Steel member and steel sheet

By forming a decarbonized layer on the surface of the steel component and enriching B elements, combined with hot stamping technology, the problems of stamping forming and collision safety of high-strength steel plates are solved, and steel with high strength, excellent bending and hydrogen embrittlement resistance are achieved. Component, suitable for automotive body parts.

CN118922573APending Publication Date: 2024-11-08NIPPON STEEL CORPORATION
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380029343.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-30
Filing Date
2023-03-30
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Existing high-strength steel plates are difficult to create complex shapes during stamping and are prone to early breakage in collision accidents, unable to fully exert compressive strength and absorption energy, and lack of hydrogen embrittlement resistance.

Method used

By forming a decarbonized layer on the surface of the steel member and enriching elements B, bending and hydrogen embrittlement resistance are improved, and oxide scales are formed on the steel plate to introduce cracks for decarbonization, and a high-strength and good toughness are formed in combination with hot stamping technology to form steel members with high strength and good toughness. .

Benefits of technology

The steel component that achieves high strength, excellent bending and hydrogen embrittlement resistance can show sufficient absorption energy and compressive strength in collision accidents, and is suitable for automotive body parts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005054058260000271
    Figure BDA0005054058260000271
  • Figure BDA0005054058260000281
    Figure BDA0005054058260000281
  • Figure BDA0005054058260000291
    Figure BDA0005054058260000291
Patent Text Reader

Abstract

The steel member has a prescribed chemical composition, and when a position at a depth of 1 / 4 of the thickness from the surface in the thickness direction is denoted as a 1 / 4 depth position, the maximum B content in a range from the surface to a depth of 10 [mu] m in the thickness direction is at least five times the B content at the 1 / 4 depth position. The decarburization depth is 20 [mu] m or more and the Vickers hardness at the 1 / 4 depth position is 310-890 when the C content is measured from the surface in the thickness direction using GDS and the distance from the surface to the position at which the C content reaches the 1 / 4 depth position for the first time is denoted as the decarburization depth.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a steel member and a steel plate.

[0002] This application claims priority based on Japanese Patent Application No. 2022-055819 filed in Japan on March 30, 2022, and the contents are incorporated herein by reference. Background Art

[0003] In the field of automotive steel sheets, the application of steel sheets with high tensile strength (high-strength steel sheets) is expanding in order to improve both fuel efficiency and collision safety, against the backdrop of recent stricter environmental regulations and collision safety standards. However, as the strength increases, the stamping formability of the steel sheet decreases, making it difficult to manufacture products with complex shapes.

[0004] Specifically, as the strength increases, the ductility of the steel sheet decreases, and when it is processed into a complex shape, the problem of fracture at the high processing position arises. In addition, as the strength of the steel sheet increases, there are also problems of springback and wall warping and deterioration of dimensional accuracy due to residual stress after processing. Therefore, it is not easy to stamp a steel sheet with high strength, especially a tensile strength of more than 780MPa, into a product with a complex shape. If roll forming is used instead of stamping, it is easy to process high-strength steel sheets, but its application is limited to parts with the same cross-section along the length direction.

[0005] Therefore, in recent years, hot stamping technology has been used as a technology for stamping hard-to-form materials such as high-strength steel sheets. Hot stamping technology refers to a hot forming technology that heats the material to be formed before forming.

[0006] This technology heats the material before forming it. Therefore, the steel is soft during forming and has good formability. As a result, even high-strength steel plates can be formed into complex shapes with good precision. In addition, hot stamping technology uses stamping dies to quench while forming, so the formed steel components have sufficient strength.

[0007] For example, Patent Document 1 discloses that a tensile strength of 1400 MPa or more can be imparted to a steel member after forming by a hot stamping technique.

[0008] On the other hand, cars are also required to have collision safety. The collision safety of cars is evaluated by the compressive strength and absorbed energy of the entire car body and some of its components in collision tests. In particular, since compressive strength is greatly dependent on material strength, the demand for ultra-high-strength steel components as car components has increased dramatically.

[0009] However, as the steel members are generally strengthened, the fracture toughness and deformation capacity decrease. Therefore, sometimes they may break at an early stage when they are crushed by collision, or break in the position where the deformation is concentrated, and the compressive strength consistent with the material strength cannot be exerted, and sufficient absorption energy cannot be obtained. Therefore, in order to improve the collision safety of the automobile, the steel members used not only require material strength, but also require improved fracture toughness and deformation capacity, that is, improved toughness and bendability. Therefore, in order to apply high-strength steel members with a tensile strength exceeding 1.0GPa to the vehicle body, technology is required to provide steel members with more than the toughness and bendability so far and showing sufficient absorption energy even in the event of a collision accident.

[0010] Patent document 2 discloses a stamped product having excellent toughness and a tensile strength of 1.8 GPa or more, which is obtained by hot stamping. Patent document 3 discloses a steel material having an extremely high tensile strength of 2.0 GPa or more, and also having good toughness and ductility. Patent document 4 discloses a steel material having a high tensile strength of 1.8 GPa or more, and also having good toughness. Patent document 5 discloses a steel material having an extremely high tensile strength of 2.0 GPa or more, and also having good toughness.

[0011] However, Patent Documents 1 to 5 do not describe bendability, and when high-strength steel materials having a tensile strength exceeding 1.0 GPa are used as automobile components, they may not be able to fully meet higher demands.

[0012] In addition, most metal materials deteriorate in various properties as they become stronger, and in particular, their sensitivity to hydrogen embrittlement increases. In steel components, it is known that the sensitivity to hydrogen embrittlement increases as the tensile strength increases, and there are examples of hydrogen embrittlement cracking in bolt steel, which was promoted to higher strength before the automotive field.

[0013] However, the techniques of Patent Documents 1 to 5 have room for further improvement from the viewpoint of hydrogen embrittlement resistance.

[0014] Prior art literature

[0015] Patent Literature

[0016] Patent Document 1: Japanese Patent Application Publication No. 2002-102980

[0017] Patent Document 2: Japanese Patent Application Publication No. 2012-180594

[0018] Patent Document 3: Japanese Patent Application Publication No. 2012-1802

[0019] Patent Document 4: International Publication No. 2015 / 182596

[0020] Patent Document 5: International Publication No. 2015 / 182591 Summary of the invention

[0021] Problems to be solved by the invention

[0022] The present invention has been made in view of the above-mentioned problems. An object of the present invention is to provide a steel member having high strength and excellent bendability and hydrogen embrittlement resistance (hydrogen embrittlement resistance characteristics), and a steel plate suitable as a material of the steel member.

[0023] Means used to solve problems

[0024] The present inventors have conducted studies to obtain excellent bendability and hydrogen embrittlement resistance in a high-strength steel member obtained by hot stamping a steel sheet.

[0025] As a result, it was found that excellent bendability and hydrogen embrittlement resistance can be obtained by forming a decarburized layer on the surface of the steel member and enriching B. It was also found that in the steel sheet (raw material steel sheet) provided for hot stamping, the above-mentioned steel member can be stably obtained by introducing cracks into the oxide scale formed on the surface.

[0026] The present invention has been made in view of the above problems. The gist of the present invention is as follows.

[0027] [1] A steel member according to one embodiment of the present invention has a chemical composition containing the following elements in mass %: C: 0.10 to 0.70%, Si: 3.00% or less, Mn: 0.01 to 3.00%, P: 0.100% or less, S: 0.0100% or less, N: 0.020% or less, O: 0.010% or less, B: 0.0002 to 0.0200%, Ti: 0 to 0.200%, Cr: 0 to 1.00%, Mo: 0~1.00%, Ni: 0~2.00%, Nb: 0~0.10%, Cu: 0~2.00%, V: 0~1.00%, Ca: 0~0.020%, Mg: 0~0.020%, Al: 0~1.00%, Sn: 0~1.00%, W: 0~2.00%, Sb: 0~1.00%, Zr: 0~1.00%, Se: 0~1.00%, Bi :0~1.00%,As:0~1.00%,Ta:0~1.00%,Re:0~1.00%,Os:0~1.00%,Ir:0~1.00%,Tc:0~1.00%,Co:0~1.00%,REM:0~0.30%,and the balance: Fe and impurities,when a position at a depth of 1 / 4 of the thickness from the surface in the thickness direction is referred to as a 1 / 4 depth position,the maximum B content in a range from the surface to a depth of 10 μm in the thickness direction is 5 times or more of the B content at the 1 / 4 depth position,when the C content is measured from the surface in the thickness direction using GDS and the distance from the surface to a position where the C content first reaches the C content at the 1 / 4 depth position is referred to as a decarburization depth,the decarburization depth is 20 μm or more,and the Vickers hardness at the 1 / 4 depth position is 310~890.

[0028] [2] The steel member according to [1], wherein, when a position at a depth of 0.1 mm from the surface in the thickness direction is recorded as a 0.1 mm depth position, the Vickers hardness at the 0.1 mm depth position may be less than 0.95 times the Vickers hardness at the 1 / 4 depth position.

[0029] [3] The steel member according to [2], wherein the Vickers hardness at the 1 / 4 depth position is 310 to 450, and when the steel member having a plate thickness of 1.6 mm is deformed to a bending angle of 50 degrees, the maximum principal plastic strain at the center of the bending outer surface layer is less than 0.340.

[0030] [4] The steel member according to [2], wherein the Vickers hardness at the 1 / 4 depth position is greater than 450 and less than 530, the Vickers hardness at the 0.1 mm depth position is less than 0.90 times the Vickers hardness at the 1 / 4 depth position, and when the steel member having a plate thickness of 1.6 mm is deformed to a bending angle of 50 degrees, the maximum principal plastic strain at the center of the bent outer surface layer is less than 0.310.

[0031] [5] The steel member according to [2], wherein the Vickers hardness at the 1 / 4 depth position is greater than 530 and less than 700, the Vickers hardness at the 0.1 mm depth position is less than 0.88 times the Vickers hardness at the 1 / 4 depth position, and when the steel member having a plate thickness of 1.6 mm is deformed to a bending angle of 50 degrees, the maximum principal plastic strain at the center of the bent outer surface layer is less than 0.280.

[0032] [6] The steel member according to [2], wherein the Vickers hardness at the 1 / 4 depth position is greater than 700 and less than 890, the Vickers hardness at the 0.1 mm depth position is less than 0.86 times the Vickers hardness at the 1 / 4 depth position, and when the steel member having a plate thickness of 1.6 mm is deformed to a bending angle of 50 degrees, the maximum principal plastic strain at the center of the bent outer surface layer is less than 0.260.

[0033] [7] The steel member according to any one of [1] to [6], further comprising an alloy layer on the surface.

[0034] [8] The steel member according to [7], wherein the alloy layer may be a Fe—Al alloy layer.

[0035] [9] The steel member according to [7], wherein the alloy layer may be a Fe—Zn alloy layer.

[0036]

[10] A steel plate according to another embodiment of the present invention comprises: a base steel plate, and an iron oxide scale formed on the surface of the base steel plate, wherein the base steel plate has a chemical composition containing the following elements in mass %: C: 0.10 to 0.70%, Si: 3.00% or less, Mn: 0.01 to 3.00%, P: 0.100% or less, S: 0.0100% or less, N: 0.020% or less, O: 0.010% or less, B: 0.0002 to 0.0200%, Ti: 0 to 0.200%, Cr: 0 to 1.00%, Mo: 0 to 1.00%, Ni: 0 to 2.00%, Nb: 0 to 0.10%, Cu: 0 to 1.00%, Cu: 0 to 2.00%, Cu: 0 to 3.00%, Cu: 0 to 1.00%, Cu: 0 to 2.00%, Cu: 0 to 3.00%, Cu: 0 to 1.00%, Cu: 0 to 3.00%, Cu: 0 to 1.00%, Cu: 0 to 2.00%, Cu: 0 to 3 ...3.00%, Cu: 0 to 1.00%, Cu: 0 to 3.00%, Cu: 0 to 1.00%, Cu: 0 to 2.00%, Cu: 0 to 3.00%, Cu: 0 to 3.00%, Cu: 0 to 1.00%, Cu: 0 to 3.00%, Cu: 0 to 2.00%, V: 0-1.00%, Ca: 0-0.020%, Mg: 0-0.020%, Al: 0-1.00%, Sn: 0-1.00%, W: 0-2.00%, Sb: 0-1.00%, Zr: 0-1.00%, Se: 0-1.00%, Bi: 0-1.00%, As: 0-1.00%, Ta: 0-1.00%, Re: 0-1.00%, Os: 0-1.00%, Ir: 0-1.00%, Tc: 0-1.00%, Co: 0-1.00%, REM: 0-0.30%, and the balance: Fe and impurities, the above iron oxide scale is 90 pieces / mm 2 Densities above this include cracks.

[0037] Effects of the Invention

[0038] According to the above aspects of the present invention, it is possible to provide a steel member having high strength and excellent bendability and hydrogen embrittlement resistance, and a steel plate suitable as a material thereof. DETAILED DESCRIPTION

[0039] Hereinafter, a steel member (steel member of the present embodiment) and a steel plate (steel plate of the present embodiment) according to an embodiment of the present invention and a preferred method for producing the same will be described.

[0040] In the present embodiment, the steel member includes a case where it has an alloy layer on the surface, and the steel plate includes a case where it has a plating layer (a case where it is a plated steel plate).

[0041] (A) Steel components

[0042] When a position at a depth of 1 / 4 of the thickness from the surface in the thickness direction is recorded as a 1 / 4 depth position, the maximum B content in the range from the surface to a depth of 10 μm in the thickness direction is 5 times or more of the B content at the 1 / 4 depth position, and when the C content is measured using GDS in the thickness direction from the surface, and the distance from the surface to the position where the C content first reaches the C content at the 1 / 4 depth position is recorded as the decarburization depth, the decarburization depth is 20 μm or more, and the Vickers hardness at the 1 / 4 depth position is 310 to 890.

[0043] Steel components can have strength gradients.

[0044] The steel member may have an alloy layer (coating) on ​​the surface. In the case where the steel member has an alloy layer, the surface of the steel member used as a reference in "a depth of 1 / 4 of the thickness from the surface in the thickness direction" or "a depth of 10 μm from the surface in the thickness direction" refers to the surface of the portion (so-called base material) from which the alloy layer is removed.

[0045] Hereinafter, each requirement will be described in detail.

[0046] (A1) Chemical composition

[0047] The steel member of the present embodiment has a chemical composition containing the following elements in mass %: C: 0.10-0.70%, Si: 3.00% or less, Mn: 0.01-3.00%, P: 0.100% or less, S: 0.0100% or less, N: 0.020% or less, O: 0.010% or less, B: 0.0002-0.0200%, Ti: 0-0.200%, Cr: 0-1.00%, Mo: 0-1.00%, Ni: 0-2.00%, Nb: 0-0.10%, Cu: 0-2.00%, V: 0-1.0 0%, Ca: 0~0.020%, Mg: 0~0.020%, Al: 0~1.00%, Sn: 0~1.00%, W: 0~2.00%, Sb: 0~1.00%, Zr: 0~1.00%, Se: 0~1.00%, Bi: 0~1.00%, As: 0~1.00%, Ta: 0~1.00%, Re: 0~1.00%, Os: 0~1.00%, Ir: 0~1.00%, Tc: 0~1.00%, Co: 0~1.00%, REM: 0~0.30%, and the balance: Fe and impurities.

[0048] Here, the chemical composition of the steel member refers to the chemical composition of the portion other than the surface (e.g., the position of the steel member that is 1 / 4 of the thickness from the surface in the thickness direction: 1 / 4 depth position). Hereinafter, % in relation to the content is mass % unless otherwise stated.

[0049] The reasons for limiting the content of each element are as follows.

[0050] C: 0.10~0.70%

[0051] C is an element that improves the hardenability of steel and the strength of steel components obtained by hot stamping steel sheets. However, when the C content is less than 0.10%, it is difficult to ensure sufficient strength (1.0 GPa or more) in the steel components. Therefore, the C content is set to 0.10% or more. The C content is preferably 0.15% or more.

[0052] On the other hand, when the C content exceeds 0.70%, the strength of the steel member increases excessively, and the deterioration of the bendability and hydrogen embrittlement resistance becomes significant. In addition, the weldability also deteriorates. Therefore, the C content is set to 0.70% or less. The C content is preferably 0.60% or less.

[0053] Si: 3.00% or less

[0054] Si is an element effective for improving the hardenability of steel and stably ensuring the strength in steel components. Therefore, Si may be contained. In order to obtain the above-mentioned effects, the Si content is preferably set to 0.05% or more, and more preferably set to 0.10% or more.

[0055] On the other hand, when the Si content in the steel sheet is greater than 3.00%, the heating temperature required for austenite transformation during heat treatment will increase significantly. As a result, the cost required for heat treatment may increase. Furthermore, when the Si content is greater than 3.00%, the toughness of the quenched portion will deteriorate. Therefore, the Si content is set to 3.00% or less. The Si content is preferably 2.00% or less, and more preferably 1.80% or less.

[0056] Mn: 0.01~3.00%

[0057] Mn is an element that is very effective in improving the hardenability of steel and stably ensuring strength in steel components. Mn is also an element that reduces the Ac3 point and promotes the low temperature of the quenching treatment temperature. When the Mn content is less than 0.01%, these effects are not sufficient, so the Mn content is set to 0.01% or more. The Mn content is preferably 0.05% or more.

[0058] On the other hand, when the Mn content exceeds 3.00%, the above effects are saturated, and the toughness, bendability, and hydrogen embrittlement resistance of the quenched portion are deteriorated. Therefore, the Mn content is set to 3.00% or less. The Mn content is preferably 2.80% or less, and more preferably 2.50% or less.

[0059] P: 0.100% or less

[0060] P is an element that deteriorates the toughness and hydrogen embrittlement resistance of steel components. In particular, when the P content is greater than 0.100%, the deterioration of toughness and hydrogen embrittlement resistance becomes significant. Therefore, the P content is limited to 0.100% or less. The P content is preferably limited to 0.050% or less. The P content is preferably less, so it can be 0%, but from a cost perspective, it can be set to 0.001% or more.

[0061] S: 0.0100% or less

[0062] S is an element that deteriorates the toughness, bendability, and hydrogen embrittlement resistance of steel components. In particular, when the S content is greater than 0.0100%, the deterioration of toughness, bendability, and hydrogen embrittlement resistance becomes significant. Therefore, the S content is limited to 0.0100% or less. The S content is preferably limited to 0.0050% or less. The S content is preferably less, so it can be 0%, but from a cost perspective, it can be set to 0.0001% or more.

[0063] N: 0.020% or less

[0064] N is an element that deteriorates the toughness and hydrogen embrittlement resistance of steel components. In particular, when the N content is greater than 0.020%, coarse nitrides will be formed in the steel, and the toughness and hydrogen embrittlement resistance will be significantly deteriorated. Therefore, the N content is set to 0.020% or less. The lower limit of the N content does not need to be specifically limited, and can be 0%, but setting the N content to less than 0.0002% will increase the steelmaking cost, which is not economically preferred. Therefore, the N content can be set to more than 0.0002%, and can also be set to more than 0.0008%.

[0065] O: 0.010% or less

[0066] O is an element that deteriorates the toughness and hydrogen embrittlement resistance of steel components. In particular, when the O content is greater than 0.010%, coarse nitrides will be formed in the steel, and the toughness and hydrogen embrittlement resistance will be significantly deteriorated. Therefore, the O content is set to 0.010% or less. The lower limit of the O content does not need to be specifically limited, and can be 0%, but setting the O content to less than 0.0002% will increase the steelmaking cost, which is not economically preferred. Therefore, the O content can be set to more than 0.0002%, and can also be set to more than 0.0008% or more than 0.001%.

[0067] B: 0.0002~0.0200%

[0068] B is an element that has the effect of greatly improving the hardenability of steel even in a trace amount. In addition, B is an element that strengthens the grain boundary, improves toughness and hydrogen embrittlement resistance by segregating at the grain boundary, and is an element that inhibits the grain growth of austenite when the steel plate is heated. In addition, B is an element that is effective for obtaining a surface structure with a strong grain boundary and a fine martensite body by being enriched in the surface layer as described later. When the B content is less than 0.0002%, these effects are not sufficient. Therefore, the B content is set to 0.0002% or more. The B content is preferably 0.0005% or more, and more preferably 0.0010% or more.

[0069] On the other hand, when the B content exceeds 0.0200%, a large amount of coarse compounds precipitate, and the toughness and hydrogen embrittlement resistance of the steel member deteriorate. Therefore, when B is contained, the B content is set to 0.0200% or less. The B content is preferably 0.0100% or less.

[0070] The steel member of the present embodiment may further contain one or more elements selected from Ti, Cr, Mo, Ni, Nb, Cu, V, Ca, Mg, Al, Sn, W, Sb, Zr, Se, Bi, As, Ta, Re, Os, Ir, Tc, Co and REM shown below on the basis of the above elements in order to improve strength, toughness, bendability, corrosion resistance, deoxidation, and hydrogen embrittlement resistance. These elements are optional elements and do not necessarily need to be contained, so the lower limit is 0%. If the content is below the upper limit described later, these elements may be contained as impurities.

[0071] Ti: 0~0.200%

[0072] Ti is an element having the following effects: when the steel plate is heated to a temperature above the Ac3 point and heat-treated, recrystallization is suppressed, and fine carbides are formed to suppress grain growth, thereby making the austenite grains fine. Therefore, by containing Ti, the toughness of the steel member can be greatly improved. In addition, Ti is an element that suppresses the consumption of B caused by BN precipitation by preferentially combining with N in the steel, and promotes the hardenability improvement effect brought by B described later. Therefore, Ti can be contained. In the case of fully obtaining the above-mentioned effects, the Ti content is preferably set to 0.010% or more. The Ti content is more preferably 0.020% or more.

[0073] On the other hand, when the Ti content exceeds 0.200%, the amount of TiC precipitated increases and consumes C, so the strength of the steel member decreases. Therefore, the Ti content is set to 0.200% or less. The Ti content is preferably 0.100% or less.

[0074] Cr: 0~1.00%

[0075] Cr is an element effective in improving the hardenability of steel and stably ensuring the strength of steel components. Therefore, Cr may be contained. In order to obtain the above-mentioned effects, the Cr content is preferably set to 0.01% or more. The Cr content is more preferably 0.05% or more, and further preferably 0.08% or more.

[0076] On the other hand, when the Cr content exceeds 1.00%, the above effect is saturated and the cost increases. In addition, Cr has the effect of stabilizing iron carbides, so when the Cr content exceeds 1.00%, coarse iron carbides may be melted and remain when the steel plate is heated, and the toughness of the steel member may deteriorate. Therefore, when Cr is contained, the Cr content is set to 1.00% or less. The Cr content is preferably 0.80% or less.

[0077] Mo: 0~1.00%

[0078] Mo is an element effective in improving the hardenability of steel and stably ensuring the strength of steel components. Therefore, Mo may be contained. In order to obtain the above-mentioned effects, the Mo content is preferably set to 0.01% or more. The Mo content is more preferably 0.05% or more.

[0079] On the other hand, when the Mo content exceeds 1.00%, the above effect is saturated and the cost increases. In addition, Mo has the effect of stabilizing iron carbides, so when the Mo content exceeds 1.00%, coarse iron carbides may be melted and remain when the steel plate is heated, and the toughness of the steel member may deteriorate. Therefore, when Mo is contained, the Mo content is set to 1.00% or less. The Mo content is preferably 0.80% or less.

[0080] Ni: 0~2.00%

[0081] Ni is an element effective for improving the hardenability of steel and stably ensuring the strength of steel components. Therefore, Ni may be contained. In order to obtain the above-mentioned effects, it is preferred that the Ni content be set to 0.01% or more. The Ni content is more preferably 0.10% or more.

[0082] On the other hand, when the Ni content exceeds 2.00%, the above-mentioned effect is saturated and the economic efficiency is reduced. Therefore, when Ni is contained, the Ni content is set to 2.00% or less. The Ni content is preferably 1.00% or less.

[0083] Nb: 0~0.10%

[0084] Nb is an element that forms fine carbides and improves the toughness of steel through its grain refinement effect. Therefore, Nb may be contained. In the case where the above-mentioned effects are fully obtained, the Nb content is preferably set to 0.02% or more. The Nb content is more preferably 0.03% or more.

[0085] On the other hand, when the Nb content exceeds 0.10%, carbides coarsen and the toughness of the steel member deteriorates. Therefore, when Nb is contained, the Nb content is set to 0.10% or less. The Nb content is preferably 0.08% or less.

[0086] Cu: 0~2.00%

[0087] Cu is an element effective for improving the hardenability of steel and stably ensuring the strength of steel components. Therefore, Cu may be contained. In addition, Cu is an element having the effect of improving the corrosion resistance of steel components. In order to obtain the above-mentioned effect, it is preferred that the Cu content is set to 0.01% or more. The Cu content is more preferably 0.05% or more.

[0088] On the other hand, when the Cu content exceeds 2.00%, the above-mentioned effect is saturated and the cost increases. Therefore, when Cu is contained, the Cu content is set to 2.00% or less. The Cu content is preferably 1.00% or less.

[0089] V: 0~1.00%

[0090] V is an element that forms fine carbides and improves the toughness of steel by its grain refining effect. Therefore, V may be contained. In order to obtain the above-mentioned effect, the V content is preferably set to 0.01% or more. The V content is more preferably 0.10% or more.

[0091] On the other hand, when the V content exceeds 1.00%, the above-mentioned effect is saturated and the economic efficiency is reduced. Therefore, when V is contained, the V content is set to 1.00% or less.

[0092] Ca: 0~0.020%

[0093] Ca is an element that has the effect of miniaturizing inclusions in steel and improving the toughness of steel components. Therefore, Ca may be contained. In order to obtain the above-mentioned effect, it is preferable to set the Ca content to 0.001% or more. The Ca content is more preferably 0.002% or more.

[0094] On the other hand, when the Ca content exceeds 0.020%, the effect is saturated and the cost increases. Therefore, when Ca is contained, the Ca content is set to 0.020% or less. The Ca content is preferably 0.010% or less, and more preferably 0.005% or less.

[0095] Mg: 0~0.020%

[0096] Mg is an element that has the effect of miniaturizing inclusions in steel and improving the toughness of steel components. Therefore, Mg may be contained. In order to obtain the above-mentioned effect, it is preferred that the Mg content be set to 0.001% or more. The Mg content is more preferably 0.002% or more.

[0097] On the other hand, when the Mg content exceeds 0.020%, the effect is saturated and the cost increases. Therefore, when Mg is contained, the Mg content is set to 0.020% or less. The Mg content is preferably 0.010% or less, and more preferably 0.005% or less.

[0098] Al: 0~1.00%

[0099] Al is an element generally used as a deoxidizer for steel. Therefore, Al may be contained. In order to obtain the above-mentioned effect, the Al content is preferably set to 0.01% or more.

[0100] On the other hand, when the Al content exceeds 1.00%, the above-mentioned effect is saturated and the economic efficiency is reduced. Therefore, when Al is contained, the Al content is set to 1.00% or less. The Al content here refers to the total Al content.

[0101] Sn: 0~1.00%

[0102] Sn is an element that improves corrosion resistance in a corrosive environment. Therefore, Sn may be contained. In order to obtain the above-mentioned effect, it is preferable to set the Sn content to 0.01% or more.

[0103] On the other hand, when the Sn content exceeds 1.00%, the grain boundary strength decreases and the toughness of the steel member deteriorates. Therefore, when Sn is contained, the Sn content is set to 1.00% or less.

[0104] W: 0~2.00%

[0105] W is an element that can improve the hardenability of steel and stably ensure the strength of steel components. Therefore, W can be contained. In addition, W is an element that improves corrosion resistance in a corrosive environment. In order to obtain the above-mentioned effects, it is preferred that the W content be set to 0.01% or more.

[0106] On the other hand, when the W content exceeds 2.00%, the above-mentioned effect is saturated and the economic efficiency is reduced. Therefore, when W is contained, the W content is set to 2.00% or less. The W content is preferably 1.00% or less.

[0107] Sb: 0~1.00%

[0108] Sb is an element that improves corrosion resistance in a corrosive environment. Therefore, Sb may be contained. In order to obtain the above-mentioned effect, the Sb content is preferably set to 0.01% or more.

[0109] On the other hand, when the Sb content exceeds 1.00%, the grain boundary strength decreases and the toughness of the steel member deteriorates. Therefore, when Sb is contained, the Sb content is set to 1.00% or less.

[0110] Zr: 0~1.00%

[0111] Zr is an element that improves corrosion resistance in a corrosive environment. Therefore, Zr may be contained. In order to obtain the above-mentioned effect, the Zr content is preferably set to 0.01% or more.

[0112] On the other hand, when the Zr content exceeds 1.00%, the grain boundary strength decreases and the hydrogen embrittlement resistance of the steel member decreases. Therefore, when Zr is contained, the Zr content is set to 1.00% or less.

[0113] Se: 0~1.00%

[0114] Se is an element that improves hydrogen embrittlement resistance, and therefore may be contained. In order to obtain the above-mentioned effect, the Se content is preferably set to 0.01% or more.

[0115] On the other hand, when the Se content exceeds 1.00%, the effect is saturated and the cost increases. Therefore, when Se is contained, the Se content is set to 1.00% or less.

[0116] Bi: 0~1.00%

[0117] Bi is an element that improves hydrogen embrittlement resistance. Therefore, it may be contained. In order to obtain the above-mentioned effect, it is preferable to set the Bi content to 0.01% or more.

[0118] On the other hand, when the Bi content exceeds 1.00%, the effect is saturated and the cost increases. Therefore, when Bi is contained, the Bi content is set to 1.00% or less.

[0119] As: 0~1.00%

[0120] As is an element that improves hydrogen embrittlement resistance, and therefore may be contained. In order to obtain the above-mentioned effect, the As content is preferably set to 0.01% or more.

[0121] On the other hand, when the As content exceeds 1.00%, the effect is saturated and the cost increases. Therefore, when As is contained, the As content is set to 1.00% or less.

[0122] Ta: 0~1.00%

[0123] Ta is an element that improves hydrogen embrittlement resistance. Therefore, it may be contained. In order to obtain the above-mentioned effect, it is preferable to set the Ta content to 0.01% or more.

[0124] On the other hand, when the Ta content exceeds 1.00%, the effect is saturated and the cost increases. Therefore, when Ta is contained, the Ta content is set to 1.00% or less.

[0125] Re: 0~1.00%

[0126] Re is an element that improves hydrogen embrittlement resistance. Therefore, it may be contained. In order to obtain the above-mentioned effect, it is preferable to set the Re content to 0.01% or more.

[0127] On the other hand, when the Re content exceeds 1.00%, the effect is saturated and the cost increases. Therefore, when Re is contained, the Re content is set to 1.00% or less.

[0128] Os: 0~1.00%

[0129] Os is an element that improves hydrogen embrittlement resistance, and therefore may be contained. In order to obtain the above-mentioned effect, the Os content is preferably set to 0.01% or more.

[0130] On the other hand, when the Os content exceeds 1.00%, the effect is saturated and the cost increases. Therefore, when Os is contained, the Os content is set to 1.00% or less.

[0131] Ir: 0~1.00%

[0132] Ir is an element that improves hydrogen embrittlement resistance, and therefore may be contained. In order to obtain the above-mentioned effect, the Ir content is preferably set to 0.01% or more.

[0133] On the other hand, when the Ir content exceeds 1.00%, the effect is saturated and the cost increases. Therefore, when Ir is contained, the Ir content is set to 1.00% or less.

[0134] Tc: 0~1.00%

[0135] Tc is an element that improves hydrogen embrittlement resistance, and therefore may be contained. In order to obtain the above-mentioned effect, the Tc content is preferably set to 0.01% or more.

[0136] On the other hand, when the Tc content exceeds 1.00%, the effect is saturated and the cost increases. Therefore, when Tc is contained, the Tc content is set to 1.00% or less.

[0137] Co: 0~1.00%

[0138] Co is an element that improves corrosion resistance in a corrosive environment. Therefore, Co may be contained. In order to obtain the above-mentioned effect, the Co content is preferably set to 0.01% or more.

[0139] On the other hand, when the Co content exceeds 1.00%, the above-mentioned effect is saturated and the economic efficiency is reduced. Therefore, when Co is contained, the Co content is set to 1.00% or less.

[0140] REM: 0~0.30%

[0141] REM is an element that has the effect of miniaturizing inclusions in steel and improving the toughness of steel components, similar to Ca. Therefore, REM may be contained. In order to obtain the above-mentioned effect, it is preferable to set the REM content to 0.01% or more. The REM content is more preferably 0.02% or more.

[0142] On the other hand, when the REM content exceeds 0.30%, the effect is saturated and the cost increases. Therefore, when REM is contained, the REM content is set to 0.30% or less. The REM content is preferably 0.20% or less.

[0143] Here, REM refers to 17 elements including Sc, Y, La, Nd and other lanthanoid elements, and the content of REM refers to the total content of these elements. REM is added to the molten steel using, for example, Fe-Si-REM alloy, which contains, for example, La, Nd, Ce and Pr.

[0144] The chemical composition of the steel member of the present embodiment includes the elements described above, that is, the balance is Fe and impurities.

[0145] Here, "impurities" refer to components mixed in by various main reasons such as raw materials such as ore and scrap steel and manufacturing processes when the steel plate is manufactured industrially, and represent components that are allowed within a range that does not adversely affect the characteristics of the steel member of this embodiment. The industrial manufacturing method refers to blast furnace steelmaking and electric furnace steelmaking, and also covers the level (impurity level) mixed in when manufacturing by any method.

[0146] The chemical composition of steel components can be obtained by the following method.

[0147] It is obtained by cutting out analysis samples from steel components and performing elemental analysis such as ICP (inductively coupled plasma) emission spectrometry. C and S can be measured using the combustion-infrared absorption method, N can be measured using the inert gas fusion-thermal conductivity method, and O can be measured using the inert gas fusion-non-dispersive infrared absorption method.

[0148] As described in JIS G 0417:1999, the analysis sample was taken from a position 1 / 4 of the thickness from the surface in the thickness direction, avoiding the width direction ends of the base steel plate, so as to obtain the average chemical composition of the entire thickness of the steel member.

[0149] The C content and B content obtained here are the C content and B content at the 1 / 4 depth position described later. Since the chemical composition of the steel member of this embodiment is roughly uniform, it can also be regarded as the average chemical composition of the entire steel member excluding the decarburized layer and the surface layer where B is enriched.

[0150] (A2) Structure of steel components

[0151] In the following description, the position at a depth of 1 / 4 of the thickness from the surface in the thickness direction is referred to as the 1 / 4 depth position, and the position at a depth of 0.1 mm from the surface in the thickness direction is referred to as the 0.1 mm depth position. In addition, when the C content is measured from the surface in the thickness direction using GDS, the distance from the surface to the position where the C content first reaches the same level as the C content at the aforementioned 1 / 4 depth position (the position closest to the surface among the positions where the C content reaches the same level as the C content at the 1 / 4 depth position) is referred to as the decarburization depth for description.

[0152] In the structure of the surface layer of the steel member of the present embodiment, the maximum B content in the range from the surface to a depth of 10 μm is 5 times or more the B content at a 1 / 4 depth, and the decarburization depth is 20 μm or more.

[0153] In order to improve the bendability of steel components, decarburization and softening the surface layer are extremely effective. Since the stress and deformation generated by bending deformation are greater as the surface layer is bent to the outside, the bendability can be improved by softening the surface layer to increase the fracture limit. When the decarburization depth of the steel component is 20μm or more, the bendability is improved. Therefore, the decarburization depth is set to 20μm or more.

[0154] As mentioned above, decarburization and softening of the surface layer are effective in improving the bendability of steel components. On the other hand, since carbon is an element that segregates at grain boundaries for strengthening, the reduction of carbon at grain boundaries is not preferred. Since carbon is an element that segregates at grain boundaries for strengthening, when the amount of carbon at grain boundaries is reduced and the grain boundary strength is reduced, hydrogen embrittlement resistance and toughness may be reduced.

[0155] In addition, although decarburization and softening the surface are effective, it is not preferred to make the surface a ferrite main structure. This is because ferrite is coarse and soft relative to the dense martensite main structure of the base material, so the mismatch between the ferrite main structure of the surface layer and the martensite main structure of the base material is large, which becomes the cause of deterioration of bendability, hydrogen embrittlement resistance, and toughness.

[0156] Therefore, in the steel member of the present embodiment, while the surface layer is decarburized, B is enriched in the surface layer. B is an element that segregates at the grain boundary like carbon to strengthen the grain boundary and improve hardenability. Therefore, when B is enriched in the surface layer, a structure of a martensite main body with strong and fine grain boundaries can be obtained. The martensite main structure of the surface layer is softer than the martensite main structure of the base material due to decarburization, and a high level of bendability, hydrogen embrittlement resistance, and toughness can be obtained.

[0157] Specifically, when the maximum B content in the range from the surface of the steel member to a depth of 10 μm is 5 times or more the B content at a position of 1 / 4 of the depth, bendability and hydrogen embrittlement resistance are improved.

[0158] In addition, the hardness (Vickers hardness (HV)) of the steel member of this embodiment at the 1 / 4 depth position is 310 to 890. This Vickers hardness is equivalent to a tensile strength of 1.0 GPa to 3.1 GPa for the steel member, and when applied to automobile parts, it helps to reduce the weight of the automobile body and enhance the collision safety. The relationship between hardness and tensile strength is described in, for example, SAE J 417.

[0159] The steel member of this embodiment preferably decarburizes and softens the surface layer and further controls the strength gradient from the surface layer to the inside within the following range. In this case, the bendability is further improved. The reason for this is that, in bending deformation, as described above, the maximum deformation and stress act on the outer surface of the bend, and cracks will advance from the surface to the inside. If there is an appropriate strength gradient, it has the effect of suppressing the expansion of deformation on the surface.

[0160] In order to obtain the above-mentioned effect in a steel member, it is preferable to control the Vickers hardness at a position 0.1 mm deep from the surface in the thickness direction (0.1 mm depth position) within an appropriate range based on the Vickers hardness at a 1 / 4 depth position which is highly correlated with the tensile strength of the steel member.

[0161] Specifically, the Vickers hardness at a depth of 0.1 mm is preferably 0.95 times or less of the Vickers hardness at a depth of 1 / 4.

[0162] Furthermore, it is more preferable to further control the hardness ratio based on the Vickers hardness at the 1 / 4 depth position and control the maximum principal plastic strain at the center of the curved outer surface layer within a prescribed range.

[0163] When the Vickers hardness at the 1 / 4 depth position is greater than 700 and less than 890 (equivalent to a tensile strength greater than 2.4 GPa and less than 3.1 GPa), the Vickers hardness at the 0.1 mm depth position is preferably less than 0.86 times the Vickers hardness at the 1 / 4 depth position, and when a steel member with a plate thickness of 1.6 mm is deformed to a bending angle of 50 degrees, the maximum principal plastic strain at the center of the bent outer surface layer is less than 0.260.

[0164] In the case of a steel member having a plate thickness other than 1.6 mm, the bending angle is adjusted so as to be deformed to be equivalent to the case where the steel member having a plate thickness of 1.6 mm is deformed to a bending angle of 50 degrees.

[0165] Specifically, the deformation is performed to a bending angle so as to satisfy the following formula.

[0166] Bending angle = 6 x (plate thickness) 2 -32×(plate thickness)+86

[0167] For example, when the plate thickness is 1.0 mm, the maximum principal plastic strain at the center of the outer surface of the bending when the plate is deformed to a bending angle of 60 degrees is evaluated, and when the plate thickness is 2.3 mm, the maximum principal plastic strain at the center of the outer surface of the bending when the plate is deformed to a bending angle of 44 degrees is evaluated. The plate thickness is not limited, but is preferably 0.6 to 4.0 mm.

[0168] In addition, when the Vickers hardness at a 1 / 4 depth position is greater than 530 and less than 700 (equivalent to a tensile strength greater than 1.8 GPa and less than 2.4 GPa), the Vickers hardness at a 0.1 mm depth position is preferably less than 0.88 times the Vickers hardness at a 1 / 4 depth position, and when a steel member with a plate thickness of 1.6 mm is deformed to a bending angle of 50 degrees, the maximum principal plastic strain at the center of the bent outer surface layer is less than 0.280.

[0169] In addition, when the Vickers hardness at the 1 / 4 depth position is greater than 450 and less than 530 (equivalent to a tensile strength greater than 1.5 GPa and less than 1.8 GPa), the Vickers hardness at the 0.1 mm depth position is preferably less than 0.90 times the Vickers hardness at the 1 / 4 depth position, and when a steel member with a plate thickness of 1.6 mm is deformed to a bending angle of 50 degrees, the maximum principal plastic strain at the center of the bent outer surface layer is less than 0.310.

[0170] In addition, when the Vickers hardness at the 1 / 4 depth position is 310 to 450 (equivalent to a tensile strength of 1.0 to 1.5 GPa), the Vickers hardness at the 0.1 mm depth position is preferably less than 0.95 times the Vickers hardness at the 1 / 4 depth position, and when a steel member with a plate thickness of 1.6 mm is deformed to a bending angle of 50 degrees, the maximum principal plastic strain at the center of the bent outer surface layer is less than 0.340.

[0171] In any case, the Vickers hardness at a depth of 0.1 mm is preferably 0.70 times or more the Vickers hardness at a depth of 1 / 4.

[0172] The B enrichment degree of the surface layer (B enrichment ratio: ratio of the maximum B content within a range of 10 μm in depth to the B content at a 1 / 4 depth position) and the decarburization depth can be determined by the following method using GDS.

[0173] At a position of 1 / 4 of the plate width (short side) from the end of the steel member in the width direction, GDS (glow discharge emission spectroscopy) was performed at a pitch of 50 nm or less from the outermost surface of the steel member (the surface of the oxide scale if the surface has oxide scale, the surface of the alloy layer if the surface has an alloy layer) toward the plate thickness direction to measure the B content, C content and Fe content. As a result of the measurement, the position where the Fe content first reaches 95 mass % or more is regarded as the surface.

[0174] In addition, the maximum value of the B content in the range from the above-mentioned surface to a depth of 10 μm obtained by the GDS spectrum is taken as the maximum B content. However, in the case where the surface has a Fe-Al alloy layer described later, the maximum value of the B content in the range from the position where the sum of Fe and Al first reaches 70% by mass or more to a depth of 10 μm is taken as the maximum B content. In the case where the surface has a Fe-Zn alloy layer described later, the maximum value of the B content in the range from the position where the sum of Fe and Zn first reaches 70% by mass or more to a depth of 10 μm is taken as the maximum B content. The case of having a Fe-Al alloy layer refers to the case where the Al content of the alloy layer region on the surface of the steel component obtained by the GDS spectrum is 25% by mass or more. In addition, the case of having a Fe-Zn alloy layer refers to the case where the Zn content of the alloy layer region on the surface of the steel component obtained by the GDS spectrum is 25% by mass or more.

[0175] The B enrichment degree of the surface layer is calculated based on the maximum B content and the B content at the 1 / 4 depth position determined by the above method.

[0176] Furthermore, the position where the C content obtained by the same GDS spectrum first reaches the same level as the C content at the 1 / 4 depth position is defined as the end of the decarburization depth, and the distance from the surface to the end is defined as the decarburization depth.

[0177] The GDS measurement was performed 5 times with the position changed, and the average value of the 5 times was adopted.

[0178] The hardness at the 1 / 4 depth position and the hardness at the 0.1 mm depth position were determined as follows.

[0179] A sample for cross-sectional observation was taken from a position 1 / 4 of the width (short side) from the end of the steel member in the width direction, and the Vickers hardness was measured at the depth position (1 / 4 depth position, 0.1 mm depth position) as the object according to JIS Z2244-1: 2020. The test force was 100 gf. Five measurements were performed at each depth, and the average value was taken as the hardness at that position.

[0180] The maximum principal plastic strain at the center of the outer surface of the bending when deformed to a predetermined bending angle is determined by the following method.

[0181] The steel member having a strength gradient on the surface was modeled using the finite element method. The total plate thickness was set so that the ranges of 50 μm, 50 to 100 μm, and 100 to 250 μm from the surface had the same hardness as the steel member to be evaluated.

[0182] In addition, a test jig for performing a bending test of VDA238-100 was modeled. According to the standard, for example, the punch diameter R was set to 0.4 mm, the roller diameter was set to 30 mmφ, and the distance between the rollers was set to 2×plate thickness+0.05.

[0183] Using the modeled steel member and test fixture, press-fit to the specified bending angle (simulation). Output the maximum principal plastic strain at the specified bending angle and find the maximum principal plastic strain at the center of the outer surface of the bending (the point where the maximum principal plastic strain on the bending ridgeline reaches the maximum).

[0184] The software for the finite element method analysis is not limited, and for example, Marc manufactured by MSC Software Corporation is used. The mesh size is set to 5 μm, and the friction coefficient μ of the contact portion between the steel member and the test jig is set to 0.05.

[0185] The metal structure (internal structure) at the 1 / 4 depth position of the steel member of the present embodiment is not limited, and is preferably a structure containing 80% or more martensite by volume fraction. By having the above chemical composition and making the volume fraction of martensite 80% or more, the Vickers hardness at the 1 / 4 depth position can be made to be 310 or more (equivalent to a tensile strength of 1.0 GPa or more). Preferably, the volume fraction is 90% or more martensite. More preferably, it is 95% or more. Martensite can be 100%. If the volume fraction of martensite is small, it becomes difficult to obtain a tensile strength of 1.0 GPa or more.

[0186] The metal structure at the 1 / 4 depth position of the steel member may contain retained austenite, bainite, ferrite and / or pearlite as the remaining structure other than martensite.

[0187] Martensite includes not only so-called fresh martensite but also tempered martensite and autotempered martensite. Autotempered martensite refers to tempered martensite generated during cooling during quenching without heat treatment for tempering, and is generated by in-situ tempering of martensite generated by self-heating accompanying martensitic transformation.

[0188] The structural fraction in the metal structure at the 1 / 4 depth position of the steel member can be measured by the following method.

[0189] The area fraction of martensite (including fresh martensite, tempered martensite, and autotempered martensite) is measured using a transmission electron microscope (TEM) and an electron beam diffraction device attached to the TEM.

[0190] Specifically, a measurement sample including a position 1 / 4 of the width of the steel member from the width end of the steel member (1 / 4 width position) and a 1 / 4 depth position of the steel member was cut out as a thin film sample for TEM observation. 2 TEM observation was performed in the above range.

[0191] According to the diffraction pattern of the electron beam of the thin film sample, the martensite and bainite of the body-centered cubic lattice are distinguished from the retained austenite of the face-centered cubic lattice. Then, the iron carbide (Fe3C) in the martensite and bainite is found according to the diffraction pattern, and the tissue fractions of the martensite and bainite are measured respectively by observing their precipitation morphology. Specifically, if the precipitation morphology is precipitation in three directions, it is judged to be martensite (tempered martensite), and if it is limited precipitation in one direction, it is judged to be bainite. In the case where no iron carbide precipitation is found, it is also judged to be martensite (primary martensite).

[0192] The tissue fractions of martensite and bainite measured by TEM are measured as area %, and since the metal structure of the steel member of this embodiment has isotropy, the value of the area fraction can be directly replaced by the volume fraction. Carbides are observed to distinguish martensite from bainite, but in this embodiment, carbides are not included in the volume fraction of the tissue.

[0193] In the case where ferrite or pearlite exists as the residual structure, it can be easily confirmed with an optical microscope or a scanning electron microscope. Specifically, a measurement sample including a position of 1 / 4 width of the steel member and a position of 1 / 4 depth of the steel member is cut out as a sample for observation. The cut sample is mechanically ground and then mirror-finished. Next, the sample is etched with nitric acid to expose the ferrite and pearlite, and a scanning electron microscope is used to observe the area of ​​40,000 μm 2 By observing the above range, the presence of ferrite or pearlite is confirmed. A structure in which ferrite and cementite are alternately arranged in layers is identified as pearlite, and a structure in which cementite is precipitated in particles is identified as bainite.

[0194] (A3) Alloy layer

[0195] The steel member of the present embodiment may include an alloy layer on at least a portion (or the entire surface) of the surface.

[0196] The alloy layer may be a Fe—Al alloy layer or a Fe—Zn alloy layer.

[0197] The Fe—Al alloy layer refers to an alloy layer containing 70 mass % or more of Fe and Al in total, and the Fe—Zn alloy layer refers to an alloy layer containing 70 mass % or more of Fe and Zn in total.

[0198] By providing the alloy layer, the corrosion resistance is improved, and thus the hydrogen embrittlement resistance in automobile use can be improved.

[0199] The thickness of the alloy layer is preferably 5 to 100 μm.

[0200] As described above, when an alloy layer is formed on the surface of a steel member, the surface serving as a reference for each depth position is the surface of a portion (base steel material) from which the alloy layer is removed.

[0201] The thickness of the alloy layer can be determined by observing a cross section in the thickness direction using a scanning electron microscope.

[0202] Specifically, a measurement sample is cut out from the half of the length direction (the position of half the length in the length direction from the end in the length direction) and the quarter of the width (the position of quarter the width in the width direction from the end in the width direction) of the steel member and observed. The observation range based on the microscope is, for example, 40000 μm in area at a magnification of 400 times. 2 The range is above. The cut sample is mechanically ground and then mirror finished. Next, the thickness of the alloy layer in any 10 fields of view is measured, and the average value is used as the thickness of the alloy layer. By observing the BSE image (or COMPO image), a clear contrast difference can be confirmed between the alloy layer and the bottom steel (steel plate substrate). Therefore, by measuring the thickness from the outermost surface to the position where the contrast changes, the thickness of the alloy layer can be measured. The measurement is performed by measuring 20 positions at equal intervals in the observation photograph, and the distance between the measurement positions is 6.5μm. In addition, when measuring, 5 fields of view are observed according to the above method, and the average value is used as the thickness of the alloy layer.

[0203] In addition, regarding the chemical composition of the alloy layer, the content of Fe, Al, Zn, etc. contained in the alloy layer can be obtained by performing elemental analysis of the site using an electron probe microanalyzer (EPMA) for the same observation range as above (beam diameter 1 μm or less). A total of 10 points are analyzed in the alloy layer of any 10 fields of view, and the average value is used as the Fe, Al, and Zn content contained in the alloy layer. The same method is used to obtain the content when elements other than Fe, Al, and Zn are contained.

[0204] (A4) Shape of steel components

[0205] The shape of the steel member of the present embodiment is not particularly limited. That is, the steel member may be a flat plate or a formed body obtained by forming a steel plate into a prescribed shape. In most cases, the hot-formed steel member is a formed body, and in the present embodiment, both the formed body and the flat plate are referred to as "steel members". In addition, the steel member may be a tailored property material whose strength varies depending on the position. In this case, it is preferred that the tensile strength of at least a portion of the steel member is 1.0 GPa (1000 MPa) or more. The tailored property material may be a material obtained by joining steel plates with different chemical compositions, strengths, and plate thicknesses, and may also be a steel plate that has been locally heat-treated.

[0206] (B) Steel Plate

[0207] Next, a steel plate (hereinafter sometimes referred to as the steel plate of the present embodiment) serving as a raw material of the steel member of the present embodiment will be described. The steel member can be obtained by subjecting the steel plate described below to a heat treatment described later.

[0208] The steel plate of the present embodiment includes a base steel plate and iron oxide scale formed on the surface of the base steel plate.

[0209] The steel sheet according to the present embodiment may have a plating layer on the iron oxide scale (on the surface of the iron oxide scale).

[0210] (B1) Chemical composition of steel plate

[0211] The range of the chemical composition of the base material steel plate included in the steel plate of the present embodiment is the same as that of the chemical composition of the steel member of the present embodiment described above, and the reasons for the limitation are also the same.

[0212] The chemical composition of the base steel plate can be obtained, for example, by taking a position (1 / 4 depth position) of the base steel plate 1 / 4 of the thickness from the surface in the thickness direction as a representative position and performing elemental analysis at that position using a conventional method such as ICP.

[0213] (B2) Oxide scale of steel plate

[0214] The oxide scale of the steel plate of this embodiment is 90 pieces / mm. 2 Densities above this have cracks.

[0215] As described later, the steel plate of the present embodiment effectively utilizes O of the oxide scale formed on the surface of the base steel plate by hot rolling, etc. to decarburize the base steel plate. In the case of decarburization by annealing in the shape of a steel coil (box annealing), the plates are more tightly fitted and sealed inside the steel coil, so the discharge of CO as a decarburization reaction cannot be promoted, and uniform decarburization cannot be obtained in the length and width directions of the steel coil. In contrast, by introducing cracks in the oxide scale, a discharge path for CO is formed, and the decarburization reaction is carried out rapidly and uniformly. In order to obtain the above-mentioned effect, the steel plate of the present embodiment controls the crack density of the oxide scale.

[0216] The crack density of the oxide scale can be obtained by SEM observation of the surface.

[0217] Avoid the end of the steel plate (for example, within 50 mm from the end) and take a sample of about 15 mm square. At this time, be careful not to peel off the oxide scale, and cut out a size larger than 15 mm square as needed. Observe the surface with oxide scale by SEM, obtain BSE image, and count the crack density using the cutting method. Avoid the end of the sample (for example, within 2 mm from the end) by SEM observation to form a 50000μm 2 Observe at 500 times in the above / 1 field of view. If observed through BSE image (or COMPO image), a clear contrast difference between oxide scale and crack can be confirmed. Cut the obtained BSE image (or COMPO image) into 10 vertical partitions and 10 horizontal partitions, count the number of cracks overlapping with the cutting line, and convert it into number density. Observe any 10 fields of view, and take the average value of the crack density of each field of view as the crack density of oxide scale.

[0218] (B3) Steel plate coating

[0219] The steel sheet of this embodiment may have a coating (coating) on ​​a part of the surface (or the entire surface). The coating may be an Al-based coating mainly composed of Al, or a Zn-based coating mainly composed of Zn. The Al-based coating refers to a coating containing 70% by mass or more of Al, and the Zn-based coating refers to a coating containing 70% by mass or more of Zn.

[0220] (B4) Shape of steel plate

[0221] The shape of the steel plate of the present embodiment is not particularly limited. That is, the steel plate may be a flat plate or a customized property material obtained by joining steel plates having different strengths and plate thicknesses.

[0222] (C) Method for manufacturing steel plate

[0223] The steel plate steel member of the present embodiment can obtain the effect as long as it has the above-mentioned characteristics regardless of the manufacturing method, and a manufacturing method including the steps shown below is preferred because stable manufacturing can be performed.

[0224] (I) Billet manufacturing process, manufacturing a billet having a predetermined chemical composition

[0225] (II) Hot rolling process: heating the steel slab and hot rolling it to produce a hot-rolled steel sheet

[0226] (III) Coiling step: Coiling the hot-rolled steel sheet

[0227] (IV) a light reduction step of performing light reduction on the hot rolled steel sheet after the coiling step

[0228] Each step is described below. Steps and conditions not described below can be appropriately carried out according to known methods.

[0229] (I) Billet Manufacturing Process

[0230] The steel billet manufacturing step manufactures a steel billet such as a slab having the preferred chemical composition of the steel plate according to the present embodiment described above.

[0231] Under known conditions, molten steel adjusted to a predetermined chemical composition may be formed into a steel billet by continuous casting or the like.

[0232] (II) Hot rolling process

[0233] The hot rolling step heats the obtained steel slab and performs hot rolling to produce a hot-rolled steel sheet. In the hot rolling step, iron oxide scale (hot rolling scale) is formed on the surface of the steel sheet.

[0234] The hot rolling conditions are not particularly limited and may be appropriately set within a known range of conditions depending on the properties required of the steel sheet.

[0235] (III) Coiling process

[0236] The coiling step is to coil the hot-rolled steel sheet obtained in the hot rolling step into a coil.

[0237] The conditions such as the coiling temperature are not particularly limited.

[0238] (IV) Soft pressing process

[0239] The light reduction process is to unwind the steel coil and perform light reduction on the hot-rolled steel sheet with hot-rolled scale formed on the surface. The aforementioned scale cracks can be introduced by performing light reduction with a reduction rate of 0.2% or more. There is no particular upper limit to the reduction rate, but it is not preferred to perform a reduction rate of 10.0% or more because the scale will peel off. The reduction rate is preferably less than 5.0%, or less than 2.0%, or less than 1.0%. As a means of introducing the aforementioned amount of scale cracks, shot peening can be performed on the hot-rolled steel sheet in conjunction with or instead of light reduction.

[0240] As described above, a steel plate having a base steel plate having a predetermined chemical composition and an iron oxide scale formed on the surface of the base steel plate, wherein the iron oxide scale includes cracks at a predetermined density, can be obtained.

[0241] So far, as a case where a hot rolled sheet is subjected to a light reduction, there is a case where a temper rolling is performed before pickling. However, the purpose is generally to facilitate pickling. That is, the light reduction of a hot rolled sheet whose next step is not a pickling step will also increase the number of steps, so it is usually not implemented.

[0242] In contrast, the method for manufacturing a steel sheet according to the present embodiment performs light reduction on a steel sheet that has been subjected to hot-rolled sheet annealing without descaling (in a so-called black scale state) as described later. This can also provide effects that have not been previously anticipated.

[0243] (D) Manufacturing method of steel structure

[0244] The method for producing the steel member of the present embodiment is not limited, and the steel member can be produced by applying a production method including the following steps to the above-mentioned steel plate.

[0245] (V) a hot rolled sheet annealing step of annealing the hot rolled steel sheet after the soft rolling step

[0246] (VI) a pickling step as required, wherein the hot rolled steel sheet after the hot rolled steel sheet annealing step is pickled.

[0247] (VII) a cold rolling step as required, wherein the hot rolled steel sheet after the pickling step is cold rolled to produce a cold rolled steel sheet

[0248] (VIII) an annealing step as required, annealing the cold-rolled steel sheet after the cold rolling step

[0249] (IX) a plating step as required, wherein the cold-rolled steel sheet after the annealing step is plated.

[0250] (X) a heat treatment step of heat-treating the hot-rolled steel sheet after the hot-rolled sheet annealing step, or the cold-rolled steel sheet after the cold-rolling step, the annealing step, or the plating step to obtain a steel member

[0251] (V) Hot rolled sheet annealing process

[0252] Hot rolled sheet annealing step The steel sheet of the present embodiment (steel sheet having hot rolled scale with cracks introduced on the surface) is subjected to box annealing (BAF) in a coil state without descaling (in a so-called black scale state).

[0253] During annealing, the annealing atmosphere is set to an inert gas atmosphere (N2 atmosphere, H2 atmosphere, etc.), and annealing is performed at 650 to 950°C for 4 to 30 hours.

[0254] In this embodiment, the hot-rolled steel sheet with hot-rolled scale is annealed to perform decarburization using O in the scale as a decarburization source. Specifically, decarburization is performed by reacting C in the outermost layer of the base steel sheet with O in the scale to form CO gas. In addition, insufficient C is then supplied from the inside of the base steel sheet to the outermost layer, and the C forms CO gas, thereby further promoting the decarburization reaction.

[0255] However, if the annealing temperature is lower than 650°C or the annealing time is less than 4 hours, decarburization cannot be fully performed. On the other hand, if the annealing temperature is higher than 950°C or the annealing time is longer than 30 hours, the reduction reaction of the oxide scale ends and C continues to be supplied from the inside of the steel sheet to the surface layer, so the decarburization becomes shallow.

[0256] In addition, when the hot-rolled steel sheet in the form of a coil is subjected to box annealing, the more airtight the inside of the coil is, the CO gas discharge is suppressed, and thus uniform decarburization cannot be obtained in the length direction and width direction of the coil. Therefore, by introducing the aforementioned scale cracks, a decarburized layer can be obtained quickly and uniformly at any position. The hot-rolled steel sheet provided for the hot-rolled sheet annealing process is preferably 9 mm or less in thickness, 2100 mm or less in width, 2000 mm or less in outer shape when made into a coil, and 30 tons or less in weight of one coil.

[0257] (VI) Pickling process

[0258] The pickling process is to pickle the hot-rolled steel sheet after the hot-rolled sheet annealing process. The pickling solution can be hydrochloric acid or sulfuric acid. If the scale is not fully peeled off during pickling, shot peening can be performed before pickling to mechanically help peeling off the scale. The shot size can be, for example, #60. The pickling process can be omitted.

[0259] (VII) Cold rolling process

[0260] The cold rolling process is to cold roll the cold-rolled steel sheet after the pickling process. The reduction ratio is not particularly limited. From the perspective of ensuring good flatness, the cumulative reduction ratio of cold rolling is preferably set to 30% or more. On the other hand, in order to avoid the rolling load becoming too large, the cumulative reduction ratio of cold rolling is preferably set to 80% or less. The cold rolling process can be omitted.

[0261] (VIII) Annealing process

[0262] The cold rolled sheet is annealed in the annealing process. The annealing atmosphere is humidified to a high dew point in a wet hydrogen atmosphere at a temperature range of 700 to 950°C. For example, in a two-stage heating furnace with an open flame burner and a radiant tube, the temperature is heated to 560 to 650°C at an air-fuel ratio of 0.9 to 1.2, and heated to 700 to 950°C in an atmosphere with an oxygen potential of -1.5 or more, a hydrogen concentration of 1 to 20% by mass, and a dew point of -10°C to +30°C. It is preferred to maintain the temperature above 700°C for more than 30 seconds in a high dew point atmosphere containing hydrogen.

[0263] However, this annealing step may be omitted or performed under conditions other than those described above.

[0264] (IX) Plating process

[0265] The coating process forms a coating on the surface of the steel sheet to produce a coated steel sheet. There is no particular limitation on the coating method, and it can be an electroplating method headed by hot dip coating, vacuum evaporation method, cladding method, spray coating method, etc. The hot dip coating method is the most popular in industry.

[0266] Examples of the coating include Al-based plating containing Al and Zn-based plating containing Zn.

[0267] The plating step can be omitted.

[0268] When an Al-based plating layer is formed by hot-dip plating, Fe is often mixed in the plating bath as an impurity in addition to Al. In addition, as long as 70% by mass or more of Al is contained, Si, Ni, Mg, Ti, Zn, Sb, Sn, Cu, Co, In, Bi, Ca, mixed rare earth metals, etc. may be contained in the plating bath in addition to the above elements.

[0269] In the case of hot dip coating, the steel sheet after the annealing step may be cooled to room temperature and then heated again for coating, or may be cooled to 650 to 750° C. near the coating bath temperature (i.e., without temporarily cooling to room temperature) after the annealing step and then hot dip coated.

[0270] There is no particular limitation on the pre-treatment and post-treatment of plating, and it may be pre-coating, solvent coating, alloying treatment, temper rolling, etc. As alloying treatment, for example, it may be maintained at 450 to 800° C. In addition, as post-treatment, temper rolling is useful for shape adjustment, etc., and it may be reduced by 0.1 to 0.5%, for example.

[0271] (X) Heat treatment process

[0272] The heat treatment step is to heat treat the steel plate having a predetermined chemical composition after the above steps to produce a steel member. The heat treatment is performed, for example, under the following conditions: the steel plate obtained by the method described below is heated to Ac3 point to (Ac3 point + 300)°C at an average heating rate of 1.0 to 1000°C / sec, and cooled to below Ms point at an average cooling rate above the critical cooling rate.

[0273] When the heating rate is less than 1.0°C / sec, the productivity of the heat treatment decreases, which is not preferred. On the other hand, when the heating rate is more than 1000°C / sec, a mixed crystal structure is formed, and the bendability decreases, which is not preferred.

[0274] In addition, when the heat treatment temperature is lower than the Ac3 point (°C), ferrite remains after cooling, and the strength is insufficient, which is not preferred. On the other hand, when the heat treatment temperature is higher than the Ac3 point + 300°C, the structure becomes coarse and the hydrogen embrittlement resistance decreases, which is not preferred.

[0275] The upper critical cooling rate refers to the minimum cooling rate at which austenite is supercooled to form martensite without precipitating ferrite and pearlite in the structure. When cooling is performed at a rate lower than the upper critical cooling rate, ferrite and pearlite are formed, resulting in insufficient strength.

[0276] During heating, the temperature may be maintained within a range of ±10° C. of the heating temperature for 1 to 300 seconds.

[0277] Furthermore, after cooling to a temperature below the Ms point, a tempering treatment may be performed in a temperature range of about 100 to 600° C. in order to adjust the strength of the steel member.

[0278] The Ac3 point, Ms point and upper critical cooling rate are measured as follows.

[0279] A strip test piece with a width of 30 mm and a length of 200 mm was cut out from the steel plate of this embodiment, and the test piece was heated to 1000°C at a heating rate of 10°C / second in a nitrogen atmosphere, kept at this temperature for 5 minutes, and then cooled to room temperature at various cooling rates. The cooling rate was set from 1°C / second to 100°C / second at intervals of 10°C / second (wherein the next setting of 1°C / second was 10°C / second). The Ac3 point and the Ms point were determined by measuring the thermal expansion change of the test piece during heating and cooling.

[0280] In addition, the minimum cooling rate at which no ferrite phase precipitation occurs in each test piece cooled at the above cooling rate is taken as the upper critical cooling rate. In addition, the Ms point obtained from the thermal expansion change when cooling at a rate higher than the above critical cooling rate is taken as the Ms point of the steel member.

[0281] Here, during the above series of heat treatments, from heating to the temperature range of Ac3 point to (Ac3 point + 300) ° C to cooling to below the Ms point, that is, while cooling at a speed above the above critical cooling rate, hot forming such as hot stamping can be implemented. As hot forming, bending, deep drawing, bulging, hole expansion and flange forming (flanging) can be listed. In addition, if there is a means for cooling the steel plate at the same time as or just after forming, forming methods other than stamping, such as roll forming, can be applied to the present invention. According to the above thermal history, hot forming can be repeatedly implemented. In addition, the above series of heat treatments can be repeated many times.

[0282] As described above, the steel member of the present embodiment includes both a formed body formed by hot forming a steel plate and a flat plate subjected to only heat treatment.

[0283] Furthermore, as the steel member of the present embodiment, a steel member having regions with different strengths can be obtained by hot forming or heat treating a part of a steel plate as a raw material.

[0284] The above series of heat treatments can be implemented by any method, for example, heating can be implemented by high frequency heating, electric heating, infrared heating, furnace heating. In addition, cooling can also be implemented by water cooling, mold cooling, etc. In addition, the atmosphere in the heating furnace can also use city gas and nitrogen in addition to air. In addition, in order to suppress the generation of hydrogen during heat treatment, the dew point in the heating furnace can be controlled.

[0285] Example

[0286] Steels having the chemical compositions shown in Table 1A and Table 1B were melted to obtain slabs.

[0287] The obtained slab was hot rolled to produce a hot rolled steel sheet with a thickness of 3.2 mm and a width of 1000 mm, and then coiled at a temperature below 800° C. to produce a hot rolled steel coil with an outer shape of 1700 mm and a weight of 14 tons.

[0288] The obtained hot-rolled steel coils were subjected to light reduction at the reduction ratios described in Table 2.

[0289]

[0290]

[0291] Table 2

[0292]

[0293] Steel sheets (billets) of a predetermined size were cut out from the obtained lightly reduced steel coils and subjected to SEM observation according to the above-mentioned procedure to evaluate the crack density of the oxide scale.

[0294] Furthermore, the chemical composition at a 1 / 4 depth position of the steel plate was measured, and the result was the same as the chemical composition of the slab.

[0295] As shown in Table 2, B1 to B21 satisfying the scope of the present invention yielded base steel plates having a predetermined chemical composition and steel plates having a predetermined crack density of oxide scale. Comparative Examples b1 to b15 not satisfying the scope of the present invention did not satisfy the chemical composition or crack density of oxide scale.

[0296] The steel sheets shown in Table 2 were subjected to hot-rolled sheet annealing under the conditions shown in Table 3A.

[0297] In addition, a portion of the steel sheets (C2 to C30, c2 to c16) after hot-rolled sheet annealing was pickled and cold-rolled to obtain a cold-rolled steel sheet with a thickness of 1.6 mm. Furthermore, a portion of the cold-rolled steel sheets (C4 to C22, C24 to C30, c5 to c16) was subjected to Al hot-dip plating or Zn hot-dip plating.

[0298] The hot-rolled steel sheet after hot-rolled sheet annealing, or the cold-rolled steel sheet after pickling, cold rolling, annealing, or the cold-rolled steel sheet after pickling, cold rolling, annealing and plated during the annealing process (cooling process after holding), was subjected to heat treatment under the conditions shown in Table 3A to obtain a steel member. In the steel member obtained by heat-treating the plated steel sheet, an Fe-Al alloy layer containing a total of 70 mass % or more of Fe and Al, or an Fe-Zn alloy layer containing a total of 70 mass % or more of Fe and Zn was formed on the surface with a thickness of 5 to 100 μm.

[0299] The obtained steel member was cut out and subjected to GDS (glow discharge emission spectroscopy) according to the above-mentioned method to determine the B enrichment ratio and decarburization depth. In addition, the martensite volume fraction at the 1 / 4 depth position was measured. The results are shown in Table 3B.

[0300] Furthermore, the obtained steel members and coated steel members were subjected to hardness tests, tensile tests, and bending tests according to the following methods to evaluate Vickers hardness, tensile strength, bendability, and hydrogen embrittlement resistance. The results are shown in Table 3B.

[0301] <Vickers Hardness>

[0302] A cross-sectional observation sample was taken from a position 1 / 4 of the width (short side) from the end of the steel member in the width direction, and the Vickers hardness was measured at the 1 / 4 depth position and the 0.1 mm depth position according to JIS Z2244-1: 2020. The test force was 100 gf. Five measurements were performed at each depth, and the average value was taken as the hardness at that position.

[0303] <Tensile Strength>

[0304] The tensile test was carried out in accordance with the provisions of ASTM standard E8. After grinding the heat-saturated part of the steel member to a thickness of 1.2 mm, a half-size plate-shaped test piece of ASTM standard E8 (parallel part length: 32 mm, parallel part plate width: 6.25 mm) was taken in such a way that the test direction was parallel to the rolling direction. Then, a strain gauge (strain gauge length: 5 mm, for example, FLAB-5 manufactured by Tokyo Messaging Laboratory Co., Ltd.) was attached to the center of the width and length direction of the parallel part of the test piece, and a room temperature tensile test was carried out at a strain rate of 3 mm / min to measure the tensile strength (maximum strength).

[0305] In the present example, a case where the tensile strength was 1000 MPa or more was evaluated as high strength.

[0306] <Flexibility>

[0307] A bending test piece having a length of 60 mm in a direction parallel to the rolling direction and a length of 30 mm in a direction perpendicular to the rolling direction was taken from the heat-saturated portion of the steel member, and a bending test was performed on the test piece in accordance with the provisions of DA238-100.

[0308] During the test, the bending punch was aligned perpendicular to the rolling direction, and the bending angle at the maximum load was measured.

[0309] Since there is a correlation between the bending angle and the strength, in this embodiment, according to the tensile strength, the bending angles of more than 70 degrees when the tensile strength is less than 1500 MPa, more than 55 degrees when the tensile strength is greater than 1500 MPa and less than 2100 MPa, and more than 45 degrees when the tensile strength is greater than 2100 MPa are evaluated as having better bendability than the prior art.

[0310] <Hydrogen embrittlement resistance>

[0311] Regarding hydrogen embrittlement resistance, a 4-point bending test was performed on the test piece, and the evaluation was performed based on the amount of hydrogen Hc that can be absorbed in the test piece up to the limit where no cracks occur. Specifically, as a test piece, a strip-shaped test piece with a width of 8 mm and a length of 68 mm was cut out, avoiding the end of the steel member to be evaluated. Then, after a strain gauge (strain gauge length: 5 mm, for example, FLAB-5 manufactured by Tokyo Messaging Laboratory Co., Ltd.) similar to that in the tensile test was pasted on the center of the width direction and the length direction of the surface of the test piece, the steel member to be evaluated was bent along the length direction of the test piece with a 4-point supported fixture to a deformation equivalent to 3 / 5 of the tensile strength measured by the above tensile test. As a fixture, a fixture with an inner pin (two inner force application points) with an interval of 10 mm and an outer pin (two outer support points) with an interval of 60 mm was used.

[0312] For multiple test pieces with different amounts of hydrogen absorbed (hydrogen absorption amount), the presence or absence of cracks was observed, and the maximum (limit) hydrogen amount Hc (mass ppm) at which no cracks were generated was determined. In the case of steel members with Fe-Al coating, the hydrogen absorption amount was changed by changing the furnace dew point in the heat treatment process, and it was observed whether cracks occurred within 72 hours from the 4-point bending test. In addition, in the case of uncoated steel members or steel members with Fe-Zn coating, multiple test pieces were immersed in ammonium thiocyanate solutions of different concentrations after the 4-point bending test to absorb hydrogen, and it was observed whether cracks occurred within 72 hours after the immersion. Regarding the hydrogen absorbed by the steel member, the amount of diffusible hydrogen released by heating at 100°C / hour to 250°C in the temperature increase hydrogen analysis was taken as the amount of hydrogen contained in the steel member.

[0313] In this embodiment, for steel components with a tensile strength of 1500 or more and less than 2000 MPa, when the hydrogen amount Hc is 0.7 mass ppm or more, for steel components with a tensile strength of 2000 or more and less than 2500 MPa, when the hydrogen amount Hc is 0.5 mass ppm or more, and for steel components with a tensile strength of 2500 MPa or more, when the hydrogen amount Hc is 0.3 mass ppm or more, it is evaluated as excellent in hydrogen embrittlement resistance.

[0314] In addition, according to the above-mentioned principles, the finite element method is used to calculate the maximum principal plastic strain at the center of the curved outer surface layer.

[0315]

[0316]

[0317] As shown in Tables 1 to 3B, the inventive examples C1 to C30 satisfying the scope of the present invention have good structures and properties, high strength, and excellent bendability and hydrogen embrittlement resistance. However, the comparative examples c1 to c16 not satisfying the scope of the present invention have insufficient chemical composition and structure formation, and at least one of strength, bendability, and hydrogen embrittlement resistance is poor.

[0318] Industrial Applicability

[0319] According to the present invention, a high-strength steel member and steel plate having excellent collision characteristics can be obtained. The steel member of the present invention is particularly suitable for use as a frame member of an automobile.

Claims

1. A steel component, characterized in that: It has a chemical composition containing the following elements by mass %: C: 0.10 to 0.70%, Si: 3.00% or less, Mn: 0.01~3.00%, P: 0.100% or less, S: 0.0100% or less, N: 0.020% or less, O: 0.010% or less, B:0.0002~0.0200%、 Ti: 0~0.200%, Cr:0~1.00%、 Mo: 0-1.00%, Ni: 0-2.00%, Nb: 0-0.10%, Cu: 0-2.00%, V:0~1.00%、 Ca: 0~0.020%, Mg: 0~0.020%, Al:0~1.00%、 Sn: 0~1.00%, W:0~2.00%、 Sb: 0-1.00%, Zr:0~1.00%、 Se: 0~1.00%, Bi: 0~1.00%, As: 0~1.00%, Ta: 0~1.00%, Re: 0~1.00%, Os: 0~1.00%, Ir:0~1.00%、 Tc: 0~1.00%, Co: 0-1.00%, REM: 0-0.30%, and Balance: Fe and impurities, When a position at a depth of 1 / 4 of the thickness from the surface in the thickness direction is referred to as a 1 / 4 depth position, the maximum B content in the range from the surface to a depth of 10 μm in the thickness direction is 5 times or more the B content at the 1 / 4 depth position, When the C content is measured from the surface along the thickness direction using GDS and the distance from the surface to the position where the C content first reaches the C content at the 1 / 4 depth position is recorded as the decarburization depth, the decarburization depth is 20 μm or more, The Vickers hardness at the 1 / 4 depth position is 310-890.

2. The steel member according to claim 1, characterized in that When a position at a depth of 0.1 mm from the surface in the thickness direction is referred to as a 0.1 mm depth position, the Vickers hardness at the 0.1 mm depth position is 0.95 times or less of the Vickers hardness at the ¼ depth position.

3. The steel member according to claim 2, characterized in that The Vickers hardness at the 1 / 4 depth position is 310-450, When a steel member having a plate thickness of 1.6 mm is deformed to a bending angle of 50 degrees, the maximum principal plastic strain at the center of the outer surface of the bending surface is less than 0.

340.

4. The steel member according to claim 2, characterized in that The Vickers hardness at the 1 / 4 depth position is greater than 450 and is less than 530, and the Vickers hardness at the 0.1 mm depth position is less than 0.90 times the Vickers hardness at the 1 / 4 depth position. When a steel member with a plate thickness of 1.6 mm is deformed to a bending angle of 50 degrees, the maximum principal plastic strain at the center of the outer surface of the bending surface is less than 0.

310.

5. The steel member according to claim 2, characterized in that: The Vickers hardness at the 1 / 4 depth position is greater than 530 and is less than 700, and the Vickers hardness at the 0.1 mm depth position is less than 0.88 times the Vickers hardness at the 1 / 4 depth position. When a steel member having a plate thickness of 1.6 mm is deformed to a bending angle of 50 degrees, the maximum principal plastic strain at the center of the outer surface of the bending surface is less than 0.

280.

6. The steel member according to claim 2, characterized in that The Vickers hardness at the 1 / 4 depth position is greater than 700 and is less than 890, and the Vickers hardness at the 0.1 mm depth position is less than 0.86 times the Vickers hardness at the 1 / 4 depth position. When a steel member with a plate thickness of 1.6 mm is deformed to a bending angle of 50 degrees, the maximum principal plastic strain at the center of the outer surface of the bending surface is less than 0.

260.

7. The steel member according to any one of claims 1 to 6, characterized in that: An alloy layer is also provided on the surface.

8. The steel member according to claim 7, characterized in that The alloy layer is a Fe-Al alloy layer.

9. The steel member according to claim 7, characterized in that The alloy layer is a Fe-Zn alloy layer.

10. A steel plate, characterized in that: It has: Base steel plate, and The iron oxide scale formed on the surface of the base steel plate, The base steel plate has a chemical composition containing the following elements by mass %: C:0.10~0.70%、 Si: 3.00% or less, Mn: 0.01~3.00%, P: 0.100% or less, S: 0.0100% or less, N: 0.020% or less, O: 0.010% or less, B: 0.0002~0.0200%, Ti: 0~0.200%, Cr: 0~1.00%, Mo: 0~1.00%, Ni: 0~2.00%, Nb: 0~0.10%, Cu: 0~2.00%, V: 0~1.00%, Ca: 0~0.020%, Mg: 0~0.020%, Al: 0~1.00%, Sn: 0~1.00%, W: 0-2.00%, Sb: 0-1.00%, Zr: 0-1.00%, Se: 0-1.00%, Bi: 0-1.00%, As: 0-1.00%, Ta: 0-1.00%, Re: 0-1.00%, Os: 0-1.00%, Ir: 0-1.00%, Tc: 0-1.00%, Co: 0-1.00%, REM: 0-0.30%, and the balance: Fe and impurities, the iron oxide scale is 90 pieces / mm 2 Densities above this include cracks.