Sealing agent for liquid crystal display element
The sealant on large mother glass is solved by using curable resins, organic fillers and sealant adjusted by specific process in the sealant of liquid crystal display elements, combined with epoxy compounds and (meth)acrylic compounds, and sealant on large mother glass is solved by combining with epoxy compounds and (meth)acrylic compounds. The problems of poor follow-up and insufficient adhesion in high temperature and high humidity environments have achieved improvement in the stability and reliability of the substrate.
Patent Information
- Application Number
- CN202380029258.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-08-25
- Filing Date
- 2023-08-24
- Publication Date
- 2024-11-08
AI Technical Summary
In the manufacturing process of liquid crystal display components, especially when high-density coating on large mother glass, sealant cannot follow the warping of the substrate, causing the substrate to peel off, and the adhesiveness is insufficient in high temperature and high humidity environment, making it difficult to meet reliability Sexual requirements.
Using a sealant containing curable resin and organic filler, the shrinkage rate and expansion coefficient of the sealant are adjusted through the photocuring and thermal curing process to ensure that the shrinkage rate after the photocuring process is less than 3.5%, and the maximum expansion in the thermal curing process is The coefficient is 1.5% or more and less than 4%, and the shrinkage rate is maintained at 0.1% or more in the thermal curing process. Combined with epoxy compounds and (meth)acrylic compounds, an inorganic filler and a thermal radical polymerization initiator are used to improve the viscosity. Connectivity.
It effectively suppresses the peeling of the substrate, improves the adhesion and reliability of the sealant in high-density coating and high temperature and high humidity environments, and is suitable for the manufacturing of liquid crystal display components of large mother glass.
Smart Images

Figure BDA0005052828480000201 
Figure BDA0005052828480000211 
Figure BDA0005052828480000221
Abstract
Description
Technical Field
[0001] The present invention relates to a sealing agent for a liquid crystal display element. Background Art
[0002] In recent years, as a method for manufacturing liquid crystal display elements such as liquid crystal display units, from the viewpoint of shortening the production cycle time and optimizing the amount of liquid crystal used, a method called a dropping process, in which a curable resin composition is used as a sealant, as disclosed in Patent Documents 1 and 2, has been used.
[0003] In the dripping process, first, a sealant is applied to one of two substrates with electrodes to form a frame-shaped seal pattern. Next, tiny drops of liquid crystal are dripped into the sealing frame of the substrate while the sealant is not cured, and the other substrate is overlapped under vacuum. The sealant is cured by light irradiation and heating to produce a liquid crystal display element. Currently, this dripping process has become the mainstream method for manufacturing liquid crystal display elements.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent Application Publication No. 2001-133794
[0007] Patent document 2: International Publication No. 02 / 092718 Summary of the invention
[0008] Problems to be solved by the invention
[0009] Generally, a liquid crystal display element is manufactured by forming a plurality of units on a mother glass (Japanese: マザーガラス) at a time and then dividing each unit. In recent years, the size of the mother glass has been continuously developed, and a sealant is densely coated on one mother glass. As a result, the substrate warps, and even when a sealant with excellent adhesion is used, the sealant cannot follow the warping, and the substrate is prone to peeling. In particular, when the sealant is cured in a photocuring process and a heat curing process after the photocuring process, the substrate is sometimes peeled off due to the stress caused by the strain between the substrates after the photocuring process, the transport of the unit to the heating furnace in the heat curing process, the vibration in the heating furnace, etc., causing the substrate to peel off. In addition, a high degree of reliability is also required for the liquid crystal display element in driving under a high temperature and high humidity environment, and the sealant is also required to have excellent adhesion even under a high temperature and high humidity environment, and to have strain and few defects relative to changes in the external environment.
[0010] An object of the present invention is to provide a sealing agent for a liquid crystal display element which has excellent adhesiveness and can suppress separation of a substrate even when applied at a high density to a large mother glass.
[0011] Means for solving problems
[0012] The present invention 1 relates to a sealing agent for a liquid crystal display element, which contains a curable resin and an organic filler and has photocurability and thermosetting properties. The uncured sealing agent for a liquid crystal display element is irradiated with a high-pressure mercury lamp for 30 seconds at a wavelength of 300 to 500 nm and an illumination of 100 mW / cm 2 When a photocuring step is performed by ultraviolet rays, the shrinkage rate of the sealant for liquid crystal display elements after the photocuring step relative to the uncured sealant for liquid crystal display elements at 25°C is 3.5% or less, and after the photocuring step, a heat curing step is performed in which the sealant for liquid crystal display elements is heated to 130°C at a heating rate of 10°C / min and further heated at 130°C for 60 minutes, the maximum expansion coefficient of the sealant for liquid crystal display elements in the heat curing step relative to the uncured sealant for liquid crystal display elements is 1.5% or more and less than 4%, and when the heat curing step is performed after the photocuring step, in the heat curing step, the shrinkage rate of the sealant for liquid crystal display elements during the period from the moment when the sealant for liquid crystal display elements shows the maximum expansion coefficient to the end of the heat curing step is 0.1% or more.
[0013] This invention 2 is related with the sealing agent for liquid crystal display elements of this invention 1 whose said curable resin contains an epoxy compound and a (meth)acrylic-type compound.
[0014] The present invention 3 is related with the sealing agent for liquid crystal display elements of the present invention 2, wherein the total content of the epoxy compound and the organic filler is 1 / 3 or more of the content of the whole curable resin.
[0015] The present invention 4 is directed to the sealing agent for liquid crystal display elements of the present invention 1, 2 or 3, wherein the sealing agent for liquid crystal display elements further contains an inorganic filler, and the content of the organic filler is equal to or greater than the content of the inorganic filler.
[0016] Invention 5 relates to the sealing agent for liquid crystal display elements of invention 1, 2, 3 or 4, wherein the sealing agent for liquid crystal display elements further contains a thermal radical polymerization initiator.
[0017] Invention 6 relates to the sealing agent for liquid crystal display elements of invention 1, 2, 3, 4 or 5, wherein when the thermal curing step is performed after the photocuring step, the glass transition temperature of the cured product after the thermal curing step is 80° C. or higher and 110° C. or lower.
[0018] Hereinafter, the present invention will be described in detail.
[0019] The inventors of the present invention believe that the shrinkage rate of the sealant in the photocuring process, the maximum expansion coefficient of the sealant in the heat curing process after the photocuring process, and the shrinkage rate of the sealant in the heat curing process have a great influence on the followability to the substrate. Therefore, the inventors of the present invention have found that by adjusting these values to a specific range, the adhesion is excellent, and the peeling of the substrate can be suppressed even when the sealant is applied to a large mother glass at a high density, thereby completing the present invention.
[0020] The sealing agent for liquid crystal display elements of the present invention has photocurability and thermosetting property.
[0021] The sealing agent for liquid crystal display elements of the present invention was irradiated with a high pressure mercury lamp for 30 seconds at a wavelength of 300 to 500 nm and an illuminance of 100 mW / cm 2 In a photocuring step using ultraviolet rays, the shrinkage rate of the sealant for liquid crystal display elements after the photocuring step relative to the uncured sealant for liquid crystal display elements at 25°C (hereinafter, also referred to as "the shrinkage rate in the photocuring step") is 3.5% or less, and after the photocuring step, when a heat curing step is performed in which the sealant for liquid crystal display elements is heated to 130°C at a heating rate of 10°C / min and further heated at 130°C for 60 minutes, the maximum expansion coefficient of the sealant for liquid crystal display elements in the heat curing step relative to the uncured sealant for liquid crystal display elements (hereinafter, also referred to as "the maximum expansion coefficient in the heat curing step") is 1.5% or more and less than 4%, and when the heat curing step is performed after the photocuring step, in the heat curing step, the shrinkage rate of the sealant for liquid crystal display elements during the period from the time when the sealant for liquid crystal display elements shows the maximum expansion coefficient to the end of the heat curing step (hereinafter, also referred to as "the shrinkage rate in the heat curing step") is 0.1% or more. By setting the shrinkage rate in the above-mentioned photocuring process to be 3.5% or less, the maximum expansion coefficient in the above-mentioned thermal curing process to be 1.5% or more and less than 4%, and the shrinkage rate in the above-mentioned thermal curing process to be 0.1% or more, the sealant for liquid crystal display elements of the present invention has excellent adhesion and can suppress the peeling of the substrate even when it is coated on a large mother glass at a high density.
[0022] The upper limit of the shrinkage rate in the above-mentioned photocuring step is preferably 2.7%, and the more preferred upper limit is 2.2%. In addition, the shrinkage rate in the above-mentioned photocuring step is preferably as low as possible, but the actual lower limit is 1.0%.
[0023] The preferred lower limit of the maximum expansion coefficient in the thermal curing step is 2.0%, and the more preferred lower limit is 3.0%.
[0024] The preferred lower limit of the shrinkage rate in the thermal curing step is 0.5%. The preferred upper limit of the shrinkage rate in the thermal curing step is 2.5%, and the more preferred upper limit is 1.5%.
[0025] The shrinkage rate in the photocuring step, the maximum expansion coefficient in the heat curing step, and the shrinkage rate in the heat curing step can be measured using a resin curing shrinkage measuring device in accordance with JIS K 6941. As the resin curing shrinkage measuring device, Custron (manufactured by AcroEdge Co., Ltd.) can be used.
[0026] exist Figure 1 A graph showing an example of the relationship between each step of the sealing agent for liquid crystal display elements and the shrinkage rate or expansion coefficient is shown in FIG. Figure 1 It can be seen that from the start of the light irradiation process, the shrinkage progresses, and the volume reduction rate increases by 1.8% after the light curing process, that is, the shrinkage rate in the light curing process becomes 1.8%. In addition, it can be seen that if the heat curing process starts, the expansion progresses, and the volume reduction rate decreases to -3.1%, that is, it can be seen that the maximum expansion coefficient in the heat curing process becomes 3.1%. After that, the shrinkage progresses, and the volume reduction rate increases by 1.2% from the time when the maximum expansion coefficient is displayed to the end of the heat curing process, that is, it can be seen that the shrinkage rate in the heat curing process becomes 1.2%.
[0027] When the sealant for liquid crystal display elements of the present invention performs the above-mentioned heat curing process after the above-mentioned photocuring process, the preferred lower limit of the glass transition temperature of the cured product after the above-mentioned heat curing process is 80°C, and the preferred upper limit is 110°C. By making the glass transition temperature of the above-mentioned cured product above 80°C, the reliability of the liquid crystal display element obtained by using the sealant for liquid crystal display elements of the present invention becomes better. By making the glass transition temperature of the above-mentioned cured product below 110°C, the adhesion of the sealant for liquid crystal display elements of the present invention becomes better. The more preferred lower limit of the glass transition temperature of the above-mentioned cured product is 90°C, and the more preferred upper limit is 100°C.
[0028] The glass transition temperature of the cured product can be obtained as the temperature at which the loss tangent (tan δ) reaches a maximum value when the dynamic viscoelasticity is measured at -80 to 200° C. and 10 Hz using a dynamic viscoelasticity measuring apparatus.
[0029] The curable resin preferably comprises an epoxy compound and a (meth) acrylic compound. By using the epoxy compound and the (meth) acrylic compound in combination with a photoradical polymerization initiator, a thermal radical polymerization initiator, and a thermosetting agent described later, the obtained liquid crystal display element sealant can have excellent photocurability and thermosetting properties.
[0030] In addition, in this specification, the said "(meth)acrylic system" means an acrylic system or a methacrylic system.
[0031] Examples of the epoxy compound include bisphenol A epoxy compounds, bisphenol F epoxy compounds, bisphenol E epoxy compounds, bisphenol S epoxy compounds, 2,2'-diallylbisphenol A epoxy compounds, hydrogenated bisphenol epoxy compounds, propylene oxide-added bisphenol A epoxy compounds, resorcinol epoxy compounds, biphenyl epoxy compounds, sulfide epoxy compounds, diphenyl ether epoxy compounds, dicyclopentadiene epoxy compounds, and the like. Type epoxy compounds, naphthalene type epoxy compounds, phenol novolac type epoxy compounds, o-cresol novolac type epoxy compounds, dicyclopentadiene novolac type epoxy compounds, biphenyl novolac type epoxy compounds, naphthol novolac type epoxy compounds (Japanese: ナフタレンフェノールノボラック type epoxide compounds), glycidylamine type epoxy compounds, alkyl polyol type epoxy compounds, rubber modified epoxy compounds, glycidyl ester compounds, etc.
[0032] As what is marketed among the said bisphenol A type epoxy compounds, jER828EL, jER1004 (all are manufactured by Mitsubishi Chemical Corporation), EPICLON EXA-850CRP (manufactured by DIC Corporation), etc. are mentioned, for example.
[0033] As what is marketed among the said bisphenol F type epoxy compounds, jER806, jER4004 (all are manufactured by Mitsubishi Chemical Corporation), EPICLON EXA-830CRP (manufactured by DIC Corporation), etc. are mentioned, for example.
[0034] As what is marketed among the said bisphenol E type epoxy compounds, EPOMIK R710 (made by Mitsui Chemicals, Inc.) etc. are mentioned, for example.
[0035] As what is marketed among the said bisphenol S type epoxy compounds, EPICLON EXA-1514 (made by DIC Corporation) etc. are mentioned, for example.
[0036] As what is marketed among the said 2,2'- diallylbisphenol A type epoxy compounds, RE-810NM (made by Nippon Kayaku Co., Ltd.) etc. are mentioned, for example.
[0037] As what is marketed among the said hydrogenated bisphenol type epoxy compounds, EPICLON EXA-7015 (made by DIC Corporation) etc. are mentioned, for example.
[0038] As what is marketed among the said propylene oxide addition bisphenol A type epoxy compound, EP-4000S (made by ADEKA Corporation) etc. are mentioned, for example.
[0039] As what is marketed among the said resorcinol type epoxy compounds, EX-201 (made by Nagase ChemteX Co., Ltd.) etc. are mentioned, for example.
[0040] As what is marketed among the said biphenyl type epoxy compounds, jER YX-4000H (made by Mitsubishi Chemical Corporation) etc. are mentioned, for example.
[0041] As what is commercially available among the said thioether type epoxy compounds, YSLV-50TE (made by NIPPON STEEL Chemical & Material Co., Ltd.) etc. are mentioned, for example.
[0042] As what is marketed among the said diphenyl ether type epoxy compounds, YSLV-80DE (made by NIPPONSTEEL Chemical & Material Co., Ltd.) etc. are mentioned, for example.
[0043] As what is marketed among the said dicyclopentadiene type epoxy compounds, EP-4088S (made by ADEKA Corporation) etc. are mentioned, for example.
[0044] Examples of commercially available products of the naphthalene-type epoxy compounds include EPICLON HP-4032 and EPICLONEXA-4700 (both manufactured by DIC Corporation).
[0045] As what is marketed among the said phenol novolac-type epoxy compounds, EPICLON N-770 (made by DIC Corporation) etc. are mentioned, for example.
[0046] As what is marketed among the said o-cresol novolac-type epoxy compounds, EPICLON N-670-EXP-S (made by DIC Corporation) etc. are mentioned, for example.
[0047] As what is marketed among the said dicyclopentadiene novolak-type epoxy compounds, EPICLON HP-7200 (made by DIC Corporation) etc. are mentioned, for example.
[0048] As what is marketed among the said biphenyl novolak-type epoxy compounds, NC-3000P (made by Nippon Kayaku Co., Ltd.) etc. are mentioned, for example.
[0049] As a commercial item among the said naphthol novolac-type epoxy compounds, ESN-165S (made by NIPPONSTEEL Chemical & Material Co., Ltd.) etc. are mentioned, for example.
[0050] Examples of commercially available products of the glycidylamine epoxy compounds include jER630 (manufactured by Mitsubishi Chemical Corporation), EPICLON 430 (manufactured by DIC Corporation), and TETRAD-X (manufactured by Mitsubishi Gas Chemical Corporation).
[0051] Examples of commercially available products of the alkyl polyol epoxy compounds include ZX-1542 (manufactured by Nippondeel Chemical & Material Co., Ltd.), Epiclon 726 (manufactured by DIC Corporation), EPOLIGHT 80MFA (manufactured by Kyoeisha Chemical Co., Ltd.), and Denacol EX-611 (manufactured by Nagase ChemteX Corporation).
[0052] Examples of commercially available products of the rubber-modified epoxy compound include YR-450 and YR-207 (both manufactured by NIPPON STEEL Chemical & Material Co., Ltd.) and Epolead PB (manufactured by Daicel Corporation).
[0053] As a commercial item among the said glycidyl ester compound, Denacol EX-147 (made by Nagase ChemteX) etc. are mentioned, for example.
[0054] As other commercially available products of the above-mentioned epoxy compounds, for example, YDC-1312, YSLV-80XY, YSLV-90CR (all manufactured by NIPPON STEEL Chemical & Material Co., Ltd.), XAC4151 (manufactured by Asahi Kasei Corporation), jER1031, jER1032 (all manufactured by Mitsubishi Chemical Corporation), EXA-7120 (manufactured by DIC Corporation), TEPIC (manufactured by Nissan Chemical Co., Ltd.), etc. can be mentioned.
[0055] As the epoxy compound, a partially (meth)acrylic acid-modified epoxy compound can also be suitably used.
[0056] It should be noted that in this specification, the above-mentioned partially (meth)acrylic acid-modified epoxy compound refers to a compound having one or more epoxy groups and one or more (meth)acryloyl groups in one molecule, which can be obtained by reacting a part of epoxy groups of an epoxy compound having two or more epoxy groups with (meth)acrylic acid. That is, the above-mentioned partially (meth)acrylic acid-modified epoxy compound has a (meth)acryloyl group, but is treated as the above-mentioned epoxy compound.
[0057] In addition, in this specification, the said "(meth)acryloyl group" means an acryloyl group or a methacryloyl group.
[0058] As what is marketed among the said partial (meth)acrylic acid-modified epoxy compounds, UVACURE1561, KRM8287 (all are manufactured by DAICEL-ALLNEX CORPORATION) etc. are mentioned, for example.
[0059] As the above-mentioned (meth) acrylic acid compounds, for example, (meth) acrylic acid ester compounds, epoxy (meth) acrylates, urethane (meth) acrylates, etc. can be cited. Among them, epoxy (meth) acrylates are preferred. In addition, from the viewpoint of reactivity, the above-mentioned (meth) acrylic acid compounds preferably have two or more (meth) acryloyl groups in one molecule.
[0060] In addition, in this specification, the said "(meth)acrylate" means an acrylate or a methacrylate, and the said "epoxy (meth)acrylate" means the compound obtained by making all epoxy groups in an epoxy compound react with (meth)acrylic acid.
[0061] Examples of the monofunctional compound among the (meth)acrylate compounds include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-octyl (meth)acrylate, isooctyl (meth)acrylate, isononyl (meth)acrylate, isodecyl (meth)acrylate, lauryl (meth)acrylate, isomyristyl (meth)acrylate, stearyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, cyclohexyl (meth)acrylate, isobornyl (meth)acrylate, dicyclopentenyl (meth)acrylate, benzyl (meth)acrylate, 2-methoxyethyl (meth)acrylate, and 2-ethoxyethyl (meth)acrylate. , 2-butoxyethyl (meth)acrylate, 2-phenoxyethyl (meth)acrylate, methoxyethylene glycol (meth)acrylate, methoxypolyethylene glycol (meth)acrylate, phenoxydiethylene glycol (meth)acrylate, phenoxypolyethylene glycol (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, ethyl carbitol (meth)acrylate, 2,2,2-trifluoroethyl (meth)acrylate, 2,2,3,3-tetrafluoropropyl (meth)acrylate, 1H,1H,5H-octafluoropentyl (meth)acrylate, imide (meth)acrylate, dimethylaminoethyl (meth)acrylate, diethylaminoethyl (meth)acrylate, 2-(meth)acryloyloxyethyl succinate, 2-(meth)acryloyloxyethyl hexahydrophthalate, 2-(meth)acryloyloxyethyl 2-hydroxypropyl phthalate, 2-(meth)acryloyloxyethyl phosphate, glycidyl (meth)acrylate, and the like.
[0062] Examples of the bifunctional (meth)acrylate compounds include 1,3-butanediol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, 1,10-decanediol di(meth)acrylate, ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, 2-n-butyl-2-ethyl-1,3-propanediol di(meth)acrylate, dipropylene glycol di(meth)acrylate, and tripropylene glycol di(meth)acrylate. Ester, polypropylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, ethylene oxide added bisphenol A di(meth)acrylate, propylene oxide added bisphenol A di(meth)acrylate, ethylene oxide added bisphenol F di(meth)acrylate, dimethylol dicyclopentadienyl di(meth)acrylate, ethylene oxide modified isocyanuric acid di(meth)acrylate, 2-hydroxy-3-(meth)acryloxypropyl (meth)acrylate, carbonate diol di(meth)acrylate, polyether diol di(meth)acrylate, polyester diol di(meth)acrylate, polycaprolactone diol di(meth)acrylate, polybutadiene diol di(meth)acrylate, etc.
[0063] In addition, examples of the trifunctional or higher-functional compounds among the above-mentioned (meth)acrylate compounds include trimethylolpropane tri(meth)acrylate, ethylene oxide-added trimethylolpropane tri(meth)acrylate, propylene oxide-added trimethylolpropane tri(meth)acrylate, caprolactone-modified trimethylolpropane tri(meth)acrylate, ethylene oxide-added isocyanuric acid tri(meth)acrylate, glycerol tri(meth)acrylate, propylene oxide-added glycerol tri(meth)acrylate, pentaerythritol tri(meth)acrylate, tri(meth)acryloyloxyethyl phosphate, ditrimethylolpropane tetra(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, and dipentaerythritol hexa(meth)acrylate.
[0064] As said epoxy (meth)acrylate, the epoxy (meth)acrylate etc. which are obtained by making an epoxy compound and (meth)acrylic acid react in the presence of a basic catalyst by a conventional method are mentioned, for example.
[0065] As the epoxy compound used as a raw material for synthesizing the epoxy (meth)acrylate, the same epoxy compound as the epoxy compound described above as the curable resin contained in the sealing compound for liquid crystal display elements of the present invention can be used.
[0066] Examples of commercially available products of the epoxy (meth)acrylate include epoxy (meth)acrylate manufactured by Daicel-Allnex, epoxy (meth)acrylate manufactured by Shin-Nakamura Chemical Industry Co., Ltd., epoxy (meth)acrylate manufactured by Kyoeisha Chemical Co., Ltd., and epoxy (meth)acrylate manufactured by Nagase ChemteX.
[0067] Examples of the epoxy (meth)acrylate manufactured by DAICEL-ALLNEX include EBECRYL 860, EBECRYL 3200, EBECRYL 3201, EBECRYL 3412, EBECRYL 3600, EBECRYL 3700, EBECRYL 3701, EBECRYL 3702, EBECRYL 3703, EBECRYL 3708, EBECRYL 3800, EBECRYL 6040, EBECRYL KRM7985, and EBECRYL RDX63182.
[0068] As said epoxy (meth)acrylate manufactured by Shin-Nakamura Chemical Industry Co., Ltd., EA-1010, EA-1020, EA-5323, EA-5520, EA-CHD, EMA-1020 etc. are mentioned, for example.
[0069] Examples of the epoxy (meth)acrylate manufactured by Kyoeisha Chemical Co., Ltd. include Epoxy Ester M-600A, Epoxy Ester 40EM, Epoxy Ester 70PA, Epoxy Ester 200PA, Epoxy Ester 80MFA, Epoxy Ester 3002M, Epoxy Ester 3002A, Epoxy Ester 1600A, Epoxy Ester 3000M, Epoxy Ester 3000A, Epoxy Ester 200EA, and Epoxy Ester 400EA.
[0070] As said Nagase ChemteX epoxy (meth)acrylate, Denacol Acrylate DA-141, Denacol Acrylate DA-314, Denacol Acrylate DA-911 etc. are mentioned, for example.
[0071] The urethane (meth)acrylate can be obtained, for example, by reacting a (meth)acrylic acid derivative having a hydroxyl group with an isocyanate compound in the presence of a catalytic amount of a tin-based compound.
[0072] Examples of the isocyanate compound used as a raw material for the urethane (meth)acrylate include isophorone diisocyanate, 2,4-toluene diisocyanate, 2,6-toluene diisocyanate, hexamethylene diisocyanate, trimethylhexamethylene diisocyanate, diphenylmethane-4,4′-diisocyanate (MDI), hydrogenated MDI, polymerized MDI, 1,5-naphthalene diisocyanate, Norbornane diisocyanate, dimethylbiphenyl diisocyanate, xylylene diisocyanate (XDI), hydrogenated XDI, lysine diisocyanate, triphenylmethane triisocyanate, tris(isocyanatephenyl)thiophosphorothioate (Japanese: Tris(イソシアネートフェニル)チオフォスフェート), tetramethylxylylene diisocyanate, 1,6,11-undecane triisocyanate, etc.
[0073] Moreover, as the isocyanate compound used as the raw material of the above-mentioned urethane (meth)acrylate, a chain-extended isocyanate compound obtained by the reaction of a polyol with an excess of an isocyanate compound may be used.
[0074] Examples of the polyol include ethylene glycol, propylene glycol, glycerin, sorbitol, trimethylolpropane, carbonate diol, polyether diol, polyester diol, and polycaprolactone diol.
[0075] Examples of the (meth)acrylic acid derivative having a hydroxyl group include hydroxyalkyl mono(meth)acrylates, mono(meth)acrylates of diols, mono(meth)acrylates or di(meth)acrylates of triols, and epoxy(meth)acrylates.
[0076] As said hydroxyalkyl mono(meth)acrylate, 2-hydroxyethyl(meth)acrylate, 2-hydroxypropyl(meth)acrylate, 2-hydroxybutyl(meth)acrylate, 4-hydroxybutyl(meth)acrylate etc. are mentioned, for example.
[0077] Examples of the diol include ethylene glycol, propylene glycol, 1,3-propanediol, 1,3-butanediol, 1,4-butanediol, and polyethylene glycol.
[0078] Examples of the triol include trimethylolethane, trimethylolpropane, and glycerin.
[0079] As said epoxy (meth)acrylate, bisphenol A type epoxy acrylate etc. are mentioned, for example.
[0080] Examples of commercially available products of the urethane (meth)acrylates include urethane (meth)acrylates manufactured by Toagosei Co., Ltd., urethane (meth)acrylates manufactured by Daicel-Allnex Co., Ltd., urethane (meth)acrylates manufactured by Negami Industries Co., Ltd., urethane (meth)acrylates manufactured by Shin-Nakamura Chemical Co., Ltd., and urethane (meth)acrylates manufactured by Kyoeisha Chemical Co., Ltd.
[0081] As the urethane (meth)acrylate manufactured by Toagosei Co., Ltd., for example, M-1100, M-1200, M-1210, and M-1600 can be mentioned.
[0082] Examples of the urethane (meth)acrylate manufactured by DAICEL-ALLNEX include EBECRYL 210, EBECRYL 220, EBECRYL 230, EBECRYL 270, EBECRYL 1290, EBECRYL 2220, EBECRYL 4827, EBECRYL 4842, EBECRYL 4858, EBECRYL 5129, EBECRYL 6700, EBECRYL 8402, EBECRYL 8803, EBECRYL 8804, EBECRYL 8807, and EBECRYL 9260.
[0083] Examples of the urethane (meth)acrylate manufactured by Negami Industries include Artresin UN-330, Artresin SH-500B, Artresin UN-1200TPK, Artresin UN-1255, Artresin UN-3320HB, Artresin UN-7100, Artresin UN-9000A, and Artresin UN-9000H.
[0084] Examples of the urethane (meth) acrylate manufactured by Shin-Nakamura Chemical Industry Co., Ltd. include U-2HA, U-2PHA, U-3HA, U-4HA, U-6H, U-6HA, U-6LPA, U-10H, U-15HA, U-108, U-108A, U-122A, U-122P, U-324A, U-340A, U-340P, U-1084A, U-2061BA, UA-340P, UA-4000, UA-4100, UA-4200, UA-4400, UA-5201P, UA-7100, UA-7200, and UA-W2A.
[0085] Examples of the urethane (meth)acrylate manufactured by Kyoeisha Chemical Co., Ltd. include AH-600, AI-600, AT-600, UA-101I, UA-101T, UA-306H, UA-306I, and UA-306T.
[0086] The ratio of the (meth)acryloyl group in the total of the epoxy group and the (meth)acryloyl group in the curable resin is preferably 30 mol% or more and 95 mol% or less. By making the ratio of the (meth)acryloyl group within this range, the adhesiveness and low liquid crystal contamination of the obtained liquid crystal display element sealant become more excellent.
[0087] From the viewpoint of further suppressing liquid crystal contamination, the curable resin preferably has -OH groups, -NH- groups, -NH 2 Hydrogen bonding units such as the base.
[0088] The preferred lower limit of the content of the above-mentioned curable resin as a whole in 100 parts by mass of the sealant for liquid crystal display elements of the present invention is 50 parts by mass, and the preferred upper limit is 90 parts by mass. By making the content of the above-mentioned curable resin as a whole within this range, the curability and adhesion of the obtained sealant for liquid crystal display elements become more excellent. The more preferred lower limit of the content of the above-mentioned curable resin as a whole is 60 parts by mass, and the more preferred upper limit is 80 parts by mass.
[0089] The sealing agent for liquid crystal display elements of the present invention contains an organic filler.
[0090] Examples of the organic filler include polyester microparticles, polyurethane microparticles, vinyl polymer microparticles, (meth)acrylic polymer microparticles, etc. The organic filler may have a core-shell structure.
[0091] The preferred lower limit of the average particle size of the organic filler is 0.1 μm, and the preferred upper limit is 0.8 μm. By setting the average particle size of the organic filler to this range, it is easier to adjust the shrinkage rate in the photocuring process, the maximum expansion coefficient in the thermal curing process, and the shrinkage rate in the thermal curing process to the above range while maintaining the coating properties. The more preferred upper limit of the average particle size of the organic filler is 0.5 μm.
[0092] The average particle size of the organic filler can be measured by dispersing the organic filler in a solvent (water, organic solvent, etc.) using a particle size distribution measuring device, such as NICOMP 380ZLS (manufactured by PARTICLE SIZING SYSTEMS).
[0093] The preferred lower limit of the content of the organic filler in 100 parts by mass of the sealant for liquid crystal display elements of the present invention is 1 part by mass, and the preferred upper limit is 40 parts by mass. By making the content of the organic filler within this range, it is easier to adjust the shrinkage rate in the photocuring process, the maximum expansion coefficient in the thermal curing process, and the shrinkage rate in the thermal curing process to the above range while maintaining the coating properties. The more preferred lower limit of the content of the organic filler is 10 parts by mass, and the more preferred upper limit is 30 parts by mass.
[0094] In addition, the sealing agent for liquid crystal display elements of the present invention is preferably that the total content of the epoxy compound and the organic filler is 1 / 3 or more of the content of the curable resin as a whole. By making the total content of the epoxy compound and the organic filler be 1 / 3 or more of the content of the curable resin as a whole, it is easier to adjust the shrinkage rate in the photocuring process, the maximum expansion coefficient in the thermal curing process, and the shrinkage rate in the thermal curing process to the above range. The total content of the epoxy compound and the organic filler is more preferably 1 / 2 or more of the content of the curable resin as a whole.
[0095] In addition, when the sealing agent for liquid crystal display elements of the present invention contains an inorganic filler described later, the content of the organic filler is preferably a content greater than the content of the inorganic filler. By making the content of the organic filler greater than the content of the inorganic filler, it is easier to adjust the shrinkage rate in the photocuring process, the maximum expansion coefficient in the thermal curing process, and the shrinkage rate in the thermal curing process to the above range. The content of the organic filler is more preferably 1.5 times or more of the content of the inorganic filler.
[0096] The sealing agent for liquid crystal display elements of the present invention preferably contains an inorganic filler in addition to the above-mentioned organic filler for the purpose of increasing viscosity, improving adhesiveness due to stress dispersion effect, improving linear expansion coefficient, and the like.
[0097] Examples of the inorganic filler include silica, talc, glass beads, asbestos, gypsum, diatomaceous earth, smectite, bentonite, montmorillonite, sericite, activated clay, aluminum oxide, zinc oxide, iron oxide, magnesium oxide, tin oxide, titanium oxide, calcium carbonate, magnesium carbonate, magnesium hydroxide, aluminum hydroxide, aluminum nitride, silicon nitride, barium sulfate, and calcium silicate.
[0098] The preferred lower limit of the content of the above-mentioned inorganic filler in 100 parts by mass of the sealant for liquid crystal display elements of the present invention is 1 part by mass, and the preferred upper limit is 30 parts by mass. By making the content of the above-mentioned inorganic filler within this range, while maintaining the coating properties, the effects of improving the adhesiveness, etc. become more excellent. The more preferred lower limit of the content of the above-mentioned inorganic filler is 5 parts by mass, and the more preferred upper limit is 15 parts by mass.
[0099] It is preferable that the sealing agent for liquid crystal display elements of this invention contains a photoradical polymerization initiator.
[0100] Examples of the photoradical polymerization initiator include benzophenone compounds, acetophenone compounds, acylphosphine oxide compounds, titanocene compounds, oxime ester compounds, benzoin ether compounds, and thioxanthone compounds.
[0101] Specific examples of the photoradical polymerization initiator include 1-hydroxycyclohexyl phenyl ketone, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-1-butanone, 2-(dimethylamino)-2-((4-methylphenyl)methyl)-1-(4-(4-morpholino)phenyl)-1-butanone, 2,2-dimethoxy-1,2-diphenylethane-1-one, bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide, 2-methyl-1-(4- 1-(4-(2-hydroxyethoxy)phenyl)-2-hydroxy-2-methyl-1-propane-1-one, 1-(4-(phenylthio)phenyl)-1,2-octanedione 2-(O-benzoyl oxime), 2-(acetoxyimino)-1-(4-(4-(2-hydroxyethoxy)phenylthio)phenyl)propane-1-one, 2,4,6-trimethylbenzoyldiphenylphosphine oxide, 2,4-dimethylthioxanthen-9-one, and the like.
[0102] Relative to 100 parts by mass of the curable resin, the preferred lower limit of the content of the above-mentioned free radical polymerization initiator is 0.01 parts by mass, and the preferred upper limit is 10 parts by mass. By making the content of the above-mentioned free radical polymerization initiator within this range, the storage stability and photocurability of the obtained sealant for liquid crystal display elements become more excellent. The more preferred lower limit of the content of the above-mentioned free radical polymerization initiator is 0.1 parts by mass, and the more preferred upper limit is 5 parts by mass.
[0103] The sealing agent for liquid crystal display elements of the present invention preferably contains a thermal radical polymerization initiator. By using the thermal radical polymerization initiator, it is easier to adjust the maximum expansion coefficient in the thermal curing step and the shrinkage rate in the thermal curing step to the above ranges.
[0104] Examples of the thermal radical polymerization initiator include thermal radical polymerization initiators including azo compounds, organic peroxides, etc. Among them, azo compounds are preferred.
[0105] Examples of the azo compound include an azo compound having a structure in which a plurality of units of polyalkylene oxide, polydimethylsiloxane, or the like are bonded via an azo group.
[0106] The azo compound having a structure in which a plurality of units such as polyalkylene oxide are bonded via an azo group is preferably an azo compound having a polyethylene oxide structure.
[0107] Specific examples of the azo compound include 4,4′-azobis(4-cyanovaleric acid), a polycondensate of 4,4′-azobis(4-cyanovaleric acid) and polyalkylene glycol, and a polycondensate of 4,4′-azobis(4-cyanovaleric acid) and polydimethylsiloxane having a terminal amino group.
[0108] Examples of commercially available products of the azo compounds include VPE-0201, VPE-0401, VPE-0601, VPS-0501, VPS-1001, V-65, and V-501 (all manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.).
[0109] Examples of the organic peroxide include ketone peroxide, peroxyketal, hydroperoxide, dialkyl peroxide, peroxyester, diacyl peroxide, and peroxydicarbonate.
[0110] The preferred lower limit of the content of the thermal free radical polymerization initiator is 0.01 parts by mass, and the preferred upper limit is 10 parts by mass relative to 100 parts by mass of the curable resin. By making the content of the thermal free radical polymerization initiator within this range, it is easier to adjust the maximum expansion coefficient in the thermal curing process and the shrinkage rate in the thermal curing process to the above range. The more preferred lower limit of the content of the thermal free radical polymerization initiator is 0.1 parts by mass, and the more preferred upper limit is 5 parts by mass.
[0111] It is preferable that the sealing agent for liquid crystal display elements of this invention contains a thermosetting agent.
[0112] Examples of the thermosetting agent include organic acid hydrazides, imidazole derivatives, amine compounds, polyphenol compounds, and acid anhydrides. Among them, organic acid hydrazides are preferably used.
[0113] Examples of the organic acid hydrazide include sebacic acid dihydrazide, isophthalic acid dihydrazide, adipic acid dihydrazide, and malonic acid dihydrazide.
[0114] Examples of commercially available products of the organic acid hydrazide include organic acid hydrazide manufactured by Otsuka Chemical Co., Ltd. and organic acid hydrazide manufactured by Ajinomoto Fine-Techno Co., Ltd.
[0115] Examples of the organic acid hydrazide manufactured by Otsuka Chemical Co., Ltd. include SDH and ADH.
[0116] Examples of the organic acid hydrazide manufactured by Ajinomoto Fine-Techno include AJICURE VDH, AJICURE VDH-J, AJICURE UDH, and AJICURE UDH-J.
[0117] Relative to 100 parts by mass of the curable resin, the preferred lower limit of the content of the thermosetting agent is 1 part by mass, and the preferred upper limit is 50 parts by mass. By making the content of the thermosetting agent within this range, the obtained sealant for liquid crystal display elements becomes more excellent in thermosetting property while maintaining storage stability and coating properties. The more preferred upper limit of the content of the thermosetting agent is 30 parts by mass.
[0118] The sealing agent for liquid crystal display elements of the present invention preferably contains a silane coupling agent. The silane coupling agent mainly functions as an adhesion aid for favorably bonding the sealing agent for liquid crystal display elements to a substrate or the like.
[0119] As the silane coupling agent, for example, 3-aminopropyltrimethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-glycidoxypropyltrimethoxysilane, etc. are preferably used.
[0120] The preferred lower limit of the content of the above-mentioned silane coupling agent in 100 parts by mass of the sealant for liquid crystal display elements of the present invention is 0.1 parts by mass, and the preferred upper limit is 10 parts by mass. By making the content of the above-mentioned silane coupling agent within this range, the sealant for liquid crystal display elements obtained can improve the effect of adhesion while suppressing the occurrence of liquid crystal pollution. The more preferred lower limit of the content of the above-mentioned silane coupling agent is 0.3 parts by mass, and the more preferred upper limit is 5 parts by mass.
[0121] The sealing agent for liquid crystal display elements of the present invention may further contain additives such as a stress relaxation agent, a reactive diluent, a curing accelerator, a defoaming agent, a leveling agent, and a polymerization inhibitor as needed.
[0122] As a method for manufacturing the sealing agent for liquid crystal display elements of this invention, the method of mixing other components, such as a curable resin, an organic filler, and a photoradical polymerization initiator, etc. are mentioned, for example.
[0123] Examples of the mixer include a homodisperser, a homomixer, a universal mixer, a planetary mixer, a kneader, and a three-roll mill.
[0124] Moreover, by mix|blending conductive fine particles in the sealing agent for liquid crystal display elements of this invention, a vertical conduction material can be manufactured.
[0125] As the conductive particles, metal balls, conductive particles having a conductive metal layer formed on the surface of resin particles, etc. can be used. Among them, conductive particles having a conductive metal layer formed on the surface of resin particles are suitable because they can be electrically connected without damaging a transparent substrate, etc., due to the excellent elasticity of the resin particles.
[0126] As a method for producing a liquid crystal display element using the sealing compound for liquid crystal display elements of the present invention, a liquid crystal dropping process is preferably used, and specifically, for example, a method having the following steps can be mentioned.
[0127] First, a process of forming a frame-shaped seal pattern by applying the sealant for liquid crystal display elements of the present invention on one of two transparent substrates having electrodes such as ITO thin films by screen printing, dispenser coating, etc. is performed. Next, a process of applying tiny droplets of liquid crystal to the entire surface of the frame of the seal pattern and overlapping another transparent substrate under vacuum is performed. Then, a process of pre-curing the sealant by irradiating the seal pattern portion with light such as ultraviolet rays (photocuring process), and a process of heating the pre-cured sealant to formally cure it (thermocuring process) is performed, thereby a liquid crystal display element can be obtained.
[0128] The sealant for liquid crystal display elements of the present invention can suppress substrate peeling even when applied at high density to a large mother glass, and therefore can be suitably used particularly when applied to a mother glass of so-called 8th generation or later with a size of 2200 mm×2400 mm, 2160 mm×2460 mm or more.
[0129] Effects of the Invention
[0130] According to the present invention, it is possible to provide a sealing agent for a liquid crystal display element which has excellent adhesiveness and can suppress separation of a substrate even when applied at a high density to a large mother glass. BRIEF DESCRIPTION OF THE DRAWINGS
[0131] Figure 1 This is a graph showing an example of the relationship between each step of the sealing agent for liquid crystal display elements and the shrinkage rate or expansion coefficient. DETAILED DESCRIPTION
[0132] Hereinafter, the present invention will be described in more detail with reference to Examples, but the present invention is not limited to these Examples.
[0133] (Examples 1 to 25, Comparative Examples 1 to 5)
[0134] The materials were stirred with a planetary stirring device according to the mixing ratios listed in Tables 1 to 3 and then uniformly mixed with a ceramic three-roll mill to obtain sealing agents for liquid crystal display elements of Examples 1 to 25 and Comparative Examples 1 to 5. Awatori Rentaro (manufactured by THINKY Corporation) was used as the planetary stirring device.
[0135] (Shrinkage rate in the photocuring process, maximum expansion coefficient in the thermal curing process, and shrinkage rate in the thermal curing process)
[0136] The obtained sealant for liquid crystal display elements was measured for shrinkage in the photocuring step, maximum expansion coefficient in the thermal curing step, and shrinkage in the thermal curing step using a resin curing shrinkage measuring device in accordance with JIS K 6941. Custron (manufactured by AcroEdg) was used as the resin curing shrinkage measuring device. The results are shown in Tables 1 to 3.
[0137] (Glass transition temperature)
[0138] Each of the obtained sealing agents for liquid crystal display elements was irradiated with an illuminance of 100 mW / cm2 for 30 seconds using a high pressure mercury lamp and a cut filter that cuts off light of 340 nm or less. 2 The cured product was subjected to a photocuring step of ultraviolet rays, and then a heat curing step of heating at 130°C for 60 minutes was performed to obtain a cured product. For the cured product after the heat curing step, the dynamic viscoelasticity was measured using a dynamic viscoelasticity measuring device under the conditions of a test piece width of 5 mm, a thickness of 0.35 mm, a clamping width of 25 mm, a heating rate of 10°C / min, a temperature range of -80°C to 200°C, and a frequency of 10 Hz, and the temperature of the maximum value of the loss tangent (tanδ) was determined as the glass transition temperature. As the above-mentioned dynamic viscoelasticity measuring device, DVA-200 (manufactured by IT Measurement and Control Co., Ltd.) was used. The results are shown in Tables 1 to 3.
[0139] <Evaluation>
[0140] The following evaluations were performed on the sealing agents for liquid crystal display elements obtained in the examples and comparative examples. The results are shown in Tables 1 to 3.
[0141] (Adhesion (Compression shear bond strength))
[0142] The obtained sealant for liquid crystal display element was applied on one of the two ITO substrates with a length of 45 mm, a width of 25 mm, and a thickness of 0.7 mm, so that the diameter during bonding was 3 mm. The other ITO substrate was overlapped with the ITO substrate with the sealant applied by means of the sealant in a manner that was only staggered by 10 mm in the length direction. Then, a high-pressure mercury lamp was used to irradiate the substrate for 30 seconds at an illumination of 100 mW / cm through a cutoff filter that can cut off less than 340 nm. 2 After irradiating with ultraviolet rays, the sealant was cured by heating at 130° C. for 60 minutes to obtain a test piece. The obtained test piece was measured for compressive shear adhesive strength at 25° C. by a method in accordance with JIS K 6852 using Autograph AGX (manufactured by Shimadzu Corporation).
[0143] [Table 1]
[0144]
[0145]
[0146] [Table 3]
[0147]
[0148] Industrial Applicability
[0149] According to the present invention, it is possible to provide a sealing agent for a liquid crystal display element which has excellent adhesiveness and can suppress separation of a substrate even when applied at a high density to a large mother glass.
Claims
1. A sealant for a liquid crystal display element, characterized in that: It contains curable resin and organic filler, and has both photocuring and thermosetting properties. The uncured liquid crystal display element sealant was irradiated with a high pressure mercury lamp for 30 seconds at a wavelength of 300 nm to 500 nm and an illumination of 100 mW / cm 2 In a light curing step using ultraviolet rays, the shrinkage rate of the liquid crystal display element sealant after the light curing step relative to the uncured liquid crystal display element sealant at 25° C. is 3.5% or less, After the photocuring step, a heat curing step is performed in which the temperature of the liquid crystal display element sealant is raised to 130° C. at a temperature rising rate of 10° C. / min and further heated at 130° C. for 60 minutes, wherein the maximum expansion coefficient of the liquid crystal display element sealant in the heat curing step relative to the uncured liquid crystal display element sealant is 1.5% or more and less than 4%, and When the thermal curing step is performed after the photocuring step, in the thermal curing step, the shrinkage rate of the liquid crystal display element sealant from the time when the liquid crystal display element sealant exhibits the maximum expansion coefficient to the end of the thermal curing step is 0.1% or more.
2. The sealing agent for liquid crystal display elements according to claim 1, wherein The curable resin includes an epoxy compound and a (meth)acrylic compound.
3. The sealing agent for a liquid crystal display element according to claim 2, wherein The total content of the epoxy compound and the organic filler is 1 / 3 or more of the total content of the curable resin.
4. The sealing agent for liquid crystal display elements according to claim 1, 2 or 3, wherein The sealing agent for liquid crystal display elements further contains an inorganic filler. The content of the organic filler is equal to or greater than the content of the inorganic filler.
5. The sealing agent for liquid crystal display elements according to claim 1, 2, 3 or 4, wherein The sealing agent for liquid crystal display elements contains a thermal radical polymerization initiator.
6. The sealing agent for liquid crystal display elements according to claim 1, 2, 3, 4 or 5, wherein When the thermal curing step is performed after the photocuring step, the glass transition temperature of the cured product after the thermal curing step is 80° C. or higher and 110° C. or lower.