Ethylene polymer composition and use thereof

By adding ethylene polymers and carbon fibers with suitable intrinsic viscosity to the ethylene polymer, and using multi-stage polymerization method and surface treatment technology, the ethylene polymer composition in the prior art has been solved in forming, conductivity, and wear resistance in the ethylene polymer composition in the prior art. The deficiencies in terms of loss and heat resistance have achieved the advantages of high-performance ethylene polymer composition and its molded body.

CN118922487APending Publication Date: 2024-11-08MITSUI CHEMICALS INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380026480.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-31
Filing Date
2023-03-28
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The conventional ethylene polymer composition has shortcomings in formability, rigidity, conductivity, wear resistance and heat resistance, and it is difficult to meet the requirements of excellent performance at the same time.

Method used

By combining an ethylene-based polymer component with an intrinsic viscosity of 1.5 to 10 dl/g and 1 to 100 parts by mass of carbon fiber, a multi-stage polymerization method and surface treatment technology can be used to form excellent formability, conductivity, wear resistance and resistance. Thermal ethylene polymer composition.

Benefits of technology

The ethylene polymer composition has been achieved with excellent forming properties, and a molded body with excellent rigidity, electrical conductivity, wear resistance and heat resistance is obtained, which is suitable for a variety of industrial and daily necessities.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005034505550000221
    Figure BDA0005034505550000221
  • Figure HDA0005034505570000011
    Figure HDA0005034505570000011
Patent Text Reader

Abstract

This ethylene-based polymer composition contains: 100 parts by mass of an ethylene-based polymer component (A) having an intrinsic viscosity [eta] of 1.5-10 dl / g and a density of 930-980 kg / m3 as measured in a decalin solvent at 135 DEG C; and 1-100 parts by mass of carbon fibers (B). The ethylene-based polymer component (A) contains an ultra-high molecular weight ethylene-based polymer (a1) having an intrinsic viscosity [eta] of 10-40 dl / g as measured in a decalin solvent at 135 DEG C.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to ethylene polymer compositions and uses thereof. Background Art

[0002] Polyethylene resin is widely used as a molding material because it is easy to shape, has excellent various physical properties, and is economical. For example, Patent Document 1 discloses a high-density polyethylene resin composition containing a high-density polyethylene resin and a layered silicate, and an injection molded product of the composition. In addition, Patent Document 2 discloses a resin composition composed of a polyolefin resin (polyethylene resin, polypropylene resin, etc.), multilayer carbon nanotubes and an inorganic filler, and a molded product of the composition.

[0003] On the other hand, Patent Document 3 discloses an ethylene-based polymer comprising an ultra-high molecular weight polyethylene and a low molecular weight or high molecular weight polyethylene, and an ethylene-based polymer composition containing carbon nanotubes, and states that: the surface resistivity and volume resistivity of the resin composition are low, and it has good thermal conductivity; and the molded body obtained from the ethylene-based polymer composition has good sliding properties and rigidity.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Publication No. 2014-19733

[0007] Patent Document 2: Japanese Patent Application Publication No. 2010-196012

[0008] Patent Document 3: International Publication No. 2022 / 038941 Summary of the invention

[0009] Problems to be solved by the invention

[0010] However, conventional ethylene polymer compositions containing inorganic fillers and carbon nanotubes do not necessarily have sufficient moldability, and there is still room for further improvement from the perspective of obtaining molded products having excellent rigidity, conductivity, wear resistance and heat resistance.

[0011] Therefore, an object of the present invention is to provide an ethylene polymer composition having excellent moldability and capable of obtaining a molded product having excellent rigidity, conductivity, abrasion resistance and heat resistance, and a molded product thereof.

[0012] Methods for solving problems

[0013] Examples of the present invention are shown below.

[0014] [1] An ethylene polymer composition comprising: an intrinsic viscosity [η] of 1.5 to 10 dl / g as measured in a decalin solvent at 135° C. and a density of 930 to 980 kg / m 3 100 parts by weight of an ethylene polymer component (A) and 1 to 100 parts by weight of carbon fibers (B),

[0015] The ethylene polymer component (A) comprises an ultrahigh molecular weight ethylene polymer (a1) having an intrinsic viscosity [η] of 10 to 40 dl / g as measured in a decalin solvent at 135°C.

[0016] [2] According to the ethylene polymer composition described in item [1], the above-mentioned ethylene polymer component (A) contains a low molecular weight or high molecular weight ethylene polymer (a2) having an intrinsic viscosity [η] of 0.1 to 9 dl / g measured in a decalin solvent at 135°C.

[0017] [3] The ethylene polymer composition according to item [2], wherein the ethylene polymer component (A) comprises 10 to 90% by mass of an ethylene polymer component (AI) and 90 to 10% by mass of an ethylene polymer component (AII) (the total amount of component (AI) and component (AII) being 100% by mass);

[0018] The ethylene polymer component (AI) is a multistage polymer, comprising: more than 35% by mass and less than 90% by mass of the ultrahigh molecular weight ethylene polymer (a1), and more than 10% by mass and less than 65% by mass of the low molecular weight or high molecular weight ethylene polymer (a2) (the total amount of the polymer (a1) and the polymer (a2) is 100% by mass),

[0019] The ethylene polymer component (AII) contains an ethylene polymer (a3) ​​having an intrinsic viscosity [η] of 0.1 to 2.9 dl / g as measured in a decalin solvent at 135°C.

[0020] [4] According to the ethylene polymer composition described in item [3], the above-mentioned ethylene polymer component (AI) is obtained by a multi-stage polymerization method, and the multi-stage polymerization method includes: a step of generating the above-mentioned ultra-high molecular weight ethylene polymer (a1), and a step of generating the above-mentioned low molecular weight or high molecular weight ethylene polymer (a2).

[0021] [5] The ethylene polymer composition according to any one of items [1] to [4], wherein the carbon fiber (B) is a surface-treated carbon fiber.

[0022] [6] According to the ethylene polymer composition described in item [5], the surface treatment of the above-mentioned carbon fiber (B) is a sizing treatment using an olefin polymer, a urethane polymer, a nylon polymer or an epoxy polymer.

[0023] [7] The ethylene polymer composition according to any one of items [1] to [6], wherein the average fiber length of the carbon fiber (B) extracted from the ethylene polymer composition is greater than or equal to 100 μm and less than or equal to 400 μm.

[0024] [8] According to any one of items [1] to [7], the proportion of carbon fibers having a fiber length of greater than 100 μm and less than 300 μm in the carbon fibers (B) extracted from the ethylene polymer composition is greater than 30%.

[0025] [9] The ethylene polymer composition according to any one of items [1] to [8], comprising a modified olefin polymer (C).

[0026]

[10] The ethylene polymer composition according to any one of items [1] to [9], wherein the content of the carbon fiber (B) is 20 to 60 parts by mass relative to 100 parts by mass of the ethylene polymer component (A).

[0027]

[11] A molded article comprising the ethylene polymer composition according to any one of items [1] to

[10] .

[0028]

[12] The molded article according to item

[11] , wherein the proportion of carbon fibers having an acicular ratio of 1.5 or more in the carbon fibers (B) contained in the molded article is 30% or more.

[0029]

[13] The molded article according to item

[11] or

[12] , wherein the shrinkage rates in the longitudinal direction and the width direction of the molded article are both 2.0% or less.

[0030]

[14] The molded article according to any one of items

[11] to

[13] , wherein the bending modulus of the molded article is 5000 MPa or more.

[0031]

[15] The molded body according to any one of items

[11] to

[14] , wherein the number of repetitions when the displacement of the molded body in a vibration fatigue test (35 MPa) reaches 8 mm is 1500 or more.

[0032]

[16] The molded article according to any one of items

[11] to

[15] , which is an injection molded article.

[0033]

[17] The molded article according to any one of items

[11] to

[16] , which is a coating material or a sliding material.

[0034] Effects of the Invention

[0035] According to the present invention, there are provided an ethylene polymer composition having excellent moldability and capable of obtaining a molded product having excellent rigidity, electrical conductivity, abrasion resistance and heat resistance, and a molded product thereof. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] [ Figure 1 ] Figure 1 This is a schematic diagram for explaining the position where a sample for observation is collected from an ASTM D671 Type A test piece (molded body) and the observation surface of the sample for observation when evaluating orientation in Examples. DETAILED DESCRIPTION

[0037] Hereinafter, the present invention will be described in detail. It should be noted that in the present specification, a numerical range expressed using "to" means a range including the numerical values ​​described before and after "to" as the lower limit and the upper limit.

[0038] The ethylene polymer composition of the present invention (hereinafter also referred to as "the composition of the present invention") is characterized by comprising: an intrinsic viscosity [η] of 1.5 to 10 dl / g and a density of 930 to 980 kg / m 3 100 parts by mass of an ethylene polymer component (A) and 1 to 100 parts by mass of carbon fibers (B), wherein the ethylene polymer component (A) comprises an ultra-high molecular weight ethylene polymer (a1) having an intrinsic viscosity [η] of 10 to 40 dl / g.

[0039] In the present invention, the intrinsic viscosity [η] refers to the intrinsic viscosity [η] measured in a decalin solvent at 135° C. unless otherwise specified.

[0040] <Ethylene polymer component (A)>

[0041] The above-mentioned ethylene-based polymer component (A) is a homopolymer of ethylene or a copolymer of ethylene and α-olefin, and is a polymer mainly composed of ethylene, generally referred to as high-pressure low-density polyethylene (HP-LDPE), linear low-density polyethylene (LLDPE), medium-density polyethylene (MDPE), high-density polyethylene (HDPE), ultra-high molecular weight ethylene-based polymers, etc.

[0042] When the ethylene-based polymer component (A) is a copolymer, it may be a random copolymer or a block copolymer.

[0043] The α-olefin copolymerizable with ethylene is preferably an α-olefin having 3 to 20 carbon atoms, and specifically includes propylene, 1-butene, 4-methyl-1-pentene, 1-hexene, 1-heptene, 1-octene, 1-nonene, 1-decene, 1-undecene, 1-dodecene, 1-tridecene, 1-tetradecene, 1-pentadecene, 1-hexadecene, 1-heptadecene, 1-nonadecene, 1-eicosene, 9-methyl-1-decene, 11-methyl-1-dodecene, and 12-ethyl-1-tetradecene, etc. These α-olefins may be used alone or in combination of two or more.

[0044] The ethylene-based polymer component (A) may be a single polymer or a combination (mixture) of two or more ethylene-based polymers.

[0045] The intrinsic viscosity [η] of the ethylene polymer component (A) is 1.5 to 10 dl / g, preferably 2.0 to 8.0 dl / g, and more preferably 2.5 to 7.0 dl / g. When the ethylene polymer component (A) has an intrinsic viscosity [η] within the above range, a molded body having excellent balance of properties such as wear resistance, self-lubricity, impact strength, chemical resistance, appearance and moldability can be obtained from the composition of the present invention.

[0046] The density of the ethylene polymer component (A) (measured according to ASTM D1505) is 930 to 980 kg / m 3 , preferably 940~970kg / m 3 When the ethylene polymer component (A) has a density within the above range, a molded product having excellent abrasion resistance and flexibility can be obtained.

[0047] The ethylene polymer component (A) comprises an ultrahigh molecular weight ethylene polymer (a1) having an intrinsic viscosity [η] of 10 to 40 dl / g (hereinafter also referred to as "polymer (a1)"). Since the ethylene polymer component (A) comprises the polymer (a1), a molded body having excellent abrasion resistance, self-lubricity, impact strength, chemical resistance, etc. can be obtained from the composition of the present invention.

[0048] The intrinsic viscosity [η] of the polymer (a1) is preferably 15 to 35 dl / g, more preferably 20 to 35 dl / g.

[0049] The ethylene polymer component (A) may contain a low molecular weight or high molecular weight ethylene polymer (a2) having an intrinsic viscosity [η] of 0.1 to 9 dl / g (hereinafter also referred to as "polymer (a2)"). The polymer (a2) may be a wax.

[0050] The intrinsic viscosity [η] of the polymer (a2) is preferably 0.1 to 5 dl / g, more preferably 0.5 to 3.0 dl / g, particularly preferably 1.0 to 2.5 dl / g.

[0051] The composition of the present invention preferably contains, as the above-mentioned ethylene-based polymer component (A), 10 to 90% by mass of an ethylene-based polymer component (AI) as a multi-stage polymer and 90 to 10% by mass of an ethylene-based polymer component (AII) having an intrinsic viscosity [η] of 0.1 to 2.9 dl / g (the total amount of component (AI) and component (AII) is set to 100% by mass). The multi-stage polymer comprises: more than 35% by mass and less than 90% by mass of the above-mentioned ultra-high molecular weight ethylene-based polymer (a1), and more than 10% by mass and less than 65% by mass of the above-mentioned low molecular weight or high molecular weight ethylene-based polymer (a2) (the total amount of polymer (a1) and polymer (a2) is set to 100% by mass).

[0052] The above-mentioned ethylene polymer component (AI) can preferably be obtained by a multi-stage polymerization method, which includes: a step of generating the above-mentioned ultrahigh molecular weight ethylene polymer (a1) and a step of generating the above-mentioned low molecular weight or high molecular weight ethylene polymer (a2).

[0053] In the multi-stage polymerization method, the polymer (a1) is usually produced in the first stage, and then the polymer (a2) is produced in the second stage.

[0054] The proportion of the above-mentioned ethylene polymer component (AI) is preferably 15 to 90 mass %, more preferably 20 to 80 mass %, and further preferably 26.7 to 49 mass %. The proportion of the above-mentioned ethylene polymer component (AII) is preferably 85 to 10 mass %, more preferably 80 to 20 mass %, and further preferably 73.3 to 51 mass % (the total amount of component (AI) and component (AII) is set to 100 mass %).

[0055] 《Ethylene polymer component (AI)》

[0056] The ultra-high molecular weight ethylene polymer (a1) constituting the ethylene polymer component (AI) can usually be obtained by first-stage polymerization in a multi-stage polymerization method.

[0057] The low molecular weight or high molecular weight ethylene polymer (a2) constituting the ethylene polymer component (AI) can usually be obtained by a second stage polymerization after the polymerization of the polymer (a1) in a multi-stage polymerization method.

[0058] The ethylene polymer component (AI) can be produced by multi-stage polymerization of ethylene and, if necessary, an α-olefin in the presence of a catalyst. The multi-stage polymerization can be carried out by the same method as the polymerization method described in Japanese Patent Application Laid-Open No. 2-289636.

[0059] In addition, by above-mentioned polymer (a1) polymerization, then by above-mentioned polymer (a2) postpolymerization, thereby above-mentioned ethylene polymer component (AI) and above-mentioned ethylene polymer component (AII) have excellent intermiscibility.As a result, in composition of the present invention, above-mentioned ultra-high molecular weight ethylene polymer (a1) is evenly dispersed, and above-mentioned ultra-high molecular weight ethylene polymer (a1) is combined with above-mentioned ethylene polymer component (AII).That is, the interfacial strength between above-mentioned polymer (a1) and above-mentioned ethylene polymer component (AII) improves.Therefore, composition of the present invention, by comprising above-mentioned composition (AI) and above-mentioned composition (AII), thereby the balance of characteristics such as wear resistance, self-lubricating property, impact strength, chemical resistance, outward appearance and formability is excellent, particularly the balance of wear resistance, outward appearance and formability is excellent.

[0060] In the above-mentioned ethylene polymer component (AI), the above-mentioned ultra-high molecular weight ethylene polymer (a1) is contained in an amount preferably exceeding 35 mass % and less than 90 mass %, more preferably exceeding 40 mass % and less than 80 mass %, and further preferably 41 to 75 mass %, and the above-mentioned low molecular weight or high molecular weight ethylene polymer (a2) is contained in an amount preferably exceeding 10 mass % and less than 65 mass %, more preferably exceeding 20 mass % and less than 60 mass %, and further preferably 25 to 59 mass %.

[0061] When the ratio of the polymer (a1) to the polymer (a2) is within the above range, the compatibility between the component (AI) and the component (AII) is improved, and the composition of the present invention is excellent in particular in wear resistance, appearance and moldability.

[0062] The ethylene polymer component (AI) substantially contains only an ultrahigh molecular weight ethylene polymer (polymer (a1)) and a low molecular weight or high molecular weight ethylene polymer (polymer (a2)).

[0063] The above-mentioned component (AI) may also contain additives commonly added to polyolefins (for example, stabilizers such as heat stabilizers and weather stabilizers; cross-linking agents, cross-linking aids, antistatic agents, slip agents, anti-blocking agents, anti-fogging agents, lubricants, dyes, mineral oil-based softeners, petroleum resins, waxes, etc.), and the composition of the present invention may also contain additives added to the above-mentioned component (AI) within the range that does not impair the effects of the present invention.

[0064] The density of the ethylene polymer component (AI) (measured according to ASTM D1505) is usually 930 to 980 kg / m 3 , preferably 940~970kg / m 3 .

[0065] The intrinsic viscosity [η] of the ethylene polymer component (AI) is usually 3.0 to 10.0 dl / g, preferably 3.0 to 8.0 dl / g, and more preferably 3.0 to 7.0 dl / g.

[0066] Since the ethylene polymer component (AI) has the above-mentioned density, the dynamic friction coefficient of the molded body becomes small, and thus a molded body excellent in self-lubricating property can be obtained.

[0067] Furthermore, when the ethylene polymer component (AI) has an intrinsic viscosity [η] within the above range, the dispersion state of the ethylene polymer component (AI) and the ethylene polymer component (AII) becomes good.

[0068] That is, the polymer (a2) contained in the ethylene polymer component (AI) and the ethylene polymer component (AII) melt-mixed by an extruder or the like are finely dispersed with each other, so that the dispersion state becomes uniform. Therefore, by using the ethylene polymer component (AI), a molded body excellent in wear resistance, self-lubricity, impact strength, chemical resistance, appearance, moldability, etc. can be obtained from the composition of the present invention.

[0069] 《Ethylene polymer component (AII)》

[0070] The ethylene polymer component (AII) preferably contains an ethylene polymer (a3) ​​having an intrinsic viscosity [η] of 0.1 to 2.9 dl / g.

[0071] Examples of the ethylene polymer (a3) ​​include high pressure polyethylene (HP-LDPE), linear low density polyethylene (LLDPE), medium density polyethylene (MDPE), high density polyethylene (HDPE), ethylene / α-olefin copolymers, ethylene / vinyl alcohol copolymers, ethylene / vinyl acetate copolymers, ethylene / vinyl acetate copolymer saponification products, ethylene / (meth)acrylic acid copolymers, and ethylene / α-olefin / diene (triene, polyene) terpolymers. Here, examples of α-olefins include propylene, 1-butene, 1-pentene, 1-hexene, 1-octene, 1-decene, 1-dodecene, 4-methyl-1-pentene, and 3-methyl-1-pentene, which have 3 to 20 carbon atoms. In addition, examples of dienes (trienes, polyenes) include 5-ethylidene-2-norbornene and vinyl norbornene, which contain conjugated or non-conjugated dienes, trienes, and polyenes.

[0072] Above-mentioned ethylene-based polymer component (AII) can be a single ethylene-based polymer (a3), or can be a composition of two or more ethylene-based polymers (a3), or can be a composition of ethylene-based polymer (a3) ​​and polyolefin (polypropylene, polybutene, etc.). In addition, above-mentioned ethylene-based polymer component (AII) can also be a wax.

[0073] As the ethylene-based polymer (a3), among the above, high-density polyethylene (HDPE) and low-density polyethylene (LDPE) are preferred, and high-density polyethylene (HDPE) is more preferred.

[0074] The density of the ethylene polymer (a3) ​​(measured according to ASTM D1505) is usually 820 to 980 kg / m 3 , preferably 930~980kg / m 3 , more preferably 950-980 kg / m 3 .

[0075] The intrinsic viscosity [η] of the ethylene polymer (a3) ​​is usually 0.1 to 2.9 dl / g, preferably 0.3 to 2.8 dl / g, more preferably 0.5 to 2.5 dl / g, and further preferably 1.0 to 2.5 dl / g.

[0076] Above-mentioned ethylene polymer component (AII) is owing to comprising above-mentioned ethylene polymer (a3), therefore disperses well when mixing with above-mentioned ethylene polymer component (AI).That is, when utilizing forcing machine etc. to carry out melt mixing, by the mutual fine dispersion of low molecular weight or high molecular weight ethylene polymer (a2) contained in ethylene polymer component (AII) and the ethylene polymer component (AI), thereby dispersed state becomes even.Therefore, by using ethylene polymer component (AI) and ethylene polymer component (AII) as ethylene polymer component (A), can obtain excellent formed bodies such as wear resistance, self-lubricating property, impact strength, chemical resistance, outward appearance, flexibility and formability.

[0077] The above-mentioned component (AII) may also contain additives commonly added to polyolefins (for example, stabilizers such as heat stabilizers and weather stabilizers; cross-linking agents, cross-linking aids, antistatic agents, slip agents, anti-blocking agents, anti-fogging agents, lubricants, dyes, mineral oil-based softeners, petroleum resins, waxes, etc.), and the composition of the present invention may also contain additives added to the above-mentioned component (AII) within the range that does not impair the effects of the present invention.

[0078] <Carbon Fiber (B)>

[0079] The carbon fiber (B) is not particularly limited, and various known carbon fibers can be used, for example, polyacrylonitrile-based, rayon-based, asphalt-based, polyvinyl alcohol-based, regenerated cellulose-based, asphalt-based carbon fibers produced from mesophase asphalt, etc. These can be used alone or in combination of two or more.

[0080] The carbon fibers (B) may be general-purpose fibers or high-strength fibers. In addition, the carbon fibers (B) may be long fibers, short fibers, chopped fibers, or regenerated fibers.

[0081] The carbon fiber (B) is preferably a surface-treated carbon fiber. As a surface treatment method for the carbon fiber, any commonly used known method may be used, for example, a method of electrolytically treating the carbon fiber with an acid or alkaline aqueous solution to impart functional groups to the surface of the carbon fiber; and a method of treating with a sizing agent. Among them, sizing treatment using olefin polymers, epoxy polymers, nylon polymers, and urethane polymers is preferred.

[0082] The average length of the carbon fiber (B), i.e. the average fiber length, is preferably more than 0.1mm and less than 15.0mm, more preferably more than 0.3mm and less than 13.0mm, more preferably more than 0.5mm and less than 13.0mm. When the average fiber length is above the above lower limit, there is a tendency that the mechanical property enhancement effect brought by the carbon fiber can be fully manifested. When the average fiber length is below the above upper limit, there is a tendency that the molded body appearance is made good by dispersing the carbon fiber in the ethylene polymer composition.

[0083] The average fiber length of the carbon fiber (B) extracted from the composition of the present invention is preferably 100 μm or more and 400 μm or less, more preferably 120 μm or more and 380 μm or less, and further preferably 150 μm or more and 360 μm or less. The average fiber length of the carbon fiber (B) extracted from the composition of the present invention is within the above range, so that the processability during the production of the molded body becomes good. On the other hand, if the average fiber length is outside the above range, it is difficult to uniformly mix the carbon fiber and the resin during molding, which sometimes becomes the main reason for the reduction of the physical properties of the composition and the molded body.

[0084] In addition, in the carbon fiber (B) extracted from the composition of the present invention, the proportion of carbon fibers having a fiber length of 100 μm or more and 300 μm or less is preferably 30% or more, more preferably 35 to 99%, and further preferably 40 to 98%. By setting the proportion of carbon fibers having a fiber length of 100 μm or more and 300 μm or less to the above range, the mechanical strength can be improved and a molded body having excellent wear resistance can be obtained.

[0085] The fiber length and average fiber length of the carbon fibers (B) extracted from the composition of the present invention can be determined, for example, by the method described in the examples described below.

[0086] The average diameter of the carbon fiber (B) is preferably 0.5 μm or more and 30 μm or less, more preferably 1 μm or more and 21 μm or less, and further preferably 1 μm or more and 19 μm or less. When the average diameter of the carbon fiber is above the lower limit, the carbon fiber is not easily damaged during molding, and the impact strength of the obtained molded body tends to be improved. When the average diameter of the carbon fiber is below the upper limit, the appearance of the molded body becomes good, and the aspect ratio of the carbon fiber does not decrease, and there is a tendency that the mechanical properties such as rigidity and heat resistance of the molded body can be fully enhanced.

[0087] In the composition of the present invention, if the content of the above-mentioned ethylene polymer component (A) is set to 100 parts by mass, the content of the above-mentioned carbon fiber (B) is 1 to 100 parts by mass, preferably 4 to 70 parts by mass, more preferably 7 to 65 parts by mass, further preferably 10 to 60 parts by mass, and particularly preferably 20 to 60 parts by mass. If the content of the above-mentioned carbon fiber (B) is within the above range, the formability of the composition of the present invention is excellent, and a molded body having excellent rigidity, conductivity, wear resistance, and heat resistance can be obtained from the composition of the present invention.

[0088] Commercially available products of the carbon fiber (B) include, for example, TENAX manufactured by Teijin Co., Ltd. (HT P802 (polyolefin-based polymer sizing agent), HT C605 (nylon-based polymer sizing agent), HT C503 (urethane-based polymer sizing agent)); Torayca staple fiber T008-006 manufactured by Toray Industries, Ltd. (epoxy-based polymer sizing agent); EX-1LC manufactured by Nippon Polymer Industry Co., Ltd. (epoxy-based polymer sizing agent), etc.

[0089] <Modified olefin polymer (C)>

[0090] The composition of the present invention may contain a modified olefin polymer (C).

[0091] The modified olefin-based polymer (C) can be used, for example, as a compatibilizer for improving the compatibility between the ethylene-based polymer component (A) and the carbon fiber (B).

[0092] The modified olefin polymer (C) is not particularly limited, and examples thereof include acid-modified products (e.g., maleic anhydride-modified products), air-oxidized products, or styrene-modified products of homopolymers or copolymers of ethylene and an α-olefin having 3 to 12 carbon atoms. Among these, modified products of polymers selected from the group consisting of ethylene polymers (ethylene homopolymers and copolymers of ethylene and at least one α-olefin selected from α-olefins having 3 to 12 carbon atoms) and propylene polymers (propylene homopolymers and copolymers of propylene and at least one α-olefin selected from α-olefins having 4 to 12 carbon atoms) are preferred.

[0093] Here, examples of the α-olefin (α-olefin having 3 to 12 carbon atoms or α-olefin having 4 to 12 carbon atoms) include propylene, 1-butene, 1-pentene, 1-hexene, 4-methyl-1-pentene, and 1-octene.

[0094] The modified olefin-based polymer (C) is preferably a modified ethylene-based polymer.

[0095] The modified olefin polymer (C) is more preferably a modified ethylene polymer (c11) obtained by graft-modifying the following ethylene polymer (c1) with an unsaturated carboxylic acid or a derivative thereof.

[0096] The above-mentioned ethylene polymer (c1) preferably has a density of 930 to 975 kg / m 3 , and the melt flow rate (MFR) at 190°C and 2.16 kg load measured according to ASTM D1238 is 0.1 to 10 g / 10 minutes, or the melt flow rate (MFR) at 190°C and 10 kg load measured according to ASTM D1238 is 0.1 to 20 g / 10 minutes.

[0097] The density of the ethylene polymer (c1) is preferably 940 to 970 kg / m 3 When the density is within the above range, the compatibility between the ethylene polymer component (A) and the carbon fibers (B) is high.

[0098] The melt flow rate of the ethylene polymer (c1) (according to ASTM D1238, 190°C, 2.16 kg load) is preferably 0.2 to 8 g / 10 min, more preferably 0.5 to 6 g / 10 min, and further preferably 0.5 to 3 g / 10 min. The melt flow rate of the ethylene polymer (c1) (according to ASTM D1238, 190°C, 10 kg load) is preferably 0.1 to 15 g / 10 min, more preferably 0.1 to 10 kg / 10 min, and further preferably 0.1 to 8 g / 10 min. If the melt flow rate is within the above range, the compatibility of the ethylene polymer component (A) and the carbon fiber (B) is high.

[0099] The graft amount of the unsaturated carboxylic acid or its derivative in the modified ethylene polymer (c11) is usually 0.01 to 10% by mass, preferably 0.02 to 10% by mass. When the graft amount is within the above range, the compatibility between the ethylene polymer component (A) and the carbon fiber (B) is high.

[0100] Examples of the unsaturated carboxylic acid or its derivative include unsaturated carboxylic acids and their derivatives such as (meth)acrylic acid, maleic acid, fumaric acid, tetrahydrophthalic acid, itaconic acid, citraconic acid, crotonic acid, isocrotonic acid, and nadic acid (endo-cis-bicyclo[2.2.1]hept-5-ene-dicarboxylic acid), such as acyl halides, amide imides, anhydrous substances, and esters. Specific examples of the derivative include maleic chloride, maleimide, maleic anhydride, citraconic anhydride, monomethyl maleate, dimethyl maleate, glycidyl maleate, methyl (meth)acrylate, ethyl (meth)acrylate, glycidyl (meth)acrylate, monoethyl maleate, diethyl maleate, monomethyl fumarate, dimethyl fumarate, monomethyl itaconate, esters and half esters such as diethyl itaconate. Among these, unsaturated dicarboxylic acids and their anhydrides are preferred, and maleic acid, nadic acid, and their anhydrides are more preferred.

[0101] The modified ethylene polymer (c11) can be produced by various known methods. For example, the following method can be adopted, namely: dissolving the ethylene polymer in an organic solvent, then adding an unsaturated carboxylic acid or its derivative, and a free radical initiator such as an organic peroxide as required to the obtained solution, and reacting at a temperature of usually 60 to 350° C., preferably 80 to 190° C. for 0.5 to 15 hours, preferably 1 to 10 hours; or using an extruder, etc., in the absence of a solvent, adding an ethylene polymer, an unsaturated carboxylic acid or its derivative, and a free radical initiator such as an organic peroxide as required, and reacting at a temperature above the melting point of the ethylene polymer, preferably 160 to 350° C. for 0.5 to 10 minutes.

[0102] The ethylene polymer before modification can be produced by a known method, for example, a high pressure method or a low pressure method using a Ziegler-type Ti-based catalyst, a Co-based catalyst, a metallocene-based catalyst, or the like.

[0103] The ethylene-based polymer (c1) may contain a single ethylene-based polymer or two or more ethylene-based polymers.

[0104] When the ethylene polymer (c1) contains two or more ethylene polymers, the two or more ethylene polymers respectively satisfy the requirements of density and melt flow rate of the ethylene polymer (c1).

[0105] When the composition of the present invention includes the modified olefin polymer (C), if the content of the ethylene polymer component (A) is 100 parts by mass, the content of the modified olefin polymer (C) in the composition of the present invention is preferably 0.1 to 10 parts by mass, more preferably 0.3 to 8 parts by mass, and further preferably 0.5 to 7 parts by mass. If the content of the modified olefin polymer (C) is within the above range, the ethylene polymer component (A) and the carbon fiber (B) can be well compatibilized.

[0106] <Optional Ingredients>

[0107] The ethylene polymer composition of the present invention may, in addition to the above-mentioned ethylene polymer component (A), carbon fiber (B) and modified olefin polymer (C), also contain inorganic fillers other than carbon fiber (B), heat stabilizers, weather stabilizers, ultraviolet absorbers, light stabilizers, waxes, lubricants, slip agents, nucleating agents, anti-blocking agents, antistatic agents, antifogging agents, dyes, dispersants, flame retardants, flame retardant aids, plasticizers, compatibilizers and other various additives commonly used in polyolefins, or impact strength modifiers such as elastomers, polymers such as polyamides, etc., as needed, within the range not impairing the effects of the present invention.

[0108] When the ethylene polymer composition of the present invention contains the above-mentioned additives or polymers, the amount thereof is not particularly limited, and is, for example, in the range of 0.01 to 30% by mass.

[0109] The additive is preferably a wax, and examples of the wax include polyethylene waxes (excluding those corresponding to the above-mentioned ethylene polymer component (AII)) and polypropylene waxes.

[0110] If the ethylene polymer composition of the present invention contains wax, the aggregation of the carbon fibers (B) in the ethylene polymer component (A) can be suppressed, thereby facilitating kneading. It is considered that the carbon fibers (B) are easily dispersed in the ethylene polymer component (A).

[0111] When the ethylene polymer composition of the present invention contains wax, the amount thereof is preferably in the range of 0.01 to 10% by mass based on the amount of the entire composition.

[0112] The MFR of the ethylene polymer composition of the present invention measured at 190°C and a load of 10 kg in accordance with JIS K 7210-1:2014 is preferably 0.01 to 20 g / 10 min, more preferably 0.01 to 10 g / 10 min.

[0113] <Method for producing ethylene polymer composition>

[0114] The ethylene polymer composition of the present invention can be obtained by mixing the above-mentioned ethylene polymer component (A), the above-mentioned carbon fiber (B), any of the above-mentioned modified olefin polymers (C) and any of the above-mentioned arbitrary components by a conventionally known method, for example, dry mixing the components, then melt-kneading them using a single-screw or twin-screw extruder, extruding them in the form of strands and granulating them into pellets.

[0115] The carbon fibers (B) may be mixed in advance with a polymer component such as the ethylene-based polymer component (A) and used in the form of a masterbatch.

[0116] <molded body>

[0117] Shaped article of the present invention comprises above-mentioned ethylene polymer composition.As the manufacture method (forming method) of shaped article, specifically can enumerate known polyolefin forming methods in the past, for example known thermoforming methods such as extrusion molding, injection molding, film forming, inflation molding, blow molding, extrusion blow molding, injection blow molding, compression molding, vacuum forming, powder slush molding (powderslush molding), calendering, foaming.Preferably utilize injection molding that above-mentioned ethylene polymer composition is processed, thereby can obtain the shaped article that comprises above-mentioned ethylene polymer composition.

[0118] The molded article may be a molded article formed from the ethylene-based polymer composition, or may be a molded article having a portion, such as a surface layer, formed from the ethylene-based polymer composition.

[0119] Among the carbon fibers (B) contained in the molded body of the present invention, the proportion of carbon fibers having a needle-like ratio of 1.5 or more is preferably 30% or more, more preferably 30 to 70%, further preferably 31 to 65%, and particularly preferably 32 to 60%. By setting the proportion of carbon fibers having a needle-like ratio of 1.5 or more in the above range, the mechanical strength of the molded body can be improved, and a molded body with excellent rigidity and fatigue resistance can be obtained. The proportion of carbon fibers having a needle-like ratio of 1.5 or more can be obtained by the method described in the examples described later.

[0120] The shrinkage ratios in the longitudinal direction and the width direction of the molded article of the present invention are preferably both 2.0% or less, more preferably 1.5% or less, and even more preferably 0.05 to 1.0%. The shrinkage ratios can be determined by the method described in the Examples below.

[0121] The flexural modulus of the molded article of the present invention is preferably 5000 MPa or more, more preferably 6000 to 20000 MPa, and even more preferably 7000 to 15000 MPa. The flexural modulus can be determined by the method described in the examples below.

[0122] The number of repetitions when the displacement of the molded article of the present invention reaches 8 mm in the vibration fatigue test (35 MPa) is preferably 1500 or more, more preferably 2000 or more, and further preferably 5000 or more. The upper limit of the above number of repetitions is as high as possible, so it is not particularly limited, preferably 10 million times, more preferably 1 million times, and further preferably 500,000 times. The above number of repetitions can be obtained by the method described in the examples described later.

[0123] The molded article can be used in a wide range of applications such as daily necessities, household products such as entertainment, general industrial applications, and industrial products. Specific examples of the molded article include: home appliance material parts, communication equipment parts, electrical parts, electronic parts, automobile parts, other vehicle parts, ships, aircraft materials, mechanical parts, building material-related components, civil engineering components, agricultural materials, electric tool parts, food containers, films, sheets, and fibers.

[0124] The molded body of the present invention can be widely used in the polyethylene applications known in the past, especially because of the excellent balance of properties such as wear resistance, rigidity, self-lubrication, impact strength, and thin-wall molding. Therefore, as applications requiring these, for example, there can be listed: metal coating materials (laminated) such as steel pipes, wires, and automobile sliding door rails; various rubber coating materials (laminated) such as pressure-resistant rubber tubes, automobile door gaskets, clean room door gaskets, automobile glass window guide channel sealing strips, and automobile door and window waterproofing strips; linings for hoppers, chutes, etc.; sliding materials such as gears, bearings, rollers, reels, various guide rails, elevator guide rails, and various protective padding materials, etc.

[0125] Since the molded article of the present invention is also excellent in electrical conductivity, it is possible to suppress the charging of various machine parts and sliding members, and can be suitably used in applications requiring electrical conductivity and antistatic properties.

[0126] Example

[0127] Hereinafter, the present invention will be described in more detail based on Examples, but the present invention is not limited to these Examples at all.

[0128] [Measurement method]

[0129] The methods for measuring the physical properties of the polymers used in Examples, the compositions obtained in Examples, and the molded products produced using the compositions are as follows.

[0130] [Intrinsic viscosity [η]]

[0131] Measured at 135°C in decalin.

[0132] [density]

[0133] The density of the vinyl polymer component (A) was measured by the density gradient method in accordance with ASTM D1505.

[0134] The density of the composition obtained in the examples or comparative examples was measured by the immersion weighing method at 23 °C in water in accordance with JIS Z8807:2012.

[0135] [Fiber analysis of carbon fiber (B) extracted from vinyl polymer composition]

[0136] [Pretreatment]

[0137] The granular composition obtained in the examples or comparative examples was heated in an electric furnace at 500 °C for 30 minutes in an air atmosphere.

[0138] [Image analysis of carbon fiber (B)]

[0139] A part of the ash obtained by the pretreatment was taken out onto a glass slide, spread with oil, covered with a cover glass, and the resulting specimen was set as an observation sample. Using the "Stereo Microscope SZX16" manufactured by Olympus Corporation, the reflected bright field image of the above sample was observed at a lens magnification of 4 times. From the observation field of view, a field of view containing fibers of 100 μm or more was selected, and after obtaining the image, it was analyzed using image analysis software ("WinROOF 2018" manufactured by MITANI Corporation) to calculate the fiber length and number of carbon fibers (B).

[0140] [Average fiber length of carbon fiber (B)]

[0141] Based on the results obtained by the above image analysis, the average fiber length of the carbon fibers contained in the composition was calculated.

[0142] [Ratio of carbon fiber (B) with fiber length of 100 - 300 μm]

[0143] Based on the results obtained by the above image analysis, the fiber ratio of fibers with a fiber length of 100 - 300 μm among all the analyzed fibers was calculated.

[0144] [Orientation]

[0145] [Production of ASTM D671 Type A test piece]

[0146] The composition obtained in the examples or comparative examples was put into the hopper part of the "EC-75SXIII molding machine" manufactured by Shibaura Machine Co., Ltd., melted at 230 °C, and injection molded into a mold to produce a shape as Figure 1ASTM D671 Type A test piece (molded body) of the plate shape having the outer shape shown in the figure. The mold temperature during injection molding was set to 30 to 50°C, the injection pressure was set to 90 to 110 MPa, and the holding pressure was set to 55 to 65 MPa.

[0147] <Preparation of samples for observation>

[0148] against Figure 1 The ASTM D671 Type A test piece (molded body) shown in the schematic diagram is firstly subjected to injection molding along the same direction as the flow direction during injection molding (injection molding direction), that is, Figure 1 The sample collection area is cut in the direction of the AA line in the image. Then, the sample collection area is embedded in resin, the cut surface in the direction of the AA line is polished, and the sample is further cut into a desired thickness using a microtome, and finally carbon vapor deposition is performed to prepare a sample for observation.

[0149] <Observation and Analysis>

[0150] The observation samples were observed using a scanning electron microscope S-3700N manufactured by Hitachi High-Technologies Corporation at an accelerating voltage of 10 kV and a magnification of 150 times. Figure 1 As shown, the polished surface of the part cut from the molded body is set to the front direction, and the observation surface seen from this observation direction is photographed in a manner parallel to the long side on the shooting screen. In the photographed image, the depth of 0.7 to 0.8 mm from the molded body surface (upper surface) is set as the image center.

[0151] After obtaining the image, it was analyzed using image analysis software ("Win ROOF 2018" manufactured by MITANI Corporation). Carbon fibers (CF) were extracted from the image by binarization, and the needle-like ratio of all extracted CFs was calculated and the average value was obtained. The needle-like ratio was calculated from the absolute maximum length of the observed elliptical CF and the ratio of the absolute maximum length to the perpendicular diagonal width (absolute maximum length / diagonal width).

[0152] [Conductivity (surface resistivity, volume resistivity)]

[0153] <Preparation of a Test Specimen of Length 120 mm × Width 130 mm × Thickness 3 mm>

[0154] The composition obtained in the examples or comparative examples was put into the hopper of the "EC-75SXIII type molding machine" manufactured by Shibaura Machine Co., Ltd., melted at 230°C, and injection molded into a mold to produce a test piece of 120 mm in length × 130 mm in width × 3 mm in thickness. The mold temperature was set to 50 to 70°C, the injection pressure was set to 90 to 110 MPa, and the holding pressure was set to 40 to 70 MPa.

[0155] <Measurement of Surface Resistivity and Volume Resistivity>

[0156] Using a test piece of length 120 mm × width 130 mm × thickness 3 mm, the surface resistivity and volume resistivity were measured by the double ring method using a "Digital Ultra High Resistance / Particle Amperemeter 8340A" manufactured by ADC Co., Ltd. under the conditions of 23°C, humidity: 50%, applied voltage: 500 V, and applied time: 60 seconds.

[0157] It should be noted that the surface resistivity in the above measurement is 1.0×10 7 The following levels were measured according to JIS K7194:1994 using "LORESTA-GX-MCP-T700 low resistance resistivity meter" manufactured by Nitto Seiko Analytech Co., Ltd. under the conditions of applied current: 1 mA, application time: 10 seconds, temperature: 23°C, and humidity: 50%.

[0158] [Heat resistance (heat deformation temperature HDT)]

[0159] The heat deformation temperature was determined by setting the test piece shape to the shape described in JIS K7162 1A according to ISO-75-1, 2. The heat deformation temperature was measured when the bending stress was 0.45 MPa (HDT 0.45 MPa) and when the bending stress was 1.80 MPa (HDT 1.80 MPa).

[0160] [Moldability (Molding shrinkage)]

[0161] Using the same method as described above, a test piece with a length of 120 mm × width of 130 mm × thickness of 3 mm was fabricated by injection molding. The dimensional changes of the test piece (length in the length direction and width in the width direction) after 3 days of molding relative to the mold dimensions (length in the length direction and width in the width direction) were calculated, and this was set as the evaluation of formability. Specifically, the molded body (test piece) after injection molding was removed from the mold and left to stand at room temperature for 3 days. Then, for each of the four sides, the differences in the lengths of the sides in the length direction and width direction of the test piece and the lengths of the sides in the length direction and width direction of the injection mold were measured. For each of these four sides, the percentage ratio relative to the difference in the side length of the mold was calculated, and the average value of these percentages was set as the molding shrinkage rate. The molding shrinkage rate in the length direction was set as the shrinkage rate MD, and the molding shrinkage rate in the width direction was set as the shrinkage rate TD.

[0162] [Sliding property (coefficient of kinetic friction) and abrasion resistance (relative wear amount)]

[0163] The test piece with a length of 120 mm × width of 130 mm × thickness of 3 mm fabricated by the same method as described above was punched to produce a test piece with a length of 30 mm × width of 30 mm × thickness of 3 mm. Using this test piece, according to JIS K7218 "Method A for Sliding Wear Test of Plastics", the coefficient of kinetic friction and the relative wear amount were measured using a Matsuyama type friction and wear testing machine.

[0164] The test conditions were set as follows: target material: S45C, speed: 50 cm / second, distance: 3 km, load: 15 kg, measurement ambient temperature: 23 °C.

[0165] [Tensile fracture strength, tensile fracture elongation, and tensile elastic modulus]

[0166] According to ISO 527-1,2, the shape of the test piece was set to the shape described in JIS K7162 1A, the tensile speed was set to 50 mm / minute, and the tensile fracture strength and tensile fracture elongation were obtained. Additionally, according to ISO 527-1,2, the shape of the test piece was set to the shape described in JIS K7162 1A, the tensile speed was set to 1 mm / minute, and the tensile elastic modulus was obtained.

[0167] [Flexural strength, flexural elastic modulus]

[0168] [Fabrication of JIS K7162 1A test piece]

[0169] The composition obtained in the examples or comparative examples was put into the hopper part of the "EC-75SXIII type molding machine" manufactured by Shibaura Machine Co., Ltd., melted at 230 °C, and a JIS K7162 1A test piece was produced by injection molding into a mold. The mold temperature was set to 50 - 70 °C, the injection pressure was set to 80 - 120 MPa, and the holding pressure was set to 60 - 90 MPa. Among them, only in the case of the composition obtained in Comparative Example 1, the injection pressure was changed to 70 - 90 MPa and the holding pressure was changed to 25 - 45 MPa.

[0170] <Measurement of flexural strength and flexural modulus>

[0171] Using the JIS K7162 1A test piece, according to ISO 178, the shape of the above test piece was set to 80 mm (length), 10 mm (width), and 4 mm (thickness), and the flexural strength and flexural modulus were determined with a span distance of 64 mm and a test speed of 2 mm / minute.

[0172] [Flexural fatigue test]

[0173] <Fabrication of ASTM D671 Type A test piece>

[0174] The composition obtained in the examples or comparative examples was put into the hopper part of the "EC-75SXIII type molding machine" manufactured by Shibaura Machine Co., Ltd., melted at 230 °C, and an ASTM D671 Type A test piece was produced by injection molding into a mold. The mold temperature was set to 30 - 50 °C, the injection pressure was set to 90 - 110 MPa, and the holding pressure was set to 55 - 65 MPa.

[0175] <Measurement of vibration fatigue life>

[0176] The ASTM D671 Type A test piece was installed in the "B70 type repeated vibration fatigue testing machine" manufactured by Toyo Seiki Seisaku-sho, Ltd., and a vibration fatigue test was carried out at room temperature, a frequency of 30 Hz, and a pressure of 35 MPa. The number of repetitions when the displacement reached 8 mm was determined as the fatigue resistance (times).

[0177] [Raw materials]

[0178] The raw materials used in the examples or comparative examples are as follows.

[0179] (Ethylene-based polymer component (AI))

[0180] 《Manufacture of ethylene-based polymer component (AI-1)》

[0181] By conventional methods, utilizing two-stage polymerization, a first-stage polymerization is performed at a mass ratio (polymer (a1) / polymer (a2)) of 41 / 59 to generate an ultra-high molecular weight ethylene polymer (polymer (a1)) having an intrinsic viscosity [η] of 30 dl / g, followed by a second-stage polymerization to generate a low molecular weight ethylene polymer (polymer (a2)) having an intrinsic viscosity [η] of 1.5 dl / g, thereby obtaining an ethylene polymer component (AI-1) having an intrinsic viscosity [η] of 4.4 dl / g.

[0182] 《Manufacturing of Ethylene Polymer Component (AI-2)》

[0183] By conventional methods, utilizing two-stage polymerization, a first-stage polymerization is performed at a mass ratio (polymer (a1) / polymer (a2)) of 75 / 25 to generate an ultra-high molecular weight ethylene polymer (polymer (a1)) having an intrinsic viscosity [η] of 30 dl / g, followed by a second-stage polymerization to generate a low molecular weight ethylene polymer (polymer (a2)) having an intrinsic viscosity [η] of 1.5 dl / g, thereby obtaining an ethylene polymer component (AI-2) having an intrinsic viscosity [η] of 6.9 dl / g.

[0184] (Ethylene polymer component (AII))

[0185] The following vinyl polymer components were used.

[0186] Ethylene polymer component (AII-1): intrinsic viscosity [η] 1.1 dl / g, density 965 kg / m 3 High-density low-molecular-weight polyethylene ("HI-ZEX 1700J" manufactured by Prime Polymer Co., Ltd.)

[0187] (Ethylene polymer component (A))

[0188] 《Production of Ethylene Polymer Component (A-1)》

[0189] The ethylene polymer component (AI-1) and the ethylene polymer component (AII-1) were mixed in a mass ratio ((AI-1) / (AII-1)) of 49 / 51, and melt-mixed using a PCM twin-screw extruder manufactured by Ikegai Iron Works to obtain a pellet having an intrinsic viscosity [η] of 3.0 dl / g and a density of 968 kg / m 3 The content of the ultra-high molecular weight ethylene polymer (polymer (a1)) in the ethylene polymer component (A-1) was 20% by mass.

[0190] 《Production of Ethylene Polymer Component (A-2)》

[0191] The ethylene polymer component (AI-2) and the ethylene polymer component (AII-1) were mixed in a mass ratio ((AI-2) / (AII-1)) of 33 / 67 and melt-mixed using a PCM twin-screw extruder manufactured by Ikegai Iron Works to obtain a pellet having an intrinsic viscosity [η] of 5.8 dl / g and a density of 966 kg / m 3 The content of the ultra-high molecular weight ethylene polymer (polymer (a1)) in the ethylene polymer component (A-2) was 25% by mass.

[0192] (Carbon fiber (B))

[0193] The following carbon fibers were used.

[0194] Carbon fiber (B-1): "TENAX HT P802" manufactured by Teijin Limited (polyolefin polymer sizing treatment, fiber length: 3 mm, diameter: 7 μm, carbon fiber ratio: 98 mass %)

[0195] Carbon fiber (B-2): Teijin Limited "TENAX HT C605" (sizing treatment with nylon polymer, fiber length: 6 mm, diameter: 7 μm, carbon fiber ratio: 95.5 mass %)

[0196] Carbon fiber (B-3): Toray Industries, Inc. "TORAYCA T008-006" (epoxy polymer sizing treatment, fiber length: 6 mm, diameter: 7 μm, carbon fiber ratio: 99 mass %)

[0197] (Other carbon-based fillers)

[0198] The following carbon nanotubes were used.

[0199] Carbon nanotubes: NC7000 manufactured by NANOCYL (average diameter: 9.5 nm, average length: 1.5 μm)

[0200] 《Preparation of Carbon Nanotube Masterbatch》

[0201] 15 mass % of the carbon nanotubes, 75 mass % of the ethylene polymer component (A-1) and 10 mass % of wax (polyethylene wax) were mixed by a conventional method to prepare a masterbatch containing carbon nanotubes.

[0202] (Modified olefin polymer (C))

[0203] The following modified olefin polymers were used as compatibilizers.

[0204] Modified olefin polymer (C-1): Maleic acid-modified ethylene polymer (density: 965 kg / m 3 , MFR (190℃, 2.16kg load): 5g / 10min, modification degree: 2.4)

[0205] Modified olefin polymer (C-2): a maleic acid-modified ethylene polymer (density 967 kg / m 3 , intrinsic viscosity [η] 5dl / g [η], MFR (190°C, 10kgf): 6.2, modification degree: 0.8)

[0206] [Example 1]

[0207] After dry mixing with the ratio of 78 mass % of ethylene polymer component (A-1), 20 mass % of carbon fiber (B-1) and 2 mass % of modified olefin polymer (C-1), twin screw compounding extruder "HK-25D" made by Parker Corporation, Co., Ltd. was used to melt extrude and obtain the composition under the conditions of 260 ℃ of barrel temperatures, 200 rpm of screw speeds and 12 kg / h of discharge. The amount of each component in the composition obtained (the total amount of ethylene polymers is set to 100 mass parts.) is as shown in Table 1. In addition, the physical property of the composition obtained was measured by the above method. The result is as shown in Table 1.

[0208] [Example 2]

[0209] The composition was prepared in the same manner as in Example 1, except that the amounts of the ethylene polymer component (A-1), the carbon fiber (B-1), and the modified olefin polymer (C-1) were adjusted to the amounts shown in Table 1, and the physical properties thereof were measured. The results are shown in Table 1.

[0210] [Example 3]

[0211] The composition was prepared in the same manner as in Example 1, except that the modified olefin polymer (C-2) was used instead of the modified olefin polymer (C-1), and the amounts of the ethylene polymer component (A-1), the carbon fiber (B-1), and the modified olefin polymer (C-2) were prepared in the amounts shown in Table 1. The physical properties of the composition were measured. The results are shown in Table 1.

[0212] [Example 4]

[0213] The composition was prepared in the same manner as in Example 1, except that the ethylene polymer component (A-2) was used instead of the ethylene polymer component (A-1), and the amounts of the ethylene polymer component (A-2), the carbon fiber (B-1), and the modified olefin polymer (C-1) were adjusted to the amounts shown in Table 1. The physical properties of the composition were measured. The results are shown in Table 1.

[0214] [Example 5]

[0215] The composition was prepared in the same manner as in Example 1, except that the carbon fiber (B-2) was used instead of the carbon fiber (B-1), and the amounts of the ethylene polymer component (A-1), the carbon fiber (B-2), and the modified olefin polymer (C-1) were adjusted to the blending amounts shown in Table 1. The physical properties were measured. The results are shown in Table 1.

[0216] [Example 6]

[0217] The composition was prepared in the same manner as in Example 1, except that the carbon fiber (B-3) was used instead of the carbon fiber (B-1), and the amounts of the ethylene polymer component (A-1), the carbon fiber (B-3), and the modified olefin polymer (C-1) were adjusted to the blending amounts shown in Table 1. The physical properties were measured. The results are shown in Table 1.

[0218] [Comparative Example 1]

[0219] The composition was prepared in the same manner as in Example 1, except that the ethylene polymer component (AII-1) was used instead of the ethylene polymer component (A-1), and the amounts of the ethylene polymer component (AII-1), the carbon fiber (B-1), and the modified olefin polymer (C-1) were adjusted to the amounts shown in Table 1. The physical properties of the composition were measured. The results are shown in Table 1.

[0220] [Comparative Example 2]

[0221] A composition was prepared in the same manner as in Example 1 except that only the ethylene polymer component (A-1) was used instead of the carbon fiber (B-1) and the modified olefin polymer (C-1). The physical properties of the composition were measured. The results are shown in Table 1.

[0222] [Comparative Example 3]

[0223] After dry mixing with 40 mass % of ethylene polymer component (A-2) and 60 mass % of carbon nanotube masterbatch, a twin screw compounding extruder "HK-25D" manufactured by Parker Corporation was used to melt extrude the composition under the conditions of barrel temperature 260°C, screw speed 200rpm and discharge 12kg / h. The amount of each component in the composition (the total amount of ethylene polymer is set to 100 mass parts) is shown in Table 1. In addition, the physical properties of the obtained composition were measured by the above method. The results are shown in Table 1.

[0224] [Table 1]

[0225]

Claims

1. An ethylene polymer composition comprising: an intrinsic viscosity [η] of 1.5 to 10 dl / g and a density of 930 to 980 kg / m 3 100 parts by weight of an ethylene polymer component (A) and 1 to 100 parts by weight of carbon fibers (B), The ethylene polymer component (A) comprises an ultrahigh molecular weight ethylene polymer (a1) having an intrinsic viscosity [η] of 10 to 40 dl / g as measured in a decalin solvent at 135°C.

2. The ethylene polymer composition according to claim 1, wherein the ethylene polymer component (A) comprises a low molecular weight or high molecular weight ethylene polymer (a2) having an intrinsic viscosity [η] of 0.1 to 9 dl / g as measured in a decalin solvent at 135°C.

3. The ethylene polymer composition according to claim 2, wherein the ethylene polymer component (A) comprises 10 to 90% by mass of an ethylene polymer component (AI) and 90 to 10% by mass of an ethylene polymer component (AII), wherein: The total amount of component (AI) and component (AII) is 100% by mass. The ethylene polymer component (AI) is a multi-stage polymer, which comprises: more than 35% by mass and less than 90% by mass of the ultra-high molecular weight ethylene polymer (a1), and more than 10% by mass and less than 65% by mass of the low molecular weight or high molecular weight ethylene polymer (a2), wherein the total amount of polymer (a1) and polymer (a2) is set to 100% by mass, The ethylene polymer component (AII) contains an ethylene polymer (a3) ​​having an intrinsic viscosity [η] of 0.1 to 2.9 dl / g as measured in a decalin solvent at 135°C.

4. The ethylene polymer composition according to claim 3, wherein the ethylene polymer component (AI) is obtained by a multi-stage polymerization process, the multi-stage polymerization process comprising: A step of producing the ultra-high molecular weight ethylene polymer (a1), and a step of producing the low molecular weight or high molecular weight ethylene polymer (a2). 5 . The ethylene polymer composition according to claim 1 , wherein the carbon fiber (B) is a surface-treated carbon fiber.

6. The ethylene polymer composition according to claim 5, wherein the surface treatment of the carbon fiber (B) is a sizing treatment using an olefin polymer, a urethane polymer, a nylon polymer or an epoxy polymer. 7 . The ethylene polymer composition according to claim 1 , wherein the carbon fibers (B) extracted from the ethylene polymer composition have an average fiber length of 100 μm to 400 μm.

8. The ethylene polymer composition according to any one of claims 1 to 7, wherein the proportion of carbon fibers having a fiber length of 100 μm or more and 300 μm or less in the carbon fibers (B) extracted from the ethylene polymer composition is 30% or more. 9 . The ethylene polymer composition according to claim 1 , comprising a modified olefin polymer (C). 10 . The ethylene polymer composition according to claim 1 , wherein the content of the carbon fiber (B) is 20 to 60 parts by mass based on 100 parts by mass of the ethylene polymer component (A). 11 . A molded article comprising the ethylene polymer composition according to claim 1 . 12 . The molded article according to claim 11 , wherein the proportion of carbon fibers having an acicular ratio of 1.5 or more among the carbon fibers (B) contained in the molded article is 30% or more. 13 . The molded article according to claim 11 , wherein the shrinkage ratios in the longitudinal direction and the width direction of the molded article are both 2.0% or less. 14 . The molded article according to claim 11 , wherein the molded article has a bending elastic modulus of 5000 MPa or more. 15 . The molded body according to claim 11 , wherein the number of repetitions when the displacement amount reaches 8 mm in a vibration fatigue test at 35 MPa is 1500 or more. 16 . The molded article according to claim 11 , which is an injection molded article. 17 . The formed body according to claim 11 , which is a coating material or a sliding material.