Multifilament
By using triangular hollow fibers with a monofilament fiber with a monofilament fiber of less than 5.0dtex in clothing, the problems of hollow fibers collapse and uneven cross-section during clothing use are solved, and fluffy and soft texture are achieved. Combined, the product quality has been improved.
Patent Information
- Application Number
- CN202380028808.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-30
- Filing Date
- 2023-03-27
- Publication Date
- 2024-11-08
AI Technical Summary
Existing hollow fibers are prone to collapse due to processing force during clothing use, resulting in reduced lightness and fluffiness, and uneven cross-section after the single filament fineness is refined, resulting in deterioration of product quality.
A triangular hollow fiber with a monofilament fiber of 5.0dtex or less is used to bring a repulsive volume effect by the projections on the triangle sides of the fiber cross-section, combining the appropriate shape and hollowness to form a multifilament with fluffy and soft texture.
It realizes that hollow fibers are not easy to collapse, maintain fluffy and soft texture, and improves the quality and durability of clothing products.
Smart Images

Figure CN118922593A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a multifilament yarn containing hollow fibers with a special cross section suitable for knitted fabrics for clothing applications, which can provide a fabric having excellent bulkiness, texture and product quality. Background Art
[0002] Synthetic fibers such as polyamide and polyester are widely used for clothing and industrial purposes because of their excellent strength, chemical resistance, heat resistance, etc.
[0003] In particular, hollow fibers obtained by hollowing out fibers for the purpose of imparting a light feel are widely used for clothing or industrial purposes. Furthermore, in order to improve not only the light feel but also the bulkiness or to obtain a change in texture, various profile-forming techniques have been proposed, such as making the hollow part irregular or forming a cross-sectional shape with a plurality of protrusions.
[0004] For example, Patent Document 1 or Patent Document 2 proposes a shaped hollow fiber having six or more convex portions and one or more circular hollow holes radially outward from the center of a monofilament. In addition, Patent Document 3 proposes a shaped hollow fiber having a triangular hollow hole and six protrusions in the extension direction of each side for use in woven fabrics, knitted fabrics, and terry fabrics.
[0005] [Prior art literature]
[0006] [Patent Document]
[0007] Patent Document 1: Japanese Patent Application Publication No. 2014-210989
[0008] Patent Document 2: Japanese Patent Application Publication No. 2020-70530
[0009] Patent Document 3: Japanese Patent Laid-Open No. 9-302518 Summary of the invention
[0010] (Problems to be solved by the invention)
[0011] For clothing applications, since the single fiber fineness is finer than that for industrial applications, if the hollow ratio is high, the hollow part is easily collapsed by the force applied from the outside during processing, and the lightness is reduced. Furthermore, the fluffiness is also reduced as the rebound force is reduced. Therefore, the hollow part of the hollow fiber is required to be not easy to collapse and have excellent fluffiness.
[0012] The irregular hollow fibers described in Patent Documents 1 and 2 are easily deformed in cross section due to the circular hollow portion, and the fluffy property is insufficient due to the hollow collapse. In addition, in the hollow fiber with six protrusions described in Patent Document 3, the protrusion shape creates a gap to maintain the fluffy property. However, since the single fiber fineness is relatively coarse, there is a problem of hard texture in clothing applications.
[0013] Furthermore, if the fineness of the single yarn is reduced in order to make the texture softer, the cross-sectional formability is deteriorated due to the special cross-sectional structure, and the cross-sectional unevenness of the single yarn is easily generated. This causes the problem of deteriorating product quality due to the ripples when forming the cloth.
[0014] The present invention is made to solve the above-mentioned problems, and the object is to provide a multifilament comprising hollow fibers with fine single filaments, which are not easily collapsed and have irregular cross-sections without uneven cross-sections, that is, a multifilament that can obtain a woven fabric with excellent bulkiness, soft texture and product quality.
[0015] (Technical means to solve the problem)
[0016] In order to solve the above-mentioned problems, the present invention adopts the following means.
[0017] (1) A multifilament comprising a hollow fiber having a triangular shape in the cross section of a single fiber and a protrusion on the extension line of each side of the triangle, wherein the single fiber fineness of the hollow fiber having a triangular shape is 5.0 dtex or less and the CV% of the degree of irregularity is 2.0 or less.
[0018] (2) The multifilament according to (1), wherein the hollow ratio of the hollow fiber with a profiled cross section is 20% or less and the profile degree is 1.1 to 2.0.
[0019] Effects of the Invention
[0020] According to the present invention, a multifilament comprising hollow fibers having fine single filaments, which are not easily collapsed and have no cross-sectional unevenness can provide a fabric (woven fabric, knitted fabric) having excellent bulkiness, soft texture and product quality. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 One embodiment of a production apparatus which can be preferably used for the multifilament production method of the present invention is shown.
[0022] Figure 2 One embodiment of the shape of the ejection hole of the spinneret used in the present invention is shown.
[0023] Figure 3A It is a schematic diagram explaining the shape of the cross section of the fiber of the present invention.
[0024] Figure 3B It is a schematic diagram explaining the shape of the cross section of the fiber of the present invention.
[0025] Figure 3C It is a schematic diagram explaining the shape of the cross section of the fiber of the present invention.
[0026] Figure 4 One embodiment of the shape of the ejection hole of the spinneret used in the comparative example is shown.
[0027] Figure 5 A schematic diagram showing the shape of a fiber cross section of a comparative example.
[0028] Figure 6 One embodiment of the shape of the ejection hole of the spinneret used in the comparative example is shown.
[0029] Figure 7 A schematic diagram showing the shape of a fiber cross section of a comparative example.
[0030] Figure 8 One embodiment of the shape of the ejection hole of the spinneret used in the comparative example is shown.
[0031] Fig. 9 A schematic diagram showing the shape of a fiber cross section of a comparative example. DETAILED DESCRIPTION
[0032] Hereinafter, the present invention will be described in more detail.
[0033] The single-filament fineness of the profiled cross-section hollow fiber in the present invention is 5.0 dtex or less. In this way, the multifilament containing the profiled cross-section hollow fiber in the present invention is suitable for clothing applications requiring a soft texture. By making the single-filament fineness 5.0 dtex or less, a clothing product with excellent soft texture can be obtained. In the case where the single-filament fineness is greater than 5.0 dtex, the texture becomes hard. Preferably, the single-filament fineness is 4.0 dtex or less. The finer the single-filament fineness, the softer the texture, but from the viewpoint of the fluffiness in order to reduce the hollow rate, the single-filament fineness is preferably 0.8 dtex or more.
[0034] The number of filaments of the multifilament of the present invention is preferably 5 or more. When the number of filaments is 5 or more, the excluded volume effect by the protrusions can be exerted, and bulkiness can be expressed.
[0035] The cross-sectional shape of the fiber of the special-shaped cross-section hollow fiber of the present invention is that a protrusion protrudes from the triangle of the hollow part to the extension line of each side. FIG. 3A to FIG. 3CThe illustrated shape. By having a protruding protrusion on the extension line of each side of the triangle of the hollow part, the exclusion volume effect caused by the interference between the monofilaments in the multifilament is exerted. In this way, the spaces between the monofilaments can be ensured and the fluffiness can be obtained. In the case of no protrusion, the spaces between the monofilaments cannot be fully obtained, and the fluffiness cannot be obtained. Furthermore, by making the hollow part triangular (hereinafter referred to as triangular hollow), the hollow part is not easy to collapse even if an external force is applied during high-order processing, and the fluffiness can be maintained. The protrusion and the triangular hollow complement each other to obtain excellent fluffiness when the multifilament of the present invention is formed into a woven fabric. In the case where the hollow shape is circular or a polygon with more than four sides, the hollow part is easy to collapse during high-order processing, and sufficient fluffiness cannot be obtained.
[0036] The degree of irregularity of the hollow fiber with irregular cross section in the present invention is preferably 1.1 to 2.0. Figure 3B and Figure 3C The degree of irregularity is explained. Figure 3B , Figure 3C The radius of the circumscribed circle A of the three outermost points (point g, point h, point i) of the protrusions protruding from the intersection points (point d, point e, point f) of the protrusions is set as radius Ra. The radius of the circumscribed circle B passing through the three intersection points (point d, point e, point f) is set as radius Rb.
[0037] The irregularity is defined by irregularity=radius Ra / radius Rb.
[0038] The degree of irregularity of the hollow fiber with irregular cross section in the present invention is obtained by measuring the degree of irregularity of the hollow fiber with irregular cross section in all the fibers and taking the average value.
[0039] The higher the degree of irregularity, the longer the protrusions, and the lower the degree of irregularity, the shorter the protrusions. When the protrusions are too long or too short, the bulkiness is excellent due to the exclusion volume effect caused by the interference between the monofilaments, so the degree of irregularity of the hollow fiber with an irregular cross section is preferably 1.1 to 2.0. More preferably, the degree of irregularity is 1.1 to 1.5.
[0040] In the multifilament yarn of the present invention, the CV% of the irregularity of the profiled cross-section hollow fiber is 2.0 or less. The so-called CV% of the irregularity here refers to the value obtained by dividing the standard deviation value of the irregularity of all yarns by the average value of the irregularity. The higher the CV% of the irregularity, the more uneven the protrusion length. By making the CV% of the irregularity less than 2.0, a clothing product with excellent product quality can be obtained. The product quality here refers to the cleanliness of the surface of the fabric observed comprehensively, such as the presence or absence of ripples, streaks, and hairiness that become product defects. If the CV% of the irregularity exceeds 2.0, any one of ripples, streaks, and hairiness will occur, or any of the defects will occur in combination, and the product quality will be poor. In the multifilament yarn of the present invention, the CV% of the irregularity of the profiled cross-section hollow fiber is preferably 1.5 or less.
[0041] The hollow ratio of the hollow fiber with a special cross section in the present invention is preferably 20% or less. Figure 3B and Figure 3C The hollowness will be described below. The radius of the circumscribed circle C of the triangular hollow is defined as radius Rc.
[0042] Hollowness is calculated by Hollowness = (radius Rc / radius Rb) 2 ×100 to define.
[0043] The higher the hollow ratio, the easier it is for the hollow part to collapse due to the force applied from the outside, and the lower the fluffiness. By setting the hollow ratio of the profiled cross-section hollow fiber to 20% or less, excellent fluffiness accompanied by rebound force is obtained. The hollow ratio of the profiled cross-section hollow fiber is more preferably 15% or less, and particularly preferably 10% or less.
[0044] The strength of the multifilament of the present invention is preferably 1.5 cN / dtex or more. By setting it within this range, the fabric tearing strength, knitted fabric rupture strength, and abrasion resistance are excellent, and practical durability of clothing products can be obtained. More preferably, it is 2.0 cN / dtex or more.
[0045] The U% of the multifilament of the present invention is preferably 3.0% or less. By setting it in this range, the unevenness of the fineness is reduced, and the streaks when formed into a woven fabric are suppressed, so the quality is improved. It is more preferably 2.0% or less.
[0046] Next, an example of the method for producing a multifilament yarn according to the present invention will be specifically described.
[0047] Figure 1 One embodiment of a production apparatus preferably used in the multifilament production method of the present invention is shown.
[0048] The multifilament of the present invention is formed by melting a polymer, metering and conveying it with a gear pump, and finally extruding it from the ejection hole provided in the spinneret 1 to form individual filaments. Figure 1The heating cylinder 2 shown in the figure is provided with a full circumference for slow cooling, and is cooled and solidified to room temperature by a cooling device 3. Then, each filament moves through a spinning cylinder 4, and is oiled and bundled by an oil supply device 5, interlaced by a fluid rotating nozzle device 6, stretched by a traction roller 7 and a stretching roller 8, and then wound by a winding device 9.
[0049] The constituent components of the hollow fiber with a special cross section in the present invention are not particularly limited, but preferably thermoplastic synthetic resins such as polyester and polyamide are used. In particular, polyamide is more preferred because it can provide a soft texture and has excellent abrasion resistance.
[0050] The higher the viscosity of the thermoplastic synthetic resin, the easier it is to obtain high profile, but if the profile is high, the protrusions will fibrillate due to friction, thereby deteriorating product quality. In addition, the lower the viscosity of the thermoplastic synthetic resin, the more difficult it is to obtain profile and sufficient fluffiness.
[0051] In the present invention, when the thermoplastic synthetic resin is polyamide, the 98% sulfuric acid relative viscosity of the polyamide resin scraps is preferably in the range of 2.5 to 4.0. When the thermoplastic synthetic resin is polyester, the o-chlorophenol (hereinafter referred to as OCP) relative viscosity of the polyester resin scraps is preferably in the range of 0.60 to 0.90. By making the relative viscosity within this range, the desired fiber cross-sectional shape, profile, and hollow ratio can be obtained. In addition, from the viewpoint of yarn making properties, the extrusion pressure of the molten polymer during spinning and its rising speed over time can be suppressed, and the excessive load on the production equipment or the extension of the replacement cycle of the spinneret can be sought, and productivity can be ensured, so it is more preferable to make the relative viscosity within this range.
[0052] In the production of the multifilament of the present invention, the realization of the desired fiber cross-sectional profile and hollow ratio also depends on the single filament fineness of the multifilament, but it is preferred to set a slow cooling zone under the spinneret to maintain the ambient temperature at a high temperature, fully promote the orientation relaxation of the polymer, and then rapidly solidify in the cooling zone to fix the fiber cross-sectional shape.
[0053] In the manufacture of the multifilament of the present invention, it is important to cool the monofilaments uniformly one by one by means of the cooling device 3, and to cool by means of an annular cooling device. If the method is exemplified, either an annular cooling device (RIQ) that blows cooling and rectifying air from the outer periphery toward the center, or an annular cooling device (ROQ) that blows cooling and rectifying air from the center toward the outer periphery is used. By using an annular cooling device, the CV% of the degree of irregularity can be controlled to be less than 2%, especially when the monofilament fineness is fine. In the case of a single-flow cooling device that blows cooling and rectifying air from one direction, the CV% of the degree of irregularity increases due to the difference in cooling of the monofilaments near the front side of the blowing port and the monofilaments on the inner side.
[0054] In order to achieve the desired profile and hollowness of the fiber cross section in the present invention, it is preferred that the solidification point of the polymer is closer to the position after ejection. The reason is that the elastic force acting on the polymer is directed outward and acts in the direction that minimizes the surface area (surface tension), so the working time of the surface tension is shortened. In other words, it is preferred that the polymer that comes out from the lower surface of the heating cylinder 2 and enters the cooling area has its solidification point as close to the upper end of the cooling area as possible.
[0055] Therefore, it is preferred that the vertical distance LS from the lower surface of the spinneret 1 to the upper end of the cooling air blowing portion of the cooling device 3 (hereinafter referred to as the cooling start distance LS) is 20 mm to 100 mm. By making the cooling start distance LS 20 mm or more, the poor polymer ejection caused by the cooling of the spinneret surface can be suppressed, and the CV% of the irregularity can be suppressed. In addition, by making the cooling start distance LS 100 mm or less, the polymer is solidified before the cross section is close to a circle due to surface tension, and the desired irregularity and hollowness of the fiber cross section can be achieved.
[0056] The spinning drum 4 is provided for the multifilaments so that the descending airflow generated by the annular cooling device and the traveling yarn group is uniformly applied to the multifilaments. The vertical length Lb of the spinning drum 4 (hereinafter referred to as the spinning drum length Lb) also varies depending on the total fineness, but is preferably greater than 200 mm. By making the spinning drum length Lb greater than 200 mm, the descending airflow generated by the traveling yarn is stabilized, the uneven solidification point caused by the shaking of the traveling yarn can be suppressed, and the CV% of the irregularity can be suppressed.
[0057] Furthermore, the spinning drum 4 is preferably provided between a lower position of the cooling device 3 and 1800 mm in the downstream direction, and the upper end of the spinning drum is particularly preferably provided right below the cooling device.
[0058] In addition, as an effective method for bringing the solidification point closer to the upstream side, it is preferred to increase the cooling wind speed, and the cooling wind speed at the lower end of the cooling zone is preferably in the range of 0.40 m / sec to 0.60 m / sec. By making the cooling wind speed 0.40 m / sec or more, the heat exchange rate of the polymer is increased, and the solidification point is closer to the upper end of the cooling zone, so the desired fiber cross-sectional profile and hollowness can be achieved. On the other hand, from the perspective of operability, the cooling wind speed is preferably 0.60 m / sec or less.
[0059] Similarly, the cooling air temperature in the cooling zone is also an important factor in heat exchange, and the cooling air temperature is preferably below 20° C. By setting the cooling air temperature below 20° C., the heat exchange rate of the polymer is accelerated, and the solidification point is close to the upper end surface of the cooling zone, so the desired irregularity and hollowness can be achieved.
[0060] [Example]
[0061] Hereinafter, the present invention will be described in further detail by way of examples.
[0062] A.Total fineness
[0063] The fiber sample was set at a ruler of 1.125 m / week and rotated 500 times to make a wire arc winding bobbin. After drying in a hot air dryer (105±2°C×60 minutes), the mass of the bobbin was measured using a balance, and the fineness was calculated by multiplying the value by the official moisture content (also known as: official moisture regain). In addition, the official moisture content of polyamide is 4.5%.
[0064] B. Relative viscosity of sulfuric acid ηr
[0065] 0.25 g of a polyamide scrap sample was dissolved in 100 ml of 98% by mass sulfuric acid to give 1 g, and the flow time (T1) at 25°C was measured using an Ostwald viscometer. Next, the flow time (T2) of only 98% by mass sulfuric acid was measured. The ratio of T1 to T2, i.e., T1 / T2, was defined as the relative viscosity of sulfuric acid.
[0066] C. OCP relative viscosity IV
[0067] 0.8 g of polyester scrap sample was dissolved in 10 mL of OCP with a purity of 98% or more, and the flow time (T3) at 25°C was measured using an Ostwald viscometer. Then, the flow time (T4) of only OCP was measured. The ratio of T3 to T4, i.e., T3 / T4, was defined as the relative viscosity of OCP.
[0068] D. Hollowness, irregularity, irregularity CV%
[0069] Thin scraps were cut from any position of the yarn in the cross-sectional direction, and all the filaments in the cross-sectional direction were photographed using a transmission microscope. The images were printed out at a magnification of 1000 times using a printer (SCT-P66 manufactured by Mitsubishi Electric Corporation), input using a scanner (GT-5500WINS manufactured by Epson Corporation) (black and white photo, 400 dpi), and magnified to 1500 times on a monitor using image processing software (WIN ROOF). The hollow ratio, irregularity, and irregularity CV% were calculated as follows.
[0070] (a) If Figure 3B and Figure 3C As an example, circumscribed circle A, circumscribed circle B, and circumscribed circle C are drawn.
[0071] Circumscribed circle A: A circle passing through the outermost points (point g, point h, point i) of the protrusions protruding from the intersection points (point d, point e, point f) of the protrusions
[0072] Circumscribed circle B: A circle passing through the three intersection points (point d, point e, point f)
[0073] Circumscribed circle C: A circle passing through the hollow triangle (point a, point b, point c)
[0074] (b) The radii of the circumscribed circles are calculated as the radius Ra, the radius Rb, and the radius Rc.
[0075] (c) Hollowness
[0076] Hollowness = (radius Rc / radius Rb) 2 ×100
[0077] The fiber cross sections of all the yarns were measured, and the average value was defined as the hollowness.
[0078] (d) Degree of irregularity, CV% of degree of irregularity
[0079] Degree of irregularity = radius Ra / radius Rb
[0080] The fiber cross sections of all yarns were measured, and the average value was defined as the irregularity. In addition, the standard deviation of the irregularity of all yarns was calculated, and the value obtained by dividing the standard deviation by the average value of the irregularity was defined as the CV% of the irregularity.
[0081] E. Strength, elongation
[0082] The fiber sample was measured for tensile strength and elongation according to JIS L1013 (2021). As the test conditions, the type of testing machine was a constant speed tension type, and the test was conducted with a chuck interval of 50 cm and a tensile speed of 50 cm / min. Furthermore, when the strength at the time of cutting was less than the maximum strength, the maximum strength and the elongation at that time were measured.
[0083] The strength and elongation were calculated using the following formula.
[0084] Strength = strength at cutting (cN) / total fineness (dtex)
[0085] Elongation = elongation at break (%).
[0086] FU%
[0087] The fiber sample was measured using USTER TESTER V manufactured by Zellweger Uster with a sample length of 500 m and a yarn measurement speed of 100 m / min to measure U% (Half). This operation was repeated 5 times, and the numerical average of the results was defined as U%.
[0088] G. Fabric Evaluation
[0089] (a) Fluffiness
[0090] For the fabric produced by the same method as in the example, the fabric cross section at any five locations was photographed using a scanning electron microscope, the fiber cross section and the void portion were trimmed to a fixed size and binarized, and the ratio (%) of the void portion was calculated. The average of the five values was set as the bulkiness. Four levels were evaluated according to the following criteria.
[0091] S: Fluffiness 30% or more
[0092] A: Fluffiness 25% or more and less than 30%
[0093] B: Fluffiness 20% or more and less than 25%
[0094] C: Fluffiness less than 20%
[0095] S, A, and B are regarded as acceptable bulkiness.
[0096] (b) Texture
[0097] The fabrics made by the same method as in the example were evaluated for softness by 5 inspectors with rich experience in evaluating texture. Comparative Example 3 was used as a reference for relative evaluation. The following evaluation scores of each inspector were taken, and when the average value of the 5 inspectors (rounded off to the nearest decimal point) was 5, it was considered S, when it was 4, it was considered A, when it was 3, it was considered B, and when it was 1 to 2, it was considered C.
[0098] 5 points: Excellent
[0099] 4 points: Slightly excellent
[0100] 3 points: Average
[0101] 2 points: slightly worse
[0102] 1 point: poor
[0103] S, A, and B are considered to be of qualified quality.
[0104] (c) Product quality
[0105] The appearance of the fabric produced by the same method as in the example was comprehensively observed by five inspectors (five persons) with rich experience in appearance inspection, and the appearance of the fabric surface, which was judged based on the following criteria, was evaluated based on the presence or absence of ripples, streaks, hairiness, etc., which are defects of the product. The evaluation scores of the five inspectors were taken, and when the average value (rounded off to the nearest decimal point) of the five inspectors was 5, it was considered S, when it was 4, it was considered A, when it was 3, it was considered B, and when it was 1 to 2, it was considered C.
[0106] 5 points: no ripples, stripes, or hairiness
[0107] 4 points: no ripples or streaks
[0108] 3 points: No ripples
[0109] 2 points: No streaks
[0110] 1 point: no hairiness
[0111] When S, A, and B are used, the product quality is considered qualified.
[0112] [Example 1]
[0113] (Manufacturing of Fiber)
[0114] As polyamide, nylon 6 crumbs with a sulfuric acid relative viscosity ηr of 3.1, a melting point of 225°C, and containing 0.3% by weight of titanium oxide were used, and dried by a conventional method to a moisture content of 0.03% or less. The obtained nylon 6 crumbs were melted at a spinning temperature (melting temperature) of 265°C and ejected from a spinneret (ejection amount 29.4 g / min). As a spinneret, a nylon 6 crumb with 24 holes and 1 sliver was used. Figure 2 The spinneret with the ejection hole shape shown in the figure forms Figure 3A The fiber cross-sectional shape shown is a profiled hollow fiber.
[0115] use Figure 1 The manufacturing device of the form shown is used for spinning. The temperature is set in such a way that the ambient temperature of the heating cylinder 2 becomes 265°C. Each filament ejected from the spinneret 1 is cooled and solidified to room temperature by passing through an annular cooling device 3 (RIQ) that blows cooling and rectifying air from the outer periphery toward the center at a cooling start distance LS of 29mm, a wind temperature of 18°C, and a wind speed of 0.53m / sec. Then, each filament is passed through a spinning cylinder 4 with a spinning cylinder length Lb of 600mm, and oil is applied and bundled at a position 1750mm away from the oil supply position Lg from the spinneret surface, and interlaced by a fluid rotating nozzle device 6. The interlacing process is performed by spraying high-pressure air on the transition yarn in the fluid rotating nozzle device 6. The pressure of the high-pressure air is set to 0.35MPa (flow rate 53L / min). Then, the yarn was stretched at a stretching ratio of 1.3 between a take-up roll 7 and a stretching roll 8, and heat-set by the stretching roll 8 set at a temperature of 170°C. The yarn was wound at 4000 m / min to obtain a nylon 6 multifilament of 78 dtex and 24 filaments.
[0116] (Manufacture of fabrics)
[0117] The obtained multifilament was used as weft yarn, and the warp density was 132 yarns / 2.54 cm, and the weft yarns were aligned on the machine, and the weft density was 95 yarns / 2.54 cm, 1 / 3 twill weaving. The obtained fabric was subjected to the following dyeing processes (a) to (d).
[0118] (a) Refining: 2 g / L sodium carbonate, 1 g / L surfactant Glanup US-20 manufactured by Sanyo Chemical Co., Ltd., 100 L liquid volume, 80°C x 20 minutes,
[0119] (b) Intermediate setting: 180℃×1 minute
[0120] (c) Dyeing: Acid dye (LANASYN BLACK M-DL 170%) 5.0% owf, 100°C x 60 minutes
[0121] (d) Final setting: 170℃×1 minute
[0122] Table 1 shows the results of evaluation of the obtained nylon 6 multifilament yarn and woven fabric.
[0123] [Example 2]
[0124] The evaluation results are shown in Table 1, except that the cooling device 3 was changed to an annular cooling device (ROQ) that blows cooling straightening air from the center toward the outer periphery, and a nylon 6 multifilament and a woven fabric were obtained in the same manner as in Example 1.
[0125] [Comparative Example 1]
[0126] Nylon 6 multifilament yarn and woven fabric were obtained in the same manner as in Example 1 except that the cooling device 3 was of a single-flow type that blows cooling rectified air in one direction and the CV% of the profile was changed. The evaluation results are shown in Table 1.
[0127] [Comparative Example 2]
[0128] The evaluation results are shown in Table 1, except that the cooling start distance LS was set to 10 mm and the CV% of the profile was changed, a nylon 6 multifilament and a woven fabric were obtained in the same manner as in Example 1.
[0129] [Example 3]
[0130] The evaluation results are shown in Table 1, except that the cooling start distance LS was set to 20 mm and the hollow ratio was changed, a nylon 6 multifilament and a woven fabric were obtained in the same manner as in Example 1.
[0131] [Example 4]
[0132] The evaluation results are shown in Table 1, except that the cooling start distance LS was 100 mm and the hollow ratio was changed, a nylon 6 multifilament and a woven fabric were obtained in the same manner as in Example 1.
[0133] [Comparative Example 3]
[0134] The evaluation results are shown in Table 1, except that the cooling start distance LS was changed to 110 mm and the CV% of the profile was changed, a nylon 6 multifilament and a woven fabric were obtained in the same manner as in Example 1.
[0135] [Comparative Example 4]
[0136] The evaluation results are shown in Table 1.
[0137] [Example 5]
[0138] The evaluation results are shown in Table 1.
[0139]
[0140] [Comparative Example 5]
[0141] In addition to changing the shape of the spinneret's ejection hole to Figure 4 , and formed into Figure 5 The evaluation results are shown in Table 2.
[0142] [Comparative Example 6]
[0143] In addition to changing the shape of the spinneret's ejection hole to Figure 6 , and formed into Figure 7 The evaluation results are shown in Table 2.
[0144] [Comparative Example 7]
[0145] In addition to changing the shape of the spinneret's ejection hole to Figure 8 , and formed into Fig. 9 The evaluation results are shown in Table 2.
[0146] [Examples 6, 7, Comparative Example 8]
[0147] Nylon 6 multifilaments and woven fabrics were obtained by the same method as in Example 1 except that a spinneret with 24 holes was used, the discharge amount was 7.2 g / min, 45.2 g / min, and 54.3 g / min, and the winding was performed at 4000 m / min, and the single yarn fineness was changed to 0.80 dtex, 5.00 dtex, and 6.00 dtex. The evaluation results are shown in Table 2.
[0148] [Examples 8 and 9]
[0149] The evaluation results are shown in Table 2, except that the polymer type was changed to nylon 66 (relative viscosity in sulfuric acid 2.8, containing no titanium oxide) and nylon 610 (relative viscosity in sulfuric acid 2.7, containing no titanium oxide).
[0150] [Example 10]
[0151] The same method as in Example 1 was used except that the polymer type was changed to PET (OCP relative viscosity 0.64, containing no titanium oxide) to obtain polyethylene terephthalate multifilaments, which were dyed under the following polyester dyeing conditions to obtain a woven fabric. The evaluation results are shown in Table 2.
[0152] Dyeing: Disperse dye (Kayalon Polyester Black UT-RN 5.0% owf, 130°C x 60 minutes)
[0153]
[0154] This application is based on Japanese patent application No. 2022-055757 filed on March 30, 2022, the contents of which are incorporated herein by reference.
[0155] Description of the accompanying drawings
[0156] 1: Spinneret
[0157] 2: Heating tube
[0158] 3: Cooling device
[0159] 4: Spinning drum
[0160] 5: Oil supply device
[0161] 6: Fluid rotating nozzle device
[0162] 7: Traction roller
[0163] 8:Stretching roller
[0164] 9: Coiler
[0165] LS: Cooling start distance
[0166] Lb: Spinning cone length
Claims
1. A multifilament comprising a hollow fiber with a special cross section, wherein a single fiber of the hollow fiber with a special cross section has a triangular hollow portion in a cross section and a protrusion on an extension line of each side of the triangle, Furthermore, the single fiber fineness of the hollow fiber with a special cross section is 5.0 dtex or less, and the degree of special shape CV% is 2.0 or less.
2. The multifilament according to claim 1, wherein the hollow ratio of the hollow fiber with a special cross section is 20% or less and the degree of special shape is 1.1 to 2.0.