bundled reinforcing fibers (A-2) are both carbon fibers.
[0030] [5] The fiber-reinforced resin molding material according to any one of [1] to [4], wherein the content of the reinforcing fibers (A-1) and the bundled reinforcing fibers (A-2) is:
[0031] The reinforcing fibers (A-1) are contained in an amount of 50 to 99 parts by weight, and the bundled reinforcing fibers (A-2) are contained in an amount of 1 to 50 parts by weight.
[0032] [6] The fiber-reinforced resin molding material according to any one of [1] to [5], wherein the resin component (D) adheres to the fiber bundle surface of the bundled reinforcing fibers (A-2).
[0033] [7] The fiber-reinforced resin molding material according to [6], wherein the resin component (D) is a thermosetting resin,
[0034] The resin component (D) is contained in an amount of 7 parts by weight or more based on 100 parts by weight of the bundled reinforcing fibers (A-2).
[0035] [8] The fiber-reinforced resin molding material according to any one of [1] to [7], wherein the thermoplastic resin (B) comprises at least one selected from the group consisting of polyamide resin, polycarbonate resin, polyphenylene sulfide resin and polypropylene resin.
[0036] [9] A fiber-reinforced resin molded product comprising reinforcing fibers (A') and a thermoplastic resin (B),
[0037] The fiber-reinforced resin molded article contains 1 to 30 parts by weight of reinforcing fiber (A') and 70 to 99 parts by weight of thermoplastic resin (B) based on 100 parts by weight of the total of (A') and (B).
[0038] The weight average fiber length Lw(A') of the reinforcing fiber (A') is 0.1 to 2.9 mm,
[0039] The reinforcing fibers (A') include bundled reinforcing fibers (A-2') composed of 10 or more single fibers each having a length of 0.5 to 2.9 mm.
[0040]
[10] The fiber-reinforced resin molded article according to [9], wherein the proportion of reinforcing fibers (A') having a fiber length of 0.3 to 1.0 mm is 40% or more.
[0041]
[11] The fiber-reinforced resin molded article according to [9] or
[10] , comprising 1 to 50 parts by weight of the bundled reinforcing fibers (A-2') based on 100 parts by weight of the reinforcing fibers (A').
[0042]
[12] . The fiber-reinforced resin molded article according to any one of [9] to
[11] , wherein the reinforcing fiber (A') is a carbon fiber.
[0043]
[13] The fiber-reinforced resin molded article according to any one of [9] to
[12] , wherein the resin component (D) adheres to the fiber bundle surface of the bundled reinforcing fibers (A-2′).
[0044]
[14] The fiber-reinforced resin molded article according to
[13] , wherein the resin component (D) is a thermosetting resin,
[0045] The resin component (D) is contained in an amount of 7 parts by weight or more based on 100 parts by weight of the bundled reinforcing fibers (A-2').
[0046]
[15] The fiber-reinforced resin molded article according to any one of [9] to
[14] , wherein the thermoplastic resin (B) comprises at least one selected from the group consisting of polyamide resin, polycarbonate resin, polyphenylene sulfide resin and polypropylene resin.
[0047] [Effects of the invention]
[0048] According to the present invention, a molding material that can achieve both excellent fluidity and mechanical properties and dimensional accuracy can be obtained. The molding material of the present invention has excellent fluidity during molding processing, and can easily produce molded products with excellent mechanical properties and dimensional accuracy. Therefore, it is not limited to molding methods such as injection molding, transfer molding, blow molding, and insert molding, and can also be applied to a wide range of molding methods such as plunger molding, press molding, and stamping molding.
[0049] As molded products obtained by molding the molding material of the present invention, there can be listed automotive parts such as thrust washers, oil filters, seals, bearings, gears, cylinder heads, bearing retainers, intake manifolds, pedals, etc.; semiconductor and liquid crystal manufacturing equipment parts such as silicon wafer carriers, IC wafer trays, electrolytic capacitor trays, insulating films, etc.; compressor parts such as pumps, valves, seals, etc., industrial machinery parts such as aircraft cabin interior parts; medical equipment parts such as sterilizers, columns, piping, etc., and food and beverage manufacturing equipment parts. In addition, if the molding material of the present invention is used, a thin-walled molded product of 0.5 to 2 mm can be obtained relatively easily. As an object requiring such thin-wall molding, for example, electrical and electronic machine components such as keyboard supports that are inside a personal computer and support the keyboard. Such electrical and electronic machine components are preferably given electromagnetic wave shielding properties when conductive carbon fibers are used in the reinforcing fibers. BRIEF DESCRIPTION OF THE DRAWINGS
[0050] Figure 1 This is a schematic diagram showing an example of the shape of the cross section in the axial direction of the molding material according to one embodiment of the present invention.
[0051] Figure 2 This is a schematic diagram showing an example of the shape of the cross section in the axial direction of the molding material according to another embodiment of the present invention.
[0052] Figure 3 This is a schematic diagram showing an example of the shape of a cross section of a molding material according to still another embodiment of the present invention in a direction perpendicular to the axis.
[0053] Figure 4 This is a schematic diagram showing an example of the shape of a cross section of a molding material according to still another embodiment of the present invention in a direction perpendicular to the axis.
[0054] Figure 5 This is a schematic diagram showing an example of the shape of a cross section of a molding material according to still another embodiment of the present invention in a direction perpendicular to the axis.
[0055] Figure 6 This is a schematic perspective view showing an example of the shape of a molding material according to still another embodiment of the present invention.
[0056] Figure 7This is a schematic perspective view showing an example of the shape of a molding material according to still another embodiment of the present invention.
[0057] Figure 8 This is a schematic perspective view showing an example of the shape of a molding material according to still another embodiment of the present invention. DETAILED DESCRIPTION
[0058] Hereinafter, the present invention will be described in detail together with embodiments.
[0059] <Molding materials>
[0060] The molding material of the present invention comprises reinforcing fibers (A) and a thermoplastic resin (B). By comprising the reinforcing fibers (A), the fiber length of the reinforcing fibers can be kept long, and excellent mechanical properties can be exhibited.
[0061] [Reinforcement fiber (A)]
[0062] The reinforcing fiber (A) in the present invention will be described.
[0063] There is no particular restriction on the type of reinforcing fiber (A) in the present invention, for example, carbon fiber, glass fiber, aromatic polyamide fiber, aluminum oxide fiber, silicon carbide fiber, boron fiber, metal fiber, natural fiber, mineral fiber, etc. can be used, and one or more of these can be used. Among them, from the viewpoint of obtaining a lightweight, high-strength, high-elastic modulus molded product, it is preferred to use carbon fibers of PAN (polyacrylonitrile), asphalt, rayon, etc. In particular, from the viewpoint of high strength, a reinforcing fiber having a tensile strength of more than 4000MPa is preferred, more preferably more than 5000MPa. From the viewpoint of high elastic modulus, a reinforcing fiber having a tensile elastic modulus of more than 200GPa is preferred, more preferably more than 400GPa. In particular, a reinforcing fiber having an elastic modulus of more than 400GPa that is difficult to maintain a long fiber length is preferred because it can better show the effect of the molding material of the present invention described later.
[0064] In addition, from the viewpoint of improving the economic efficiency of the obtained molded product, glass fiber is preferably used, and in particular, from the viewpoint of the balance between mechanical properties and economic efficiency, carbon fiber and glass fiber are preferably used in combination. Furthermore, from the viewpoint of improving the impact absorption or shaping property of the obtained molded product, aromatic polyamide fiber is preferably used, and in particular, from the viewpoint of the balance between mechanical properties and impact absorption, carbon fiber and aromatic polyamide fiber are preferably used in combination. In addition, from the viewpoint of improving the conductivity of the obtained molded product, reinforcing fibers coated with metals such as nickel, copper, and ytterbium, and asphalt-based carbon fibers may also be used.
[0065] It is preferred that the sizing agent is attached to the reinforcing fibers (A). This is because by attaching the sizing agent to the reinforcing fibers (A), the handling properties of the reinforcing fibers during transfer and the process of manufacturing the molding material can be improved. There is no particular limitation on the type of sizing agent, but one or more sizing agents such as epoxy resins, urethane resins, acrylic resins, or various thermoplastic resins can be used.
[0066] The reinforcing fiber (A) is preferably 1 to 30 parts by weight relative to 100 parts by weight of the molding material. It is more preferably 2 to 25 parts by weight, and particularly preferably 5 to 20 parts by weight. When the reinforcing fiber (A) is less than 1 part by weight, the mechanical properties and dimensional accuracy of the resulting molded product will become insufficient, and when it exceeds 30 parts by weight, the fluidity will decrease.
[0067] In the reinforcing fiber (A) of the present invention, reinforcing fibers (A-1) and bundled reinforcing fibers (A-2) are included. The length of the reinforcing fiber (A-1) is preferably 3 to 15 mm, more preferably 5 to 10 mm. The reinforcing fiber (A-1) is preferably in a state where the single fibers are arranged in one direction. As a preferred form, unidirectional fiber bundles, bidirectional fiber bundles, multidirectional fiber bundles, etc. can be exemplified, but from the perspective of productivity in the process of manufacturing molding materials, unidirectional fiber bundles are more preferably used. The reinforcing fiber (A) is more economical from the perspective of the more monofilaments of the reinforcing fiber, and when the molding material is formed into a granular form, for example, the monofilaments in one particle are preferably more than 10,000. On the other hand, there is a tendency that the more monofilaments of the reinforcing fiber are, the more unfavorable the impregnation of the matrix resin is, so from the perspective of seeking both economic and impregnation, it is more preferred to use more than 15,000 and less than 100,000, and it is particularly preferred to use more than 20,000 and less than 50,000.
[0068] In addition, the reinforcing fiber (A-1) is preferably: in the molding material, the reinforcing fiber (A-1) is aligned with the length direction of the molding material, and the length of the reinforcing fiber (A-1) is substantially the same as the length of the molding material. Here, the longitudinal direction of the molding material is aligned, which means that the axis of the major axis of the reinforcing fiber (A-1) and the axis of the major axis of the molding material point to the same direction, and the offset of the angle between the axes is preferably less than 20 °, more preferably less than 10 °, and particularly preferably less than 5 °. In addition, the substantially same length means that, for example, in a granular molding material, the reinforcing fiber (A-1) is not cut off on the way inside the particle, or substantially does not include a reinforcing fiber (A-1) that is meaningfully shorter than the total length of the particle. Furthermore, the total length of the particle is the length of the orientation direction of the reinforcing fiber (A-1) in the particle. Since the reinforcing fiber (A-1) has a substantially the same length as the molding material, the reinforcing fiber length in the molded product can be increased, and excellent mechanical properties and dimensional accuracy can be obtained.
[0069] The length of the bundled reinforcing fibers (A-2) is preferably 0.5 to 2.9 mm, more preferably 0.6 to 2.7 mm, and particularly preferably 0.7 to 2.5 mm. When the length of the bundled reinforcing fibers (A-2) is less than 0.5 mm, it is not suitable because the mechanical properties and dimensional accuracy of the molded product are poor. On the other hand, when the length of the bundled reinforcing fibers (A-2) is longer than 2.9 mm, it is not suitable because of poor fluidity. In addition, the bundled reinforcing fibers (A-2) are composed of more than 10 reinforcing fiber filaments. The reinforcing fiber filaments constituting the bundled reinforcing fibers (A-2) are preferably 10 or more, more preferably 15 or more, and particularly preferably 20 or more. When the number of filaments of the bundled reinforcing fibers (A-2) is less than 10, the mechanical properties and dimensional accuracy of the molded product are poor and not suitable because fiber breakage occurs during injection molding. There is no particular upper limit on the number of filaments, but it is preferably 100,000 or less, and more preferably 80,000 or less. When the number of monofilaments exceeds 100,000, it is not preferable because the surface quality of the molded product is poor.
[0070] As the form of the bundled reinforcing fiber (A-2) used during melt mixing, there is no restriction as long as it is a form that can be added to the melt mixing device, and pre-cut chopped strands (chopped strand), broken fibers, continuous long fibers, etc. can be listed. From the perspective of productivity, chopped strands are preferably used. As chopped strands, it can be a recycled chopped strand obtained by crushing the fiber-reinforced resin molding and thermally decomposing the matrix resin. As a method for obtaining recycled chopped strands, it can be obtained by a known method. For example, the waste sheets that have been crushed and graded for the fiber-reinforced resin molding are evenly spread on a metal plate, placed in an electric muffle furnace, and nitrogen is introduced into the furnace while the treatment temperature is maintained at a specific temperature for heat treatment. Thereafter, in the same way, air is introduced into the furnace while the treatment temperature is maintained at a specific temperature for heat treatment, and recycled chopped strands can be obtained.
[0071] Furthermore, the heat treatment temperature in the air environment in the heat treatment step is preferably 300°C to 700°C. If the heat treatment temperature in the air environment exceeds 700°C, the resin component (D) described later will completely disappear, and only the reinforcing fibers will be present, and the bundled properties of the reinforcing fiber bundle (bundle-shaped reinforcing fiber (A-2)) will disappear, and it will not be able to remain as a bundle-shaped reinforcing fiber, so the fiber breakage will increase, and the mechanical properties or dimensional accuracy will be poor, so it is not suitable. On the contrary, if the heat treatment temperature is lower than 300°C, the resin component (D) will increase, resulting in a decrease in toughness as a matrix resin, and poor mechanical properties, so it is not suitable.
[0072] In addition, it is preferred to carry out the final heat treatment in an air environment. If the initial heat treatment is carried out at 700°C for 2 hours in a nitrogen environment, the resin component (D) becomes 7 parts by weight or more. In an inert nitrogen environment, the resin component (D) does not change even if the heat treatment is carried out for more than 2 hours. By carrying out the final heat treatment in an active air environment, a recycled chopped strand having the desired resin component (D) can be obtained.
[0073] In the present invention, a fiber-reinforced resin molding can be used after being crushed. When crushing, if the subsequent processability is taken into consideration, the maximum length after crushing is preferably crushed to less than 20 mm. As a crusher for such a fiber-reinforced resin molding, a shearing crusher, an impact crusher, a cutting crusher, and a compression crusher can be used. There is no problem in using any crusher, and they can also be combined. In addition, as a classifier for crushed products, a vibrating screening machine, a rotary screening machine, and a centrifugal screening machine can be used. It is preferably used in combination with the crushing capacity of the crusher and the shape of the crushed product.
[0074] The types of reinforcing fibers (A-1) and bundled reinforcing fibers (A-2) used in the present invention are not particularly limited, and any filler having a fibrous shape may be used. Specifically, glass fibers; PAN-based and asphalt-based carbon fibers; metal fibers such as stainless steel fibers, aluminum fibers, and brass fibers; organic fibers such as aromatic polyamide fibers; fibrous and whisker-shaped fillers such as gypsum fibers, ceramic fibers, asbestos fibers, zirconium oxide fibers, aluminum oxide fibers, silica fibers, titanium oxide fibers, silicon carbide fibers, rock wool, potassium titanate whiskers, silicon nitride whiskers, wollastonite, and aluminum oxide silicates; non-metallic fibers (glass fibers, aromatic polyamide fibers, polyester fibers, carbon fibers, etc.) coated with metals (nickel, copper, cobalt, silver, aluminum, iron, and their alloys, etc.). Among the short fiber-shaped fillers, PAN-based and asphalt-based carbon fibers are cited as preferred examples, and PAN-based carbon fibers are particularly preferred.
[0075] The content of the reinforcing fiber (A-1) and the bundled reinforcing fiber (A-2) of the present invention is preferably: relative to 100 parts by weight of the reinforcing fiber (A), it contains 50 to 99 parts by weight of the reinforcing fiber (A-1) and 1 to 50 parts by weight of the bundled reinforcing fiber (A-2). If the content of the reinforcing fiber (A-1) is less than 50 parts by weight, the mechanical properties and dimensional stability of the molded product are poor, so it is not suitable. In addition, if the content of the reinforcing fiber (A-1) exceeds 99 parts by weight, the fluidity during injection molding is poor, so it is not suitable. The content of the reinforcing fiber (A-1) is more preferably 60 to 95 parts by weight, and particularly preferably 70 to 90 parts by weight. If the content of the bundled reinforcing fiber (A-2) is less than 1 part by weight, the mechanical properties and dimensional accuracy of the molded product are poor, so it is not suitable. If the content of the bundled reinforcing fiber (A-2) exceeds 50 parts by weight, the mechanical properties are poor, so it is not suitable.
[0076] [Thermoplastic resin (B)]
[0077] The molding material of the present invention contains 70 to 99 parts by weight of the thermoplastic resin (B) based on 100 parts by weight of the total of the reinforcing fiber (A) and the thermoplastic resin (B).
[0078] In the present invention, the thermoplastic resin (B) preferably has a molding temperature (melting temperature) of 200 to 450° C., and examples thereof include polyolefin resins, polystyrene resins, polyamide resins, halogenated vinyl resins, polyacetal resins, saturated polyester resins, polycarbonate resins, polyaryl sulfone resins, polyaryl ketone resins, polyphenylene ether resins, polyphenylene sulfide resins, polyaryl ether ketone resins, polyether sulfone resins, polyphenylene sulfide sulfone resins, polyarylate resins, polyamide resins, etc., all of which are equivalent to electrical insulators. Two or more of them may be used.
[0079] Among the thermoplastic resins (B), polyolefin resins, polyamide resins, polycarbonate resins, and polyarylene sulfide resins are more preferred because they are lightweight and have an excellent balance between mechanical properties and moldability.
[0080] The polyolefin resin mentioned here also includes unmodified and modified ones. For example, unmodified polypropylene resin is specifically a homopolymer of propylene or a copolymer of propylene and at least one α-olefin, conjugated diene, non-conjugated diene, etc. As α-olefin, for example, ethylene, 1-butene, 3-methyl-1-butene, 4-methyl-1-pentene, 3-methyl-1-pentene, 4-methyl-1-hexene, 4,4-dimethyl-1-hexene, 1-nonene, 1-octene, 1-heptene, 1-hexene, 1-decene, 1-undecene, 1-dodecene, etc., excluding propylene, and the like, and the like. As conjugated diene and non-conjugated diene, for example, butadiene, ethylidene norbornene, dicyclopentadiene, 1,5-hexadiene, etc., can be listed. Two or more of them can also be used. As the skeleton structure of the unmodified polypropylene resin, there can be listed homopolymers of propylene, random or block copolymers of propylene and the above-mentioned other monomers, or random or block copolymers of propylene and other thermoplastic monomers, etc. Suitable examples include: polypropylene, ethylene-propylene copolymers, propylene-1-butene copolymers, ethylene-propylene-1-butene copolymers, etc. From the viewpoint of further improving the rigidity of the molded article, a homopolymer of propylene is preferred, and from the viewpoint of further improving the impact strength of the molded article, a random or block copolymer of propylene and the above-mentioned other monomers is preferred.
[0081] In addition, as the modified polypropylene resin, an acid-modified polypropylene resin is preferred, and a polypropylene resin having a carboxylic acid and / or a salt thereof bonded to a polymer chain is more preferred. The acid-modified polypropylene resin can be obtained by various methods. For example, it can be obtained by graft-polymerizing a monomer having a neutralized or unneutralized carboxylic acid group and / or a monomer having a saponified or unsaponified carboxylic acid ester on a polypropylene resin.
[0082] Here, examples of monomers having a neutralized or unneutralized carboxylic acid group or a monomer having a saponified or unsaponified carboxylic acid ester group include ethylenically unsaturated carboxylic acids, anhydrides thereof, and esters thereof. In addition, compounds having an unsaturated vinyl group other than olefins may also be mentioned.
[0083] Examples of the ethylenically unsaturated carboxylic acid include (meth)acrylic acid, maleic acid, fumaric acid, tetrahydrophthalic acid, itaconic acid, citraconic acid, crotonic acid, isocrotonic acid, etc. Examples of the anhydride thereof include nadic acid TM (endo-cis-bicyclo[2.2.1]hept-5-ene-2,3-dicarboxylic acid), maleic anhydride, citraconic anhydride, etc.
[0084] Examples of the esters of ethylenically unsaturated carboxylic acids include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, n-pentyl (meth)acrylate, isopentyl (meth)acrylate, n-hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, octyl (meth)acrylate, decyl (meth)acrylate, dodecyl (meth)acrylate, octadecyl (meth)acrylate, (meth)acrylic acid, tridecyl (meth)acrylate, lauroyl (meth)acrylate, cyclohexyl (meth)acrylate, benzyl (meth)acrylate, phenyl (meth)acrylate, isobornyl (meth)acrylate, dicyclopentyl (meth)acrylate, dicyclopentenyl (meth)acrylate, dimethylaminoethyl (meth)acrylate, and (meth)acrylic acid. ) (Meth)acrylates such as diethylaminoethyl (meth)acrylate; hydroxyl-containing (meth)acrylates such as hydroxyethyl acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl acrylate, lactone-modified hydroxyethyl (meth)acrylate, 2-hydroxy-3-phenoxypropyl acrylate, etc.; epoxy-containing (meth)acrylates such as glycidyl (meth)acrylate and methylglycidyl (meth)acrylate; aminoalkyl (meth)acrylates such as N,N-dimethylaminoethyl (meth)acrylate, N,N-diethylaminoethyl (meth)acrylate, N,N-dimethylaminopropyl (meth)acrylate, N,N-dipropylaminoethyl (meth)acrylate, N,N-dibutylaminoethyl (meth)acrylate, and N,N-dihydroxyethylaminoethyl (meth)acrylate.
[0085] Examples of monomers having an unsaturated vinyl group other than an olefin include: vinyl groups containing an isocyanate group such as vinyl isocyanate and isopropenyl isocyanate; aromatic vinyl groups such as styrene, α-methylstyrene, vinyltoluene, and tert-butylstyrene; vinyl groups containing an amide group such as acrylamide, methacrylamide, N-methylolmethacrylamide, N-methylolacrylamide, diacetoneacrylamide, and maleic acid amide; vinyl esters such as vinyl acetate and vinyl propionate; unsaturated sulfonic acids such as styrenesulfonic acid, sodium styrenesulfonate, and 2-acrylamide-2-methylpropanesulfonic acid; and unsaturated phosphoric acids such as mono(2-methacryloyloxyethyl) acid phosphate and mono(2-acryloyloxyethyl) acid phosphate.
[0086] Two or more of these may be used. Among these, ethylenically unsaturated carboxylic acid anhydrides are preferred, and maleic anhydride is more preferred.
[0087] Here, in order to improve the bending strength and tensile strength of the molded product, it is preferred to use both the unmodified polypropylene resin and the modified polypropylene resin. In particular, from the viewpoint of the balance between flame retardancy and mechanical properties, it is preferred to use the unmodified polypropylene resin and the modified polypropylene resin in a weight ratio of 95 / 5 to 75 / 25. It is more preferably 95 / 5 to 80 / 20, and particularly preferably 90 / 10 to 80 / 20.
[0088] In addition, polyamide resin is a resin with amino acid, lactam, or diamine and dicarboxylic acid as main raw materials. Representative examples of the main raw materials include: amino acids such as 6-aminocaproic acid, 11-aminoundecanoic acid, 12-aminododecanoic acid, and p-aminomethylbenzoic acid; lactams such as ε-caprolactam and ω-laurolactam; aliphatic diamines such as tetramethylenediamine, hexamethylenediamine, 2-methylpentamethylenediamine, nonamethylenediamine, undecamethylenediamine, dodecamethylenediamine, 2,2,4- / 2,4,4-trimethylhexamethylenediamine, and 5-methylnonamethylenediamine; aromatic diamines such as m-xylylenediamine and p-xylylenediamine; 1,3-bis(aminomethyl)cyclohexane, 1,4-bis(aminomethyl)cyclohexane, 1-amino-3-aminomethyl- Alicyclic diamines such as 3,5,5-trimethylcyclohexane, bis(4-aminocyclohexyl)methane, bis(3-methyl-4-aminocyclohexyl)methane, 2,2-bis(4-aminocyclohexyl)propane, bis(aminopropyl)piperazine, and aminoethylpiperazine; aliphatic dicarboxylic acids such as adipic acid, suberic acid, azelaic acid, sebacic acid, and dodecanedioic acid; aromatic dicarboxylic acids such as terephthalic acid, isophthalic acid, 2-chloroterephthalic acid, 2-methylterephthalic acid, 5-methylisophthalic acid, 5-sodiumsulfoisophthalic acid, hexahydroterephthalic acid, and hexahydroisophthalic acid; alicyclic dicarboxylic acids such as 1,4-cyclohexanedicarboxylic acid, 1,3-cyclohexanedicarboxylic acid, and 1,2-cyclohexanedicarboxylic acid. Two or more of these may be used.
[0089] In the present invention, a polyamide resin having a melting point of 200° C. or higher is particularly useful from the viewpoint of excellent heat resistance and strength. Specific examples thereof include polycaproamide (nylon 6), polyhexamethylene adipamide (nylon 66), polycaproamide / polyhexamethylene adipamide copolymer (nylon 6 / 66), polytetramethylene adipamide (nylon 46), polyhexamethylene sebacamide (nylon 610), polyhexamethylene dodecanamide (nylon 612), polydecamethylene sebacamide (nylon 1010), polydecamethylene dodecanamide (nylon 1012), polydodecamethylene dodecanamide (nylon 1212), polyundecamide (nylon 11), polydodecanamide (nylon 12), polyhexamethylene terephthalamide / polycaproamide copolymer (nylon 6T / 6), polyhexamethylene adipamide / polyhexamethylene terephthalamide copolymer (nylon 66 / 6T), polyhexamethylene adipamide / polyhexamethylene isophthalamide copolymer (nylon 66 / 6I), polyhexamethylene adipamide / polyhexamethylene terephthalamide / polyhexamethylene isophthalamide copolymer (nylon 66 / 6T / 6I), polyhexamethylene terephthalamide / polyhexamethylene isophthalamide copolymer (nylon 6T / 6I), polyhexamethylene terephthalamide / polydodecanamide copolymer (nylon 6T / 12), polyhexamethylene terephthalamide / poly (2-methylpentamethylene) terephthalamide copolymer (nylon 6T / M5T), polyisophthalylene adipamide (nylon XD6), polynonamethylene terephthalamide (nylon 9T) and their copolymers etc. Also can use two or more of these. Among these, more preferably nylon 6, nylon 66, nylon 610, nylon 11, nylon 12 and nylon 9T.
[0090] The polymerization degree of these polyamide resins is not particularly limited, but preferably the relative viscosity of a solution of 0.25 g of the polyamide resin dissolved in 25 ml of 98% concentrated sulfuric acid is in the range of 1.5 to 5.0, and more preferably 2.0 to 3.5.
[0091] In addition, polycarbonate resin is obtained by reacting dihydric phenols and carbonate precursors. It can also be the multipolymer obtained by using more than 2 dihydric phenols or more than 2 carbonate precursors. As an example of reaction method, can list: interfacial polymerization, melt transesterification, solid phase transesterification of carbonate prepolymers and ring-opening polymerization of cyclic carbonate compounds etc. This polycarbonate resin itself is known, for example, can use the polycarbonate resin of recording in Japanese Unexamined Patent Publication No. 2002-129027 communique.
[0092] Examples of dihydric phenols include 1,1-bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane, bis(4-hydroxyphenyl)alkane (bisphenol A, etc.), 2,2-bis{(4-hydroxy-3-methyl)phenyl}propane, α,α'-bis(4-hydroxyphenyl)-m-diisopropylbenzene, 9,9-bis(4-hydroxy-3-methylphenyl)fluorene, etc. Two or more of these may be used. Among these, bisphenol A is preferred because it can produce a polycarbonate resin having a better impact strength. On the other hand, copolymers obtained using bisphenol A and other dihydric phenols are excellent in terms of high heat resistance or low water absorption.
[0093] As the carbonate precursor, for example, carbonyl halides, carbonic acid diesters, halogenated formate, etc. Specifically, phosgene, diphenyl carbonate, dihalogenated formate of dihydric phenols, etc. can be used.
[0094] When the polycarbonate resin is produced from the above-mentioned diphenols and carbonate precursors, a catalyst, a terminal blocking agent, an antioxidant for preventing oxidation of the diphenols, and the like may be used as necessary.
[0095] In addition, the polycarbonate resin of the present invention includes a branched polycarbonate resin copolymerized with a trifunctional or more polyfunctional aromatic compound, a polyester carbonate resin copolymerized with an aromatic or aliphatic (including alicyclic) difunctional carboxylic acid, a copolymerized polycarbonate resin copolymerized with a difunctional alcohol (including alicyclic), and a polyester carbonate resin copolymerized with a difunctional carboxylic acid and a difunctional alcohol. These polycarbonate resins are also known. In addition, two or more polycarbonate resins among these may also be used.
[0096] The molecular weight of the polycarbonate resin is not limited, but the viscosity average molecular weight is preferably 10,000 to 50,000. If the viscosity average molecular weight is 10,000 or more, the strength of the molded product can be further improved. It is more preferably 15,000 or more, and particularly preferably 18,000 or more. On the other hand, if the viscosity average molecular weight is 50,000 or less, the molding processability is improved. It is more preferably 40,000 or less, and particularly preferably 30,000 or less. When two or more polycarbonate resins are used, it is preferred that at least one has a viscosity average molecular weight within the above range. In this case, it is preferred to use a polycarbonate resin having a viscosity average molecular weight exceeding 50,000 (preferably exceeding 80,000) as the other polycarbonate resin. The polycarbonate resin has high entropy elasticity, which is advantageous for use in combination with gas-assisted molding, and also exhibits characteristics derived from high entropy elasticity (characteristics of improved melting characteristics such as dripping prevention characteristics, drooping characteristics, and injection improvement).
[0097] The viscosity average molecular weight (M) of the polycarbonate resin is obtained by dissolving 0.7 g of the polycarbonate resin in 100 ml of dichloromethane and determining the specific viscosity (η) at 20°C. sp ), and substitute it into the following formula to obtain:
[0098] ηsp / c=[η]+0.45×[η] 2 c (where [η] is limiting viscosity)
[0099] [η] = 1.23 × 10 -4 M 0.83
[0100] c=0.7
[0101] In the present invention, examples of the polyarylene sulfide resin include polyphenylene sulfide (PPS) resin, polyphenylene sulfide sulfone resin, polyphenylene sulfide ketone resin, and random or block copolymers thereof. Two or more of these may be used. Among them, polyphenylene sulfide resin is particularly preferably used.
[0102] The polyarylene sulfide resin can be produced by any method such as the method for obtaining a relatively small molecular weight polymer described in JP-B-45-3368, the method for obtaining a relatively large molecular weight polymer described in JP-B-52-12240 and JP-A-61-7332.
[0103] The obtained polyarylene sulfide resin may be subjected to the following various treatments: crosslinking / molecularization by heating in air; heat treatment in an inert gas environment such as nitrogen or under reduced pressure; washing with an organic solvent, hot water, an acid aqueous solution, etc.; activation with a functional group-containing compound such as an acid anhydride, amine, isocyanate, a functional group-containing disulfide compound, etc.
[0104] The melt viscosity of the polyarylene sulfide resin is preferably 80 Pa·s or less, and more preferably 20 Pa·s or less, at 310°C and a shear rate of 1000 / sec. There is no particular restriction on the lower limit, but it is preferably 5 Pa·s or more. Two or more polyarylene sulfide resins having different melt viscosities may be used in combination. The melt viscosity can be measured using a Capillograph (manufactured by Toyo Seiki Co., Ltd.) under the conditions of a die length of 10 mm and a die hole diameter of 0.5 to 1.0 mm.
[0105] As the polyarylene sulfide resin, those commercially available as “Torelina” (registered trademark) manufactured by Toray Industries, Ltd., “DIC.PPS” (registered trademark) manufactured by DIC Corporation, “Durafide” (registered trademark) manufactured by Polyplastics Corporation, etc. can be used.
[0106] The molding material of the present invention includes, for example, a fiber-reinforced thermoplastic resin molding material (X) and a fiber-reinforced thermoplastic resin molding material (Y). The fiber-reinforced thermoplastic resin molding material (X) is composed of the reinforcing fiber (A-1) and the thermoplastic resin (B-1), and the reinforcing fiber (A-1) is preferably oriented in the same direction as the length direction of the fiber-reinforced thermoplastic resin molding material (X). Furthermore, the thermoplastic resin (B-1) may be of the same type as the thermoplastic resin (B). In addition, the length of the fiber-reinforced thermoplastic resin molding material (X) is preferably 3 to 15 mm, more preferably 5 to 10 mm, from the viewpoint of handling. By making long-fiber particles of this length, particles for injection molding with high versatility can be obtained, and the mechanical properties of the molded product can be fully improved by improving the fluidity and handling properties during injection molding and being able to increase the length of the reinforcing fibers in the molded product.
[0107] In addition, the reinforcing fiber (A-1) contained in the fiber-reinforced thermoplastic resin molding material (X) can be a composite in a state where a compound different from the thermoplastic resin (B) is attached. The composite refers to a composite in a state where the individual fibers of the reinforcing fiber (A-1) are filled with resin, that is, a composite in a state where the reinforcing fiber (A-1) is dispersed like an island in a sea of the compound. Although it is desired that the reinforcing fiber (A-1) is completely impregnated with the compound, a certain degree of voids may also exist in the composite composed of the reinforcing fiber (A-1) and the compound. The void ratio of the composite is preferably in the range of 0 to 40%, more preferably 0 to 20% or less. If the void ratio is in this range, the effect of impregnation and fiber dispersion promotion is excellent. The void ratio is the portion of the composite measured by the ASTM D2734 (1997) test method. In addition, there is no particular limitation on the form of coating, but for example, a form in which the thermoplastic resin (B) coats part or all of the strand-shaped composite. In the case of this form, a form in which more than 50% of the surrounding of the strand-shaped composite is coated is preferred, a form in which more than 80% of the surrounding of the strand-shaped composite is coated is more preferred, and a form in which the thermoplastic resin (B) coats all of the surrounding of the strand-shaped composite is most preferred. By coating the composite with the thermoplastic resin (B), the handleability of the molding material is improved. If the composite is bonded to the thermoplastic resin (B), the state of the boundary between the composite and the thermoplastic resin (B) is not particularly limited, but it is preferably: the thermoplastic resin (B) partially enters a part of the composite near the boundary between the composite and the thermoplastic resin (B) and is compatible with the compound in the composite; or it is impregnated in the reinforcing fiber (A-1). If it is in this state, the coated thermoplastic resin (B) is not easy to peel off from the composite, and a molding material with good handleability can be obtained. The feeding during molding is stable, uniform plasticization can be achieved, and excellent fluidity can be exhibited.
[0108] Figures 1-2 The shape of the cross section in the axial direction of the molding material of the present invention is schematically shown. Figures 3 to 5 The shape of the cross section in the orthogonal direction of the molding material of the present invention is schematically shown.
[0109] The cross-sectional shape of the molding material is not limited to that shown in the figure, but is preferably as follows: Figure 1 As shown, it is preferable to arrange the reinforcing fiber (A-1) 1 as a core material so as to be sandwiched by the thermoplastic resin (B) 2 in layers.
[0110] Furthermore, as shown in the perspective oblique view Figure 6 , 8 As shown, the reinforcing fiber (A-1) 1 is a core structure, and the thermoplastic resin (B) 2 is a sheath structure. The molding material is preferably a core-sheath structure in which the thermoplastic resin (B) covers the reinforcing fiber (A-1). By forming a molding material with such a structure, when the molding material is molded, a long reinforcing fiber bundle can remain in the molded product, which can improve the mechanical properties as an effect of the present invention. Furthermore, it can also be a multi-core sheath structure configured in a manner that the thermoplastic resin (B) covers a plurality of reinforcing fibers (A-1), in which case the number of reinforcing fibers (A) is preferably 2 or more and 6 or less.
[0111] From the perspective of the handling of the molding material, it is important that the composite and the thermoplastic resin (B) are not separated before molding and that the thermoplastic resin (B) covers the composite. Since the compound has a low molecular weight, most of them are relatively brittle and easily broken solids. Therefore, it is desirable to configure the thermoplastic resin (B) in a way that protects the composite so that the compound is not broken or scattered due to impact, friction, etc. during material transportation and handling before molding.
[0112] The fiber-reinforced thermoplastic resin molding material (Y) is composed of bundled reinforcing fibers (A-2) and a thermoplastic resin (B-2). The fiber-reinforced thermoplastic resin molding material (Y) can be pelletized by melt kneading (for example, Figure 7 , Figure 8 The thermoplastic resin (B-1) may be the same type as the thermoplastic resin (B).
[0113] The fiber-reinforced thermoplastic resin molding materials (X) and (Y) can be dry-blended to form a molding material mixture. In this case, the content of the reinforcing fiber (A) in the molded product can be easily adjusted. Dry blending here is different from melt kneading, and refers to stirring and mixing a plurality of materials at a temperature at which the resin component does not melt to form a substantially uniform state, and is mainly suitable for the case of using a pellet-shaped molding material such as injection molding and extrusion molding.
[0114] The molding material of the present invention is preferably a core-sheath structure comprising reinforcing fibers (A-1), bundled reinforcing fibers (A-2) and a thermoplastic resin (B). Specifically, it is preferred that: the core structure of the core-sheath structure comprises reinforcing fibers (A-1), and the reinforcing fibers (A-1) and the molding material are oriented in the same direction in length, and the sheath structure of the core-sheath structure is a fiber-reinforced resin composition (C) comprising bundled reinforcing fibers (A-2) and a thermoplastic resin (B). Furthermore, the reinforcing fibers (A-1) are preferably in a form of coating the fiber-reinforced thermoplastic resin composition (C) (e.g. Figure 8 ).
[0115] In the molding material of the present invention, since the spaces between the single fibers of the reinforcing fibers (A-1) are filled with the compound (E), the dispersibility of the reinforcing fibers can be improved when the molding material is molded.
[0116] The above-mentioned compound (E) preferably has a lower melt viscosity than the thermoplastic resin (B). Since the melt viscosity of the compound (E) is lower than that of the thermoplastic resin (B), when the molding material is molded, the fluidity of the compound (E) is high, and the dispersion effect of the reinforcing fiber (A-1) in the thermoplastic resin (B) can be further improved. In addition, the compound (E) preferably has a high affinity with the thermoplastic resin (B). By selecting an impregnated resin with a high affinity with the thermoplastic resin (B), it will be compatible with the thermoplastic resin (B) efficiently during the manufacture and molding of the molding material, so the dispersibility of the reinforcing fiber can be further improved.
[0117] The compound (E) is preferably a resin selected from epoxy resins, phenol resins, terpene resins and cyclic polyphenylene sulfide. The compound (E) is preferably used because it can improve the dispersibility of the reinforcing fibers during molding of the molding material by pre-impregnating the reinforcing fibers (A-1).
[0118] The number average molecular weight of compound (E) is preferably 200 to 5000. If the number average molecular weight is 200 or more, the flexural strength and tensile strength of the molded article can be further improved. The number average molecular weight is more preferably 1000 or more. In addition, if the number average molecular weight is 5,000 or less, the viscosity of the compound is moderately low, so the impregnation property of the reinforcing fiber (A) is excellent, and the dispersibility of the reinforcing fiber in the molded article can be further improved. The number average molecular weight is more preferably 3,000 or less. Furthermore, the number average molecular weight of the compound can be measured using gel permeation chromatography (GPC).
[0119] The compound (E) is preferably used in an amount of 0.1 to 20 parts by weight, more preferably 3 to 10 parts by weight, based on 100 parts by weight of the molding material. By setting the amount within this range, a molding material having excellent moldability and handling properties can be obtained.
[0120] [Resin component (D)]
[0121] In the bundled reinforcing fibers (A-2) of the present invention, it is preferred that the resin component (D) adheres to the surface of the fiber bundle.
[0122] The resin component (D) is preferably contained in an amount of 7 parts by weight or more relative to 100 parts by weight of the bundled reinforcing fibers (A-2). When the resin component (D) is less than 7 parts by weight, the bundled reinforcing fibers (A-2) have reduced agglomeration, which may increase fiber breakage during injection molding and reduce mechanical properties, and is therefore not suitable. It is more preferably 8 parts by weight or more, and particularly preferably 9 parts by weight. There is no upper limit, but it is preferably 20 parts by weight or less, more preferably 17 parts by weight or less, and particularly preferably 15 parts by weight or less.
[0123] The resin component (D) is preferably a thermosetting resin. When the resin component (D) is melt-kneaded with the thermoplastic resin (B) or (B-2) as the matrix resin, the resin component (D) is preferably a thermosetting resin because it can be prevented from melting and reducing the shrinkage.
[0124] <Molding products>
[0125] The fiber-reinforced resin molded article of the present invention is a molded article comprising reinforcing fibers (A') and a thermoplastic resin (B), and contains 1 to 30 parts by weight of the reinforcing fibers (A') and 70 to 99 parts by weight of the thermoplastic resin (B) based on 100 parts by weight of the total of (A') and (B).
[0126] [Reinforcement fibers contained in molded products]
[0127] The weight average fiber length Lw(A') of the reinforcing fiber (A') contained in the molded product is 0.1 to 2.9 mm, preferably 0.3 to 2.5 mm, and more preferably 0.5 to 2.0 mm. By setting the weight average fiber length of the reinforcing fiber (A') to 0.1 mm or more, the mechanical properties of the molded product can be fully exhibited. On the other hand, by setting the weight average fiber length of the reinforcing fiber to 2.9 mm or less, the fluidity during molding can be improved, and the poor appearance of the molded product can be suppressed.
[0128] Here, the "weight average fiber length" in the present invention refers to the weight average fiber length calculated by the following formula by applying the calculation method of the weight average molecular weight to the calculation of the fiber length, not simply obtaining the number average value, but taking into account the contribution of the fiber length. The following formula is applicable to the case where the fiber diameter and density of the reinforcing fiber (A') are constant.
[0129] Weight average fiber length = Σ(Mi 2 ×Ni) / Σ(Mi×Ni)
[0130] Mi: Fiber length (mm)
[0131] Ni: Number of reinforcing fibers with a fiber length of Mi
[0132] The above-mentioned weight-average fiber length can be measured by the following method. Using an optical microscope with a hot stage, a test piece is appropriately cut out from the molded product, and the test piece is heated between glass plates on a hot stage appropriately set at 150 to 350°C in accordance with the melting temperature of the thermoplastic resin (B) used, so as to form a thin film so that it is evenly dispersed. In the state where the thermoplastic resin (B) has been melted, it is observed with an optical microscope (50 to 200 times). The fiber lengths of 1000 randomly selected reinforcing fibers (A') are measured, and the weight-average fiber length Lw(A') is calculated by the above formula. Alternatively, the test piece cut out from the molded product is placed in a solvent in which the thermoplastic resin (B) is dissolved, and appropriately heated to prepare a solution in which the reinforcing fibers (A') are evenly dispersed. Thereafter, the solution is filtered, and the reinforcing fibers (A') dispersed on the filter paper are observed with an optical microscope (50 to 200 times). The fiber lengths of 1000 randomly selected reinforcing fibers (A') are measured, and the weight average fiber length (LwA') is calculated by the above formula. In addition, as the filter paper used at this time, quantitative filter paper (model: No. 5C) manufactured by ADVANTECH can be cited.
[0133] The type of reinforcing fiber (A') is not particularly limited, and examples thereof include the reinforcing fibers described in the description of the reinforcing fiber (A) of the molding material. The types and combinations of preferred reinforcing fibers are also the same, and the reasons for their preference are also the same.
[0134] The reinforcing fiber (A') is preferably 1 to 30 parts by weight relative to 100 parts by weight of (A) and (B). More preferably, it is 5 to 25 parts by weight. When the reinforcing fiber is less than 1 part by weight, the mechanical properties of the resulting molded product may sometimes become insufficient, and when it exceeds 30 parts by weight, the appearance of the molded product may sometimes become poor.
[0135] In addition, the reinforcing fibers (A') preferably include bundled reinforcing fibers (A-2') composed of 10 or more monofilaments having a length of 0.5 to 2.9 mm. The effect when the bundled reinforcing fibers (A-2') are included is the same as the reason described in the description of the bundled reinforcing fibers (A-2) of the molding material.
[0136] By setting the weight average fiber length of the bundled reinforcing fibers (A-2') to 0.5 mm or more, the mechanical properties of the molded product can be fully exhibited. On the other hand, by setting the weight average fiber length of the bundled reinforcing fibers (A-2') to 2.9 mm or less, the fluidity during molding can be improved, and the appearance defects of the molded product can be suppressed. It is more preferably 0.3 to 2.5 mm, and particularly preferably 0.5 to 2.0 mm.
[0137] The reinforcing fibers (A') in the present invention preferably have a fiber length of 0.3 to 1.0 mm and a ratio of 40% or more. The fiber length ratio of the reinforcing fibers (A') can be calculated by measuring the distribution of 400 reinforcing fibers (A') taken out from the molded product. By making the ratio of reinforcing fibers having a fiber length of 0.3 to 1.0 mm 40% or more, the fiber length of the reinforcing fibers (A') contained in the molded product can be increased, so that the mechanical properties and dimensional stability of the molded product are excellent.
[0138] The molded article of the present invention preferably contains 1 to 50 parts by weight of bundled reinforcing fibers (A-2') relative to 100 parts by weight of reinforcing fibers (A'). If the content of the bundled reinforcing fibers (A-2') is less than 1 part by weight, the mechanical properties and dimensional accuracy of the molded article are poor, which is not preferred. If the content of the bundled reinforcing fibers (A-2') exceeds 50 parts by weight, the mechanical properties are poor, which is not preferred.
[0139] The molded product of the present invention is a fiber-reinforced thermoplastic resin molded product with excellent mechanical properties and dimensional accuracy. As the use of the molded product composed of the molding material of the present invention, it is extremely useful as a component of electrical / electronic machinery, household electrical appliances, automobiles, and parts for sports purposes. As for electrical / electronic machinery parts, it is suitable for electronic components represented by frames, connectors, speakers, microphones, headphones, small motors, computer-related parts, etc. of televisions, videotape players, DVD players, cameras, audio equipment, etc. For household electrical appliances, it can be listed: VTR parts, television parts, irons, hair dryers, rice cooker parts, microwave oven parts, audio parts, audio equipment, laser discs (registered trademarks), optical discs, DVDs and other audio and video machine parts, lighting parts, refrigerator parts, air conditioner parts, typewriter parts, word processor parts, etc. In addition, as for optical instruments and precision machinery related parts, it can be listed: office computer related parts, telephone related parts, fax machine related parts, copier related parts, binoculars, cameras, clocks, etc. Examples of automobile parts and vehicle-related parts include door pads, pillars, console boxes, various motor housings, roof rails, fenders, garnishes, bumpers, door panels, roof panels, hood panels, trunk lids, door mirror stays, spoilers, hood louvers, wheel covers, grille cover frames, lamp bezels, door handles, door moldings, rear quarter panels, wipers, and the like. In addition, the composition of the present invention is also suitable as sports equipment, and can be suitably used in: golf clubs and shafts, grips, golf balls and other golf-related products, tennis rackets and tennis balls, badminton rackets and their strings and racket sports related products such as badminton, sports body protection products such as masks, helmets, chest protectors, elbow pads, knee pads for American football, baseball, softball, etc., shoe-related products such as sole materials for sports shoes, fishing rods, reels, lures and other fishing tackle-related products, summer sports-related products such as surfing, winter sports-related products such as skis and snowboards, and other indoor and outdoor sports-related products.
[0140] [Example]
[0141] The present invention will be described in more detail below by showing examples, but the present invention is not limited to the description of these examples. First, the evaluation methods of various characteristics used in the present examples will be described.
[0142] (1) Weight average fiber length
[0143] The test piece cut out from the molded product is placed in a solvent in which the thermoplastic resin (B) used in each example and comparative example is dissolved, and appropriately heated to obtain a solution in which the reinforcing fiber (A) is uniformly dispersed. Thereafter, the solution is filtered using a quantitative filter paper (No. 5C) manufactured by ADVANTECH, and the reinforcing fibers (A) dispersed on the filter paper are observed under an optical microscope (50 to 200 times). The fiber lengths of 1,000 randomly selected reinforcing fibers (A) are measured, and the weight average fiber length (Lw) is calculated by the following formula.
[0144] Average fiber length = Σ(Mi 2 ×Ni) / Σ(Mi×Ni)
[0145] Mi: Fiber length (mm)
[0146] Ni: The number of fibers with a fiber length of Mi
[0147] (2) Charpy impact strength measurement of molded products
[0148] The parallel portion of the ISO dumbbell-shaped test piece obtained in each example and comparative example was cut out and subjected to a Charpy impact test with a V-notch according to ISO179 using a C1-4-01 tester manufactured by Tokyo Testing Machine Inc. The impact strength (kJ / cm 2 ).
[0149] (3) Determination of flexural modulus of molded products
[0150] For the ISO dumbbell-shaped test piece obtained by injection molding the molding material, the bending properties were measured according to ISO178 (1993). Using a 3-point bending test fixture (indenter radius 5 mm), the fulcrum distance was set to 64 mm, and the bending elastic modulus was measured under the test conditions of a test speed of 2 mm / min. As a testing machine, "INSTRON (registered trademark)" universal testing machine 5566 (manufactured by INSTRON Corporation) was used.
[0151] (4) Dimensional evaluation of molded products (evaluation of warpage)
[0152] For the 80mm×80mm×1mm thick test piece obtained in each embodiment and comparative example, the difference (t2-t1) between the height (t1) of the central part of the test piece when viewed from the side and the height (t2) of the end portion viewed from the side was evaluated. Three measurements were performed for each test piece, and the average value was used for the evaluation of each embodiment and comparative example. The following criteria were used for judgment, and A and B were considered qualified.
[0153] A: (t2-t1) = less than 3 mm
[0154] B: (t2-t1) = less than 5 mm
[0155] C: (t2-t1) = 5 mm or more
[0156] (5) Evaluation of fluidity (spiral flow length)
[0157] The molding material was molded by an injection molding machine using a mold of 10 mm width and 2 mm t under the temperature conditions shown in the embodiment, an injection speed of 100 mm / sec, and an injection pressure of 80 MPa, and the flow length during the molding was measured. The flow length is the average value of 20 shots. The average value is used in the evaluation of each embodiment and comparative example, and the following criteria are used for judgment, and A and B are regarded as qualified.
[0158] A: 100mm or more
[0159] B: 50mm or more
[0160] C: less than 50mm
[0161] Reference Example 1
[0162] Preparation of reinforcing fiber (A-1) (carbon fiber (A-1))
[0163] The copolymer mainly composed of polyacrylonitrile was spun, calcined, and surface-oxidized to obtain 24,000 single filaments, 7 μm single fiber diameter, 1.6 g / m3 mass per unit length, and 1.8 g / cm3 specific gravity. 3 , a continuous carbon fiber having a surface oxygen concentration ratio [O / C] of 0.2. The continuous carbon fiber has a strand tensile strength of 4,880 MPa and a strand tensile elastic modulus of 225 GPa. Next, a sizing agent mother solution is prepared by dissolving glycerol polyoxypropylene ether as a multifunctional compound in water to a 2% by weight, and the sizing agent is applied to the carbon fiber by an impregnation method and dried at 230°C. The carbon fiber thus obtained has a sizing agent attachment amount of 1.0% by weight.
[0164] Reference Example 2
[0165] Preparation of bundled reinforcing fibers (A-2)-(1)
[0166] 200g of the crushed and classified waste CFRP (CFRP: carbon fiber reinforced plastic) sheets were evenly spread on a metal plate and placed in an electric muffle furnace with an internal volume of 59 liters. While nitrogen was introduced into the furnace, the treatment temperature was maintained at a specific temperature (400°C) for a treatment time of 1 hour for heat treatment. Subsequently, while air was introduced into the furnace, the treatment temperature was maintained at a specific temperature (300°C) for a treatment time of 1 hour for heat treatment to obtain recycled carbon fiber chopped yarn. The obtained resin component (D) was measured, and the result showed that 10 parts by weight of thermosetting resin was attached.
[0167] Reference Example 3
[0168] Preparation of bundled reinforcing fibers (A-2)-(2)
[0169] 200g of the crushed and classified waste CFRP sheets were evenly spread on a metal plate and placed in an electric muffle furnace with an internal volume of 59 liters. While nitrogen was introduced into the furnace, the treatment temperature was maintained at a specific temperature (500°C) for a treatment time of 2 hours for heat treatment. Subsequently, air was introduced into the furnace and the treatment temperature was maintained at a specific temperature (300°C) for a treatment time of 2 hours for heat treatment to obtain recycled carbon fiber chopped yarn. The obtained resin component (D) was measured, and the result showed that 5 parts by weight of thermosetting resin was attached.
[0170] Reference Example 4
[0171] Preparation of polyphenylene sulfide (B-2)
[0172] In a 20-liter autoclave equipped with a stirrer, 2383 g (20.0 mol) of a 47% by mass sodium hydrosulfide aqueous solution, 848 g (20.4 mol) of sodium hydroxide (purity 96% by mass), 3271 g (33 mol) of N-methyl-2-pyrrolidone (NMP), 541 g (6.6 mol) of sodium acetate, and 3000 g of ion-exchanged water were added, and the mixture was gradually heated to 225° C. over about 3 hours while nitrogen was passed under normal pressure. After 4200 g of water and 80 g of NMP were distilled off, the reaction vessel was cooled to 150° C. The amount of hydrogen sulfide scattered per 1 mol of the sodium hydrosulfide added was 0.018 mol. Next, add 2940 g (20 mol) of p-dichlorobenzene (p-DCB) and 2620 g (26.2 mol) of NMP, seal the reaction vessel under nitrogen, stir at 400 rpm, heat up to 227°C at a rate of 0.8°C / min, then heat up to 270°C at a rate of 0.6°C / min, and keep at 270°C for 170 minutes. Then cool to 180°C at a rate of 0.4°C / min, and then cool to near room temperature. Take out the contents, dilute with 10 liters of NMP, filter and separate the solvent and solids with a sieve (80mesh), wash the obtained particles several times with 20 liters of warm water, filter and separate to obtain polyphenylene sulfide (B-1). Dry it with hot air at 80°C and dry it under reduced pressure at 120°C.
[0173] <Bundle-shaped reinforcing fibers (A-2)>
[0174] (Carbon fiber (A-2)-(3))
[0175] Carbon fiber "Torayca" cut fiber TV14-006 (manufactured by Toray Industries, Inc.) was used.
[0176] <Thermoplastic resin (B)>
[0177] (B-1)
[0178] A polycarbonate resin ("Panlite" (registered trademark) L-1225L, manufactured by Teijin Chemicals, Ltd.) was used.
[0179] (B-2)
[0180] The polyphenylene sulfide resin prepared in Reference Example 4 was used.
[0181] (B-3)
[0182] A pellet obtained by blending a polypropylene resin ("Prime Polypro" (registered trademark) J137 manufactured by PRIME POLYMER CO., LTD.) and a maleic acid-modified polypropylene resin ("Admer" (registered trademark) QE840 manufactured by Mitsui Chemicals, Inc.) at a weight ratio of 85 / 15 was used.
[0183] (B-4)
[0184] Polyamide 610 resin (nylon 610 resin "AMILAN" (registered trademark) CM2001) was used.
[0185] <Compound (E)>
[0186] (E-1)
[0187] An epoxy resin (manufactured by Mitsubishi Chemical Corporation, "jER" 828) was used.
[0188] (E-2)
[0189] A terpene resin ("Clearon M105" manufactured by Yasuhara Chemical Co., Ltd.) was used.
[0190] (E-3)
[0191] A terpene phenol resin ("YS Polystar N125" manufactured by Yasuhara Chemical Co., Ltd.) was used.
[0192] (Example 1)
[0193] A long fiber reinforced resin pellet manufacturing apparatus having a coating die for wire resin coating method provided at the tip of a TEX-30α twin-screw extruder (screw diameter 30 mm, L / D = 32) manufactured by Nippon Steel Works, Ltd. was used, and the extruder barrel temperature was set at 230°C, and the polycarbonate resin (B-1) shown above was supplied from the main hopper, and melt kneading was performed at a screw rotation number of 200 rpm. The discharge amount of the compound (E-1) heated and melted at 250°C was adjusted so as to be 6 parts by mass relative to 100 parts by mass of (A) and (B). After (F-1) was discharged and impregnated into a fiber bundle composed of carbon fiber (A-1), a fiber bundle of carbon fiber (A-1) to which the compound (E-1) was applied was supplied to the die (diameter 3 mm) from which the molten polycarbonate resin (B-1) was discharged, and the fiber bundle was continuously arranged so that the polycarbonate resin (B-1) coated the periphery of the carbon fiber (A-1). The internal cross section of the fiber bundle at this time is that at least a portion of the carbon fiber (A-1) is in contact with the polycarbonate resin (B-1). After the obtained strand is cooled, it is cut into a pellet length of 7 mm with a cutter to form a fiber-reinforced thermoplastic resin molding material (X). At this time, the pulling speed is adjusted in such a way that the carbon fiber (A-1) becomes 30 parts by mass relative to a total of 100 parts by mass of (A-1) and (B-1). The length of the carbon fiber (A-1) of the obtained fiber-reinforced thermoplastic resin molding material (X) is substantially the same as the pellet length, and the carbon fiber bundle is parallel to the axial direction of the molding material.
[0194] Next, after supplying the thermoplastic resin (B-1) to the main hopper of another twin-screw extruder (TEX30α manufactured by Nippon Steel Works), the bundled reinforcing fibers (A-2)-(1) are supplied to the molten resin from the side feeder, and the screw rotation number is set to 200 rpm. The strands discharged from the die are cooled in water, cut into 3.0 mm in length by a strand cutter, and pelletized to obtain fiber-reinforced thermoplastic resin molding material (Y-1) pellets. At this time, the amount of bundled reinforcing fibers (A-2)-(2) input is adjusted so that the bundled reinforcing fibers (A-2)-(1) become 30 parts by mass relative to a total of 100 parts by mass of (A-2) and (B-1). Similarly, fiber-reinforced thermoplastic resin molding material (Y-2) pellets containing 10 parts by mass of the bundled reinforcing fibers (A-2)-(1) relative to 100 parts by mass of the total of (A-2) and (B-1) and fiber-reinforced thermoplastic resin molding material (Y-3) pellets containing 5 parts by mass of the bundled reinforcing fibers (A-2)-(1) relative to 100 parts by mass of the total of (A-2) and (B-1) were obtained.
[0195] The fiber-reinforced thermoplastic resin molding materials (X) and (Y-1) thus obtained were dry-blended in the ratio shown in Table 1 to form a mixture of intermediate raw materials, and injection molding was performed using an injection molding machine (J110AD manufactured by The Japan Steel Works, Ltd.) under the conditions of injection time: 2 seconds, back pressure 5 MPa, holding pressure: 40 MPa, holding time: 10 seconds, barrel temperature: 260°C, and mold temperature: 80°C. ISO dumbbell-shaped test pieces of molded products with a thickness of 80 mm × 80 mm × 1 mm were prepared for warpage evaluation and spiral flow length was measured. The composition ratios of (A-1), (A-2) (B) and compound (E) in Table 1 were adjusted in the ratio of dry blending. Here, the barrel temperature refers to the temperature of the portion of the injection molding machine that heats and melts the molding material, and the mold temperature refers to the temperature of the mold into which the resin is injected to form a specific shape. The obtained test piece (molded product) was left to stand for 24 hours in a constant temperature and humidity chamber adjusted to 23° C. and 50% RH, and then subjected to property evaluation. The evaluation results evaluated by the above method are summarized and shown in Table 1.
[0196] (Examples 2 to 5, 11 and 12, Comparative Examples 1 to 4)
[0197] Except having used the ratio of each component described in Table 1 and Table 2, it carried out similarly to the said Example 1, and obtained the molding material and the molding product sheet.
[0198] (Example 6)
[0199] A molding material and a test piece were obtained in the same manner as in Example 1 except that the screw speed of the twin-screw extruder was set to 500 rpm when producing the fiber-reinforced thermoplastic resin molding material (Y).
[0200] (Example 7)
[0201] A molded article was produced and evaluated in the same manner as in Example 1 except that the composition ratio, the type of resin and the type of compound used were changed to those shown in Table 1, and the cylinder temperature was set at 320° C. and the mold temperature was set at 130° C. The evaluation results are summarized in Table 1.
[0202] (Example 8)
[0203] A molded article was produced and evaluated in the same manner as in Example 1 except that the composition ratio, the type of resin or the type of compound used were changed to those shown in Table 1, and the cylinder temperature was set at 220°C and the mold temperature was set at 60°C. The evaluation results are summarized in Table 1.
[0204] (Example 9)
[0205] A molded article was produced and evaluated in the same manner as in Example 1 except that the composition ratio, the type of resin and the type of compound used were changed to those shown in Table 1, and the cylinder temperature was set at 270°C and the mold temperature was set at 60°C. The evaluation results are summarized in Table 1.
[0206] (Example 10)
[0207] A long fiber reinforced resin pellet production device having a coating die for wire resin coating method at the front end of a TEX-30α twin-screw extruder (screw diameter 30 mm, L / D = 32) manufactured by Nippon Steel Works, Ltd. was used, and the extruder barrel temperature was set at 230°C, and the bundled reinforcing fibers (A-2)-(1) and the polycarbonate resin (B-1) shown above were combined, supplied from the main hopper, and melt-kneaded at a screw speed of 200 rpm to form a fiber reinforced resin composition (C-1). The compound (E-1) heated and melted at 250°C was adjusted in discharge amount to 6 parts by mass relative to 100 parts by mass of the total of (A) and (B). Thereafter, (E-1) is discharged, impregnated and imparted to a fiber bundle composed of carbon fiber (A-1), and then a fiber bundle of carbon fiber (A-1) imparted with compound (E-1) is supplied to a die (3 mm in diameter) from which the melted fiber-reinforced resin composition (C-1) is discharged, and the fiber bundle is continuously arranged in such a manner that the fiber-reinforced resin composition (C-1) covers the periphery of the carbon fiber (A-1). The internal cross-section of the fiber bundle at this time is such that at least a portion of the carbon fiber (A-1) is in contact with the fiber-reinforced resin composition (C-1). After the obtained strand is cooled, it is cut into particles with a cutter to form composite long fiber particles of 7 mm in length. At this time, the input amount and the pulling speed of the bundle-shaped reinforcing fiber (A-2)-(1) are adjusted in such a manner that the carbon fiber (A-1) becomes 20 parts by weight and (A-2) becomes 10 parts by weight relative to a total of 100 parts by weight of (A-1) and (B-1). The length of the carbon fiber (A-1) of the obtained composite long fiber pellet is substantially the same as the pellet length, and the carbon fiber bundles are arranged parallel to the axial direction of the molding material. A molded product was prepared and evaluated in the same manner as in Example 1. The evaluation results are summarized in Table 1.
[0208] Examples 1 to 6, 11 and 12 showed excellent results in terms of mechanical properties, dimensional accuracy and fluidity. Even when the resin type and compound type were changed in Examples 7 to 9, the mechanical properties, dimensional accuracy and fluidity were still excellent. Even when the composite long-fiber pellets were used in Example 10, the mechanical properties, dimensional accuracy and fluidity were still excellent.
[0209] On the other hand, Comparative Example 1 does not contain bundled reinforcing fibers (A-2), resulting in poor fluidity. Comparative Example 2 does not contain reinforcing fiber bundles (A-1), resulting in poor impact strength of the molded product. Comparative Example 3 has a small amount of resin component (D) attached to the bundled reinforcing fiber bundles (A-2), so it does not form bundles in the molded product, resulting in poor mechanical properties and dimensional accuracy of the molded product. Furthermore, since it is dispersed in monofilaments, the fiber contacts during injection molding increase, hindering the flow of resin, resulting in poor fluidity. Comparative Example 4 uses general chopped yarn, so it does not form bundles in the molded product, resulting in poor mechanical properties and dimensional accuracy of the molded product. Furthermore, since it is dispersed in monofilaments, the fiber contacts during injection molding increase, hindering the flow of resin, resulting in poor fluidity.
[0210]
[0211]
[0212] Description of Reference Numerals
[0213] 1: Reinforcement fiber (A-1)
[0214] 2: Thermoplastic resin (B)
[0215] 3: Bundle reinforcement fiber (A-2)
Claims
1. A fiber-reinforced resin molding material, comprising a reinforcing fiber (A) and a thermoplastic resin (B), The fiber-reinforced resin molding material comprises 1 to 30 parts by weight of reinforcing fiber (A) and 70 to 99 parts by weight of thermoplastic resin (B) based on 100 parts by weight of the total of (A) and (B). The reinforcing fibers (A) include reinforcing fibers (A-1) and bundled reinforcing fibers (A-2). The length of the reinforcing fiber (A-1) is 3 to 15 mm, and the reinforcing fiber (A-1) is aligned with the longitudinal direction of the molding material, and the length of the reinforcing fiber (A-1) is the same as the length of the longitudinal direction of the molding material. The bundled reinforcing fibers (A-2) are composed of 10 or more single fibers each having a length of 0.5 to 2.9 mm.
2. The fiber-reinforced resin molding material according to claim 1, The fiber-reinforced resin molding material comprises a fiber-reinforced resin molding material (X) and a fiber-reinforced resin molding material (Y), The fiber-reinforced resin molding material (X) comprises reinforcing fibers (A-1) and a thermoplastic resin (B-1). The longitudinal directions of the reinforcing fibers (A-1) and the fiber-reinforced resin molding material (X) are aligned. The fiber-reinforced resin molding material (Y) contains bundled reinforcing fibers (A-2) and a thermoplastic resin (B-2).
3. The fiber-reinforced resin molding material according to claim 1, The fiber-reinforced resin molding material has a core-sheath structure. The core structure of the core-sheath structure comprises reinforcing fibers (A-1), and the reinforcing fibers (A-1) are oriented in the same direction as the length direction of the molding material. The sheath structure of the core-sheath structure is a fiber-reinforced resin composition (C) comprising bundled reinforcing fibers (A-2) and a thermoplastic resin (B), The sheath structure covers the core structure.
4. The fiber-reinforced resin molding material according to claim 1, wherein the reinforcing fibers (A-1) and the bundled reinforcing fibers (A-2) are both carbon fibers.
5. The fiber-reinforced resin molding material according to claim 2, wherein the content of the reinforcing fibers (A-1) and the bundled reinforcing fibers (A-2) is: The reinforcing fibers (A-1) are contained in an amount of 50 to 99 parts by weight, and the bundled reinforcing fibers (A-2) are contained in an amount of 1 to 50 parts by weight. 6 . The fiber-reinforced resin molding material according to claim 1 , wherein the resin component (D) adheres to the fiber bundle surface of the bundled reinforcing fibers (A-2).
7. The fiber-reinforced resin molding material according to claim 6, wherein the resin component (D) is a thermosetting resin. The resin component (D) is contained in an amount of 7 parts by weight or more based on 100 parts by weight of the bundled reinforcing fibers (A-2). 8 . The fiber-reinforced resin molding material according to claim 1 , wherein the thermoplastic resin (B) comprises at least one selected from the group consisting of polyamide resin, polycarbonate resin, polyphenylene sulfide resin, and polypropylene resin.
9. A fiber-reinforced resin molded product comprising reinforcing fibers (A') and a thermoplastic resin (B), The fiber-reinforced resin molded article contains 1 to 30 parts by weight of reinforcing fiber (A') and 70 to 99 parts by weight of thermoplastic resin (B) based on 100 parts by weight of the total of (A') and (B). The weight average fiber length Lw(A') of the reinforcing fiber (A') is 0.1 to 2.9 mm, The reinforcing fibers (A') include bundled reinforcing fibers (A-2') composed of 10 or more single fibers each having a length of 0.5 to 2.9 mm. 10 . The fiber-reinforced resin molded article according to claim 9 , wherein the proportion of reinforcing fibers (A′) having a fiber length of 0.3 to 1.0 mm is 40% or more. 11 . The fiber-reinforced resin molded article according to claim 10 , comprising 1 to 50 parts by weight of the bundled reinforcing fibers (A-2′) based on 100 parts by weight of the reinforcing fibers (A′).
12. The fiber-reinforced resin molded article according to claim 9, wherein the reinforcing fiber (A') is a carbon fiber. 13 . The fiber-reinforced resin molded article according to claim 9 , wherein the resin component (D) adheres to the fiber bundle surface of the bundled reinforcing fibers (A-2′).
14. The fiber-reinforced resin molded article according to claim 13, wherein the resin component (D) is a thermosetting resin. The resin component (D) is contained in an amount of 7 parts by weight or more based on 100 parts by weight of the bundled reinforcing fibers (A-2'). 15 . The fiber-reinforced resin molded article according to claim 9 , wherein the thermoplastic resin (B) comprises at least one selected from the group consisting of polyamide resins, polycarbonate resins, polyphenylene sulfide resins, and polypropylene resins.
Citation Information
Cited By
Beam prefabricated part preparation device for guiding steel fibers through multi-fiber synergistic magnetic force
CN119526541A