Optical semiconductor device and method for designing antireflection film for optical semiconductor device

By using a multi-layer covering film design with a characteristic matrix not a unit matrix in an optical semiconductor device, the problem of the anti-reflection film failing to reach the minimum reflectance in the prior art, and the minimum under the central wavelength of the laser is achieved Reflectivity and adaptive effects to change in refractive index.

CN118923010APending Publication Date: 2024-11-08MITSUBISHI ELECTRIC CORP
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202280093860.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2022-04-14
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

In the conventional optical semiconductor device, the reflectivity of the anti-reflection film fails to reach the minimum at the center wavelength of the laser, and the multi-layer film thickness determination method has not been disclosed, so it cannot adapt to the change of refractive index.

Method used

The ideal single-layer covering film is replaced by a multi-layer covering film with a characteristic matrix not a unit matrix. By setting the refractive index and film thickness of each covering film, the characteristic matrix is ​​equal to the matrix of the ideal single-layer covering film. , thereby achieving zero or minimum reflectivity at the desired wavelength.

Benefits of technology

The anti-reflective film design with the smallest reflectivity at the central wavelength of the laser is realized, adapting to changes in refractive index and film thickness, and improving the reliability and performance of optical semiconductor devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118923010A_ABST
    Figure CN118923010A_ABST
Patent Text Reader

Abstract

An optical semiconductor device (100) of the present disclosure has an effective refractive index nc, a wavelength lambda, and an antireflection film (10) on an end surface, the antireflection film (10) being configured from i cover films from a first cover film having a refractive index n1 and a film thickness d1 to an i-th cover film (i > = 4) having a refractive index ni and a film thickness di, the film thickness of a k-th cover film (1 < = k < = i) being set to be other than lambda / 2 / nk, the refractive index of the one or more cover films is larger than the square root of the effective refractive index nc, namely, the refractive index nf, the refractive index of the one or more cover films is smaller than the refractive index nf, the characteristic matrix of the multi-layer cover films is equal to the characteristic matrix of the single-layer cover film with the refractive index nf and the film thickness df being lambda / 4 / nf, the film thickness of the i-3 cover films in the i cover films is preset, and the film thickness of the i-3 cover films in the i cover films is smaller than that of the i-3 cover films in the i cover films. The film thicknesses of the remaining three layers of cover films are determined by solutions of three simultaneous equations derived from a characteristic matrix of the multi-layer cover film.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to an optical semiconductor device and a method for designing an antireflection film for an optical semiconductor device. Background Art

[0002] For example, as described in Patent Document 1, an existing quantum cascade laser device comprises: a semiconductor substrate, a semiconductor stack formed on the semiconductor substrate, a first electrode formed on the upper portion of the semiconductor stack, and a second electrode formed on the lower portion of the semiconductor substrate, and an anti-reflection (AR) film is formed on one of a pair of end faces of the semiconductor stack including an active layer.

[0003] Patent document 1 discloses that, in the case where the refractive index of a semiconductor stack is 3.2, as an anti-reflection film that realizes a reflectivity of less than 0.1% at the central wavelength of 10 μm of laser light, the plurality of refractive index films constituting the anti-reflection film can be set to a multilayer film consisting of four refractive index films as described below: the first layer is a CeO2 (Cerium Oxide) film having a refractive index of 1.7 and a film thickness of 50 nm, the second layer is a ZnS (Zinc Sulfide) film having a refractive index of 2.2 and a film thickness of 50 nm, the third layer is a CeF3 (Cerium Fluoride) film having a refractive index of 1.45 and a film thickness of 600 nm, and the fourth layer is a ZnS film having a refractive index of 2.2 and a film thickness of 450 nm.

[0004] In addition, Patent Document 2 discloses that c The end face of the semiconductor laser device with an oscillation wavelength of λ is provided with a refractive index n f With the effective refractive index n c The square root of is equal and the film thickness is λ / (4n f ) in the case of an anti-reflection film, an ideal single-layer film whose reflectivity becomes zero at an oscillation wavelength λ can be replaced by a three-layer film having a refractive index of n1 and a film thickness of d1, a refractive index of n2 and a film thickness of d2, and a refractive index of n3 and a film thickness of d3.

[0005] At this time, any of the refractive indices n1, n2, and n3 is greater than the refractive index n f , and any of the refractive indices n1, n2, and n3 is less than the refractive index n f Furthermore, it is disclosed that a film having a refractive index of n is inserted at an arbitrary position between the films. a And the film thickness is λ / (2n a) film, but this only means that the characteristic matrix of the film becomes a unit matrix, and there is no record or suggestion of replacing the ideal single-layer film with a film structure of more than four layers by inserting films other than the unit matrix.

[0006] Patent Document 1: Japanese Patent Application Publication No. 2021-163922

[0007] Patent Document 2: Japanese Patent Application Laid-Open No. 05-243689

[0008] Patent Document 3: International Publication No. 2019 / 053854

[0009] Non-patent document 1: M. Born and E. Wolf, "Principles of Optics," pp. 55-60, 6th Edition, PERGAMON PRESS

[0010] The quantum cascade laser device described in Patent Document 1 is an anti-reflection film that realizes a reflectivity of less than 0.1% at the central wavelength of 10 μm of the laser when the refractive index of the semiconductor stack is 3.2. The anti-reflection film is composed of a multilayer film of four layers, starting from the end face side of the semiconductor stack: the first layer is a CeO2 film with a refractive index of 1.7 and a film thickness of 50 nm, the second layer is a ZnS film with a refractive index of 2.2 and a film thickness of 50 nm, the third layer is a CeF3 film with a refractive index of 1.45 and a film thickness of 600 nm, and the fourth layer is a ZnS film with a refractive index of 2.2 and a film thickness of 450 nm.

[0011] However, Patent Document 1 does not disclose how to determine the thickness of each film of the multilayer film, so when the refractive index of the semiconductor stack or the refractive index of each film changes, it is impossible to form an appropriate anti-reflection film. In other words, Patent Document 1 does not disclose any design method of an anti-reflection film for an optical semiconductor device. In addition, as described later, although the reflectivity at the center wavelength of the laser is less than 0.1%, it is not an anti-reflection film whose reflectivity becomes zero or minimum at this wavelength.

[0012] In addition, the antireflection film of the semiconductor laser device described in Patent Document 2 has an effective refractive index of n c The end face of the semiconductor laser device with an oscillation wavelength of λ has a refractive index n f is the effective refractive index n c The square root of the film thickness is λ / (4n f ) is replaced by a three-layer film, or a characteristic matrix is ​​inserted at any position between the replaced films to form a unit matrix with a refractive index of n a And the film thickness is λ / (2n a) is not an anti-reflection film composed of a multilayer covering film of four or more layers in which the characteristic matrix of each covering film does not become a unit matrix. Summary of the invention

[0013] The present disclosure is completed in order to eliminate the above-mentioned problems. Its purpose is to replace the ideal single-layer covering film with a multilayer covering film of more than four layers whose characteristic matrix does not become a unit matrix, thereby realizing an optical semiconductor device having an anti-reflection film whose reflectivity becomes zero or minimum at a desired wavelength, i.e., the center wavelength of the laser, and also to obtain a design method for an anti-reflection film for an optical semiconductor device.

[0014] The optical semiconductor device of the present disclosure has an effective refractive index of n c , the laser wavelength is λ, and there is an anti-reflection film on one or both end faces, wherein,

[0015] The antireflection film is composed of a plurality of cover films, and the plurality of cover films are stacked from a first cover film having a refractive index of n1 and a film thickness of d1 to a first cover film having a refractive index of n1 and a film thickness of d1. i And the film thickness is d i The i-th covering film (i≧4) is composed of i covering films,

[0016] The thickness of the kth film of the kth layer (1≦k≦i) of the multilayer film is set to be greater than λ / 2 / n k or less than λ / 2 / n k ,

[0017] In the above-mentioned multilayer covering film, the refractive index of at least one layer of the above-mentioned covering film is greater than the above-mentioned effective refractive index n c The square root of the refractive index n f , and the refractive index of at least one layer of the above-mentioned covering film is less than the above-mentioned refractive index n f ,

[0018] The characteristic matrix of the multilayer film obtained by sequentially accumulating the characteristic matrix of the first film to the characteristic matrix of the i-th film and the characteristic matrix of the multilayer film having a refractive index of n f And the film thickness d f =λ / 4 / n f The properties of an ideal single-layer covering film matrix are equal,

[0019] The film thickness of i-3 of the above i films is a preset film thickness.

[0020] The film thicknesses of the remaining three films among the i films are determined by solving three simultaneous equations derived from the characteristic matrix of the multilayer film.

[0021] The present disclosure relates to a method for designing an antireflection film for an optical semiconductor device, wherein the antireflection film for an optical semiconductor device is formed on a substrate having an effective refractive index of n c One or both end faces of an optical semiconductor device having a laser wavelength of λ, and composed of a multilayer cover film formed by stacking i cover films (i≧4),

[0022] The method for designing an antireflection film for an optical semiconductor device comprises the following steps:

[0023] For the i-th cover film, the refractive index of the first cover film is n1 and the film thickness is d1, and the refractive index of the i-th cover film is n i and the film thickness becomes d i The refractive index and film thickness of each covering film are set in sequence;

[0024] The thickness of the k-th film of the k-th layer (1≦k≦i) of the multilayer film is set to be greater than λ / 2 / n k or less than λ / 2 / n k ;

[0025] In the above-mentioned multi-layer covering film, the refractive index of at least one layer of the above-mentioned covering film is greater than the above-mentioned effective refractive index n c The square root of the refractive index n f , and the refractive index of at least one layer of the above-mentioned covering film is less than the above-mentioned refractive index n f Select the material constituting the above-mentioned covering film in a certain manner;

[0026] The characteristic matrix of the multilayer film obtained by sequentially accumulating the characteristic matrix of the first film to the characteristic matrix of the i-th film is assumed to be equal to the refractive index n. f And the film thickness d f =λ / 4 / n f The properties of the ideal single-layer covering film matrix are equal;

[0027] Presetting the film thickness of i-3 covering films among the i covering films; and

[0028] The film thicknesses of the remaining three films among the i films are determined by solving three simultaneous equations derived from the characteristic matrix of the multi-layer films.

[0029] According to the optical semiconductor device involved in the present disclosure, for the anti-reflection film composed of i layers of covering films (i≧4) formed on the end face, the film thicknesses of three layers in each covering film are determined by using the product of characteristic matrices. Therefore, even if the effective refractive index of the optical semiconductor device, the refractive index of the material constituting the anti-reflection film, and the order of the covering films constituting the anti-reflection film are changed, it is possible to easily obtain an optical semiconductor device having an anti-reflection film whose reflectivity becomes zero or minimum at a desired wavelength.

[0030] According to the design method of an anti-reflection film for an optical semiconductor device involved in the present disclosure, the anti-reflection film composed of i layers of covering films (i≧4) formed on the end surface is designed to use the product of characteristic matrices to determine the film thicknesses of three layers in each covering film. Therefore, even if the effective refractive index of the optical semiconductor device, the refractive index of the material constituting the anti-reflection film, and the order of the covering films constituting the anti-reflection film change, it is possible to easily design an anti-reflection film for an optical semiconductor device whose reflectivity becomes zero or minimum at a desired wavelength. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 This is a schematic diagram showing a quantum cascade laser device as an example of the optical semiconductor device according to the first embodiment.

[0032] Figure 2 A quantum cascade laser device as an example of the optical semiconductor device according to the first embodiment Figure 1 A cross-sectional view taken along line AA is shown.

[0033] Figure 3 This is a schematic diagram showing an example of the structure of an antireflection film in a quantum cascade laser device as an example of the optical semiconductor device according to the first embodiment.

[0034] Figure 4 This is a diagram showing the wavelength dependency of the reflectivity of an example of an antireflection film in a quantum cascade laser device which is an example of the optical semiconductor device according to the first embodiment.

[0035] Figure 5 This is a diagram showing the wavelength dependency of the reflectivity according to another example of the antireflection film in the quantum cascade laser device which is an example of the optical semiconductor device according to the first modification of the first embodiment.

[0036] Figure 6 This is a schematic diagram showing the structure of an antireflection film in a quantum cascade laser device as an example of the optical semiconductor device according to the second embodiment.

[0037] Figure 7This is a diagram showing the wavelength dependency of the reflectance of an antireflection film in a quantum cascade laser device as an example of the optical semiconductor device according to the second embodiment.

[0038] Figure 8 This is a schematic diagram showing the structure of an antireflection film in a quantum cascade laser device as an example of the optical semiconductor device according to the third embodiment.

[0039] Fig. 9 This is a diagram showing the wavelength dependency of the reflectance of an antireflection film in a quantum cascade laser device as an example of the optical semiconductor device according to the third embodiment.

[0040] Fig.10 This is a schematic diagram showing the structure of an antireflection film in a quantum cascade laser device as an example of the optical semiconductor device according to the fourth embodiment.

[0041] Fig.11 This is a diagram showing the wavelength dependency of the reflectance of an antireflection film in a quantum cascade laser device as an example of the optical semiconductor device according to the fourth embodiment.

[0042] Fig.12 This is a schematic diagram showing the structure of a wide-bandwidth semiconductor laser device having an oscillation wavelength of 975 nm, which is an example of the optical semiconductor device according to the fifth embodiment.

[0043] Fig.13 This is a schematic diagram showing the structure of an antireflection film in a wide-band semiconductor laser device having an oscillation wavelength of 975 nm, which is an example of the optical semiconductor device according to the fifth embodiment.

[0044] Fig.14 This is a diagram showing the wavelength dependency of the reflectance of an antireflection film in a wide-bandwidth semiconductor laser device having an oscillation wavelength of 975 nm, which is an example of the optical semiconductor device according to the fifth embodiment. DETAILED DESCRIPTION

[0045] Implementation Method 1

[0046] <Structure of Optical Semiconductor Device According to Embodiment 1>

[0047] Figure 11 is a schematic diagram of a quantum cascade laser device as an example of an optical semiconductor device 100 according to Embodiment 1. The quantum cascade laser device is composed of a back side n-type electrode 1, an n-type InP substrate 2, an n-type InP buffer layer 3, an n-type GaInAs first optical confinement layer 4, a core region 5 composed of 30 to 40 stages, an n-type GaInAs second optical confinement layer 6, an n-type InP cladding layer 7, an n-type GaInAs contact layer 8, and a front side n-type electrode 9.

[0048] The core region 5 is composed of a multi-quantum well (MQW) layered with quantum well layers composed of GaInAs and barrier layers composed of AlInAs alternately stacked. The oscillation wavelength of the quantum cascade laser device is mid-infrared light of 3 to 24 μm. Figure 1 In FIG. 1 , the antireflection film 10 provided on the end surface of the quantum cascade laser device is not shown.

[0049] When the quantum cascade laser device is in operation, the back side n-type electrode 1 is biased negatively and the front side n-type electrode 9 is biased positively. When in operation, a voltage is applied between the back side n-type electrode 1 and the front side n-type electrode 9, thereby injecting current into the quantum cascade laser device to perform laser oscillation.

[0050] Figure 2 It is along Figure 1 A cross-sectional view of the AA line quantum cascade laser device. Figure 2 As shown, an anti-reflection film 10 is provided on the front end surface of the quantum cascade laser device.

[0051] <Design method of anti-reflection film for optical semiconductor device>

[0052] When a cover film having a refractive index of n and a film thickness of d is provided on the end face of a quantum cascade laser device, the characteristic matrix is ​​represented by the following equation (1). In equation (1), φ is a phase term, and when the laser wavelength of the quantum cascade laser device is set to λ, the characteristic matrix is ​​represented by the following equation (2). In equation (2), i is an imaginary unit.

[0053]

[0054] φ=2πnd / λ (2)

[0055] The effective refractive index in a quantum cascade laser device is n c In the case of f Defined as the effective refractive index n c The square root of the film thickness d is set on the end face of the quantum cascade laser device. f =λ / (4n f) of the cover film, the characteristic matrix becomes the following formula (3). In formula (3), the reflectivity R becomes zero at the wavelength λ. Hereinafter, this single-layer cover film is also referred to as an ideal single-layer cover film.

[0056]

[0057] The following is a method of replacing an ideal single-layer cover film with a multi-layer cover film consisting of four layers. Figure 3 is a schematic diagram showing an example of a multilayer cover film consisting of four layers. Figure 3 In the embodiment, the anti-reflection film 10a is composed of an effective refractive index n c The quantum cascade laser device 110 with a refractive index of 3.2 is composed of four covering films, namely, a first covering film 12 composed of CeO2 with a refractive index n1 of 1.70 and a film thickness d1 of 50 nm, a second covering film 13 composed of YF3 (yttrium fluoride) with a refractive index n2 of 1.40 and a film thickness d2, a third covering film 14 composed of ZnS with a refractive index n3 of 2.20 and a film thickness d3, and a fourth covering film 15 composed of CeF3 with a refractive index n4 of 1.45 and a film thickness d4. Hereinafter, for example, the first covering film 12 composed of CeO2 may be referred to as CeO2 first covering film 12, and other covering films may be referred to similarly.

[0058] In the structure of the above-mentioned anti-reflection film 10a, the film thickness d1 of the CeO2 first covering film 12 is set to 50nm, but the film thickness d1 is not limited to this and can be set arbitrarily. In addition, the film thickness d2 of the YF3 second covering film 13, the film thickness d3 of the ZnS third covering film 14, and the film thickness d4 of the CeF3 fourth covering film 15 are unknown variables, but they are film thickness values ​​that can be calculated by the method described later. The desired wavelength λ is set to 10μm. The characteristic matrix of the above-mentioned four-layer covering film is shown in the following formula (4). Among them, m 11 、m 12 、m 21 、m 22 Represents each matrix item.

[0059]

[0060] The phase terms φ1, φ2, φ3, and φ4 of equation (4) are expressed as in the following equation (5).

[0061]

[0062] Since the refractive index n1 of the CeO2 first covering film 12 is known, and the film thickness d1 is a pre-set film thickness value, the phase term φ1 becomes a calculable value. Therefore, the unknowns are the three phase terms φ2, φ3, and φ4. Since there are three unknowns, for example, by solving three simultaneous equations as in equation (6), the film thicknesses d2, d3, and d4 are calculated according to equation (6). Among them, the refractive index of each covering film is a value inherent to the material constituting each covering film, that is, a known value. However, the refractive index of the material constituting each covering film may sometimes vary to a certain extent depending on the film forming conditions, but including this variation, the refractive index is considered to be a known value.

[0063]

[0064] The thickness of each coating film calculated by equation (6) is d2 = 513.38 nm, d3 = 374.58 nm, and d4 = 574.57 nm. The calculation results show that the reflectivity R becomes the minimum at a wavelength of 10.09 μm, but does not become the minimum at a desired wavelength of 10 μm.

[0065] Four equations can be created for three unknowns. Therefore, three unknowns can be obtained using any three equations, but sometimes the minimum reflectivity R does not appear at the desired wavelength. For this reason, the term m in row and column of the ideal single-layer coating is 11 and the 2 rows and 2 columns of item m 22 Since both are zero, three equations are created using all four terms of the matrix as shown in the following equation (7), and the three equations are solved simultaneously.

[0066]

[0067] In this case, the thickness of each coating film can be obtained as solutions of the three simultaneous equations as d2 = 493.74 nm, d3 = 387.37 nm, and d4 = 557.57 nm. According to Non-Patent Document 1, since the reflectivity R is expressed as the following equation (8), the wavelength dependence of the reflectivity R can be obtained.

[0068]

[0069] Compared with the patent document 1 Figure 7 The wavelength dependence of the reflectance R of the antireflection film 10a composed of the four-layer cover film according to the first embodiment is shown in FIG. Figure 4A dotted curve 16 and a solid curve 17 respectively represent the wavelength dependence of the reflectance R of the antireflection film composed of four layers of coatings described in Patent Document 1 and the antireflection film 10 a composed of four layers of coatings according to Embodiment 1.

[0070] In the antireflection film 10a composed of four layers of coatings according to the first embodiment, it can be seen from the solid line curve 17 that the reflectivity R becomes minimum (zero) at the desired wavelength λ=10 μm, and the frequency band where the reflectivity R becomes 0.1% or less is a wide band such as 634 nm. Figure 7 In the anti-reflection film composed of the four-layer cover film involved, it can be seen from the curve 16 composed of the dotted line that the reflectivity R does not become the minimum (zero) at the desired wavelength λ=10μm, and the frequency band where the reflectivity R becomes 0.1% or less is also a narrow band such as 589nm. That is, it can be seen that even if the structures of each film thickness are compared, the anti-reflection film 10a composed of the four-layer cover film involved in Embodiment 1 and the anti-reflection film composed of the four-layer cover film structure described in Patent Document 1 are significantly different.

[0071] In order to make the characteristic matrix of the ideal single-layer cover film consistent with the characteristic matrix of the four-layer cover film, as long as the refractive index of one or more of the four-layer cover films is greater than the refractive index n of the ideal single-layer cover film, f , and the refractive index of one or more of the four layers of the covering film is less than the refractive index n of the ideal single-layer covering film f That's it.

[0072] Since the antireflection film 10a composed of the four-layer film according to the first embodiment is a film obtained by replacing the ideal single-layer film, the total film thickness of the four-layer film is 1489 nm, which is close to the film thickness d of the ideal single-layer film. f =1398nm, and the anti-reflection film as a whole is thin. Therefore, the anti-reflection film 10a composed of the four-layer cover film involved in the first embodiment has the characteristics of small film strain that is a problem in thick anti-reflection films and is not easy to peel off, thereby achieving the effect of improving the reliability of the quantum cascade laser device.

[0073] The reason why CeO 2 is used as the material of the first cover film 12 constituting the antireflection film 10 a is to maintain good adhesion between the semiconductor constituting the quantum cascade laser device and the cover film.

[0074] Furthermore, in Embodiment 1, a quantum cascade laser device fabricated on an InP substrate is described as an example of the optical semiconductor device 100 . However, the present invention is not limited thereto, and for example, a semiconductor laser device fabricated on a GaAs substrate may be used.

[0075] <Effects of the Optical Semiconductor Device According to Embodiment 1>

[0076] As described above, according to the optical semiconductor device according to the first embodiment, when the effective refractive index is n c The end face of the optical semiconductor device is provided with a four-layer cover film with a known refractive index and an unknown thickness of any three layers and a predetermined thickness of the remaining layer. If the refractive index n f Let the effective refractive index n c The square root of the characteristic matrix of each cover film is solved by the product of the refractive index n f And the film thickness is λ / (4n f ) is equal to the characteristic matrix of the ideal single-layer cover film, and the three simultaneous equations are derived to determine the film thickness of the three layers as unknowns, thus playing a role in determining the effective refractive index n of the optical semiconductor device. c , the refractive index of the material constituting the anti-reflection film, and the order of the various covering films constituting the anti-reflection film, the effect of an optical semiconductor device having an anti-reflection film whose reflectance R is minimized at a desired wavelength λ can be easily obtained.

[0077] <Effects of the method for designing an antireflection film for an optical semiconductor device according to the first embodiment>

[0078] As described above, according to the design method of the antireflection film for the optical semiconductor device according to the first embodiment, the effective refractive index is n. c The end face of the optical semiconductor device is provided with four layers of covering films, the refractive index of which is known and the thickness of any three layers is assumed to be unknown, and the thickness of the remaining layer is predetermined. f Let the effective refractive index n c The square root of the characteristic matrix of each cover film is solved by the product of the refractive index n f And the film thickness is λ / (4n f ) is equal to the characteristic matrix of the ideal single-layer cover film, and the three simultaneous equations are derived to determine the thickness of the three layers as unknowns, so as to design the thickness of each cover film of the four-layer cover film, thereby playing a role in determining the effective refractive index n of the optical semiconductor device. c By changing the refractive index of the material constituting the anti-reflection film and the order of the respective cover films constituting the anti-reflection film, it is possible to easily design an anti-reflection film for an optical semiconductor device in which the reflectance R is minimized at a desired wavelength λ.

[0079] Modification 1 of Embodiment 1

[0080] In Embodiment 1, the film thickness d1 of the CeO2 first coating film 12 is set to 50nm, but the film thickness of any coating film in the four-layer coating film may be set arbitrarily. For example, when the film thickness d2 of the YF3 second coating film 13 is set to 70nm, the film thickness d1 of the CeO2 first coating film 12, the film thickness d3 of the ZnS third coating film 14, and the film thickness d4 of the CeF3 fourth coating film 15 become unknowns. If the three simultaneous equations are solved by the same method as in Embodiment 1, the film thicknesses of the four-layer coating films other than the pre-set film thickness d2 become d1=759.47nm, d3=262.43nm, and d4=347.32nm. In the anti-reflection film 10a composed of the above four-layer coating film, the reflectivity R becomes minimum (zero) at the desired wavelength λ=10μm. Figure 5 The wavelength dependency of the reflectance R of the antireflection film 10a composed of the above-mentioned four-layer cover film is shown.

[0081] Furthermore, assuming that the film thickness d3 of the third ZnS film 14 is set to 300 nm, the film thickness d1 of the first CeO2 film 12, the film thickness d2 of the second YF3 film 13, and the film thickness d4 of the fourth CeF3 film 15 become unknowns. If the three simultaneous equations are solved in the same way, the thicknesses of the four layers of films except for the predetermined film thickness d3 become d1 = 625.84 nm, d2 = 148.88 nm, and d4 = 366.72 nm. In the anti-reflection film 10a composed of the above four layers of films, the reflectivity R becomes minimum (zero) at the desired wavelength λ = 10 μm.

[0082] Furthermore, assuming that the film thickness d4 of the CeF3 fourth coating film 15 is set to 500nm, the film thickness d1 of the CeO2 first coating film 12, the film thickness d2 of the YF3 second coating film 13, and the film thickness d3 of the ZnS third coating film 14 become unknowns. If the three simultaneous equations are solved in the same manner, the film thicknesses of the four coating films except for the predetermined film thickness d4 become d1 = 182.38nm, d2 = 408.55nm, and d3 = 380.00nm. In the anti-reflection film 10a composed of the above-mentioned four-layer coating film, the reflectivity R becomes minimum (zero) at the desired wavelength λ = 10μm. As described above, the film thickness of any one of the four coating films may be set to a predetermined film thickness value, or may be an arbitrarily set film thickness value.

[0083] <Effects of Optical Semiconductor Device According to Modification 1 of Embodiment 1>

[0084] As described above, according to the optical semiconductor device according to the first modification of the first embodiment, in the case where the effective refractive index is n cThe end face of the optical semiconductor device is provided with a four-layer cover film with a known refractive index, an unknown thickness of any three layers, and a predetermined thickness of the remaining layer. If the refractive index n f Let the effective refractive index n c The square root of the characteristic matrix of each cover film is solved by the product of the refractive index n f And the film thickness is λ / (4n f ) is equal to the characteristic matrix of the ideal single-layer cover film, and the three simultaneous equations are derived to determine the film thickness of the three layers as unknowns, thus playing a role in determining the effective refractive index n of the optical semiconductor device. c By changing the refractive index of the material constituting the anti-reflection film, the order of the various covering films constituting the anti-reflection film, etc., it is also possible to easily obtain an optical semiconductor device having an anti-reflection film whose reflectance R is minimized at a desired wavelength λ.

[0085] Implementation Method 2

[0086] The optical semiconductor device according to Embodiment 2 has an anti-reflection film composed of a multilayer covering film having more than four layers, that is, more than five layers. The design method for an anti-reflection film for an optical semiconductor device having a four-layer covering film described in Embodiment 1 can also be applied to the anti-reflection film 10b composed of a multilayer covering film having more than four layers, which is described below.

[0087] <Structure of optical semiconductor device according to Embodiment 2>

[0088] Figure 6 1 is a schematic diagram showing the structure of an antireflection film 10b composed of five layers of cover films in a quantum cascade laser device 120 as an example of an optical semiconductor device according to Embodiment 2. Figure 6 As shown, the anti-reflection film 10b is composed of an effective refractive index n c The quantum cascade laser device 120 with a refractive index of 3.2 has a first covering film 18 made of CeO2 with a refractive index n1 of 1.70 and a film thickness d1 of 200 nm, a second covering film 19 made of ZnS with a refractive index n2 of 2.20 and a film thickness d2 of 100 nm, a third covering film 20 made of YF3 with a refractive index n3 of 1.40 and a film thickness d3, a fourth covering film 21 made of ZnSe (zinc selenide) with a refractive index n4 of 2.41 and a film thickness d4, and a fifth covering film 22 made of CeF3 with a refractive index n5 of 1.45 and a film thickness d5.

[0089] <Method for Designing Antireflection Film for Optical Semiconductor Device According to Embodiment 2>

[0090] In the above-mentioned five-layer coating, the film thickness d1 of the CeO2 first coating 18 is set to 200nm and the film thickness d2 of the ZnS second coating 19 is set to 100nm, but it is not limited to these film thickness values, but can be set to any film thickness value. In addition, the film thickness d3 of the YF3 third coating 20, the film thickness d4 of the ZnSe fourth coating 21, and the film thickness d5 of the CeF3 fifth coating 22 are unknown. The desired wavelength λ is set to 10μm. The characteristic matrix of the anti-reflection film 10b composed of the above-mentioned five-layer coating is shown in the following formula (9).

[0091]

[0092] In the equation (9), the phase terms φ1, φ2, φ3, φ4, and φ5 are expressed as in the following equation (10).

[0093]

[0094] Since the refractive index n1 of the CeO2 first coating film 18 and the refractive index n2 of the ZnS second coating film 19 are known, and the film thickness d1 of the CeO2 first coating film 18 and the film thickness d2 of the ZnS second coating film 19 are set film thickness values, the phase terms φ1 and φ2 are calculable values. Therefore, the unknowns are the three phase terms φ3, φ4, and φ5. Since there are three unknowns, if the three simultaneous equations are solved in the same way as in Embodiment 1, the film thicknesses of the remaining three layers of the five-layer coating film become d3 = 466.88nm, d4 = 256.20nm, and d5 = 412.65nm. In the anti-reflection film 10b composed of the above-mentioned five-layer coating film, the reflectivity R becomes minimum (zero) at the desired wavelength λ = 10μm. Figure 7 The wavelength dependency of the reflectance R of the antireflection film 10b composed of the above five-layer cover film is shown. The bandwidth where the reflectance R becomes 0.1% or less is 625 nm.

[0095] In embodiment 2, the film thickness of the CeO2 first covering film 18 and the ZnS second covering film 19 in the five-layer covering film constituting the anti-reflection film 10b is set to a predetermined film thickness value, but is not limited to these film thickness values. It is sufficient to pre-set the film thickness of any two layers of the five covering films, and the film thickness values ​​of the two layers can also be arbitrary.

[0096] In Embodiment 2, a five-layer covering film is exemplified as a multilayer covering film constituting the anti-reflection film 10b. However, by applying the above-mentioned design method of an anti-reflection film for an optical semiconductor device, the film thickness can also be determined in the same manner for a multilayer covering film having more than six layers. If the number of layers of the multilayer covering film constituting the anti-reflection film is set to i (i≧4), the film thickness of any i-3 covering films among the i covering films can be arbitrarily set in advance.

[0097] In order to make the characteristic matrix of the ideal single-layer cover film consistent with the characteristic matrix of the i-layer cover film (i≧4), as long as the refractive index of one or more of the i-layer cover films is greater than the refractive index n of the ideal single-layer cover film, f , and the refractive index of one or more of the i-layer covering films is less than the refractive index n of the ideal single-layer covering film f That's it.

[0098] Hereinafter, a case where an i-layer coating film is formed of i coating films will be described. In the case of the i-layer coating film, the characteristic matrix of the i-layer coating film is represented by the following formula (11).

[0099]

[0100] In equation (11), the phase terms φ1, φ2, ··φ i As shown in the following formula (12).

[0101]

[0102] The thicknesses of any i-3 films among the i films may be set arbitrarily in advance. Therefore, there are three unknowns in equation (11), and by solving three simultaneous equations in the same manner as in the first embodiment, the thicknesses of the remaining three films can be calculated.

[0103] For an effective refractive index of n c The steps of a method for designing an anti-reflection film composed of a multilayer covering film formed by stacking i covering films (i≧4) and formed on one or both end faces of an optical semiconductor device with a laser wavelength of λ, that is, a method for designing an anti-reflection film for an optical semiconductor device, are summarized as follows.

[0104] (First step)

[0105] For i-th cover film, the refractive index of the first cover film is n1 and the film thickness is d1, and the refractive index of the i-th cover film is n i and the film thickness becomes d i The refractive index and film thickness of each cover film are set in sequence in a manner where the value of each refractive index is known.

[0106] (Second step)

[0107] The thickness of the k-th film of the k-th layer (1≦k≦i) of the multilayer film is set to be greater than λ / 2 / n k or less than λ / 2 / n k .

[0108] (Third step)

[0109] The refractive index of at least one of the multilayer covering films is greater than the effective refractive index n c The square root of the refractive index n f , and the refractive index of at least one layer of the covering film is less than the refractive index n f The material constituting the covering film is selected in a certain manner.

[0110] (Step 4)

[0111] The characteristic matrix of the multilayer film obtained by sequentially accumulating the characteristic matrix of the first film to the characteristic matrix of the i-th film is assumed to be equal to the characteristic matrix of the multilayer film having a refractive index of n. f And the film thickness d f =λ / 4 / n f The properties of an ideal single-layer covering film are equal to the matrix.

[0112] (Fifth step)

[0113] The film thicknesses of i-3 films among i films constituting the multilayer film are set in advance.

[0114] (Sixth step)

[0115] The film thicknesses of the remaining three films excluding i-3 films among the i films constituting the multilayer film are determined by solving the three simultaneous equations derived from the characteristic matrix of the multilayer film.

[0116] <Effects of Embodiment 2>

[0117] As described above, according to the optical semiconductor device and the design method of the antireflection film for an optical semiconductor device according to the second embodiment, in the case where the effective refractive index is n c The end face of the optical semiconductor device is provided with i-layer covering films (i≧4) whose refractive index is known and whose thicknesses are unknown except for any i-3 covering films with predetermined film thicknesses. If the refractive index n f Let the effective refractive index n c The square root of the characteristic matrix of each cover film is solved by the product of the refractive index n f And the film thickness is λ / (4n f) is equal to the characteristic matrix of the ideal single-layer cover film, and the three simultaneous equations are derived to determine the film thickness of the three layers as unknowns, thus playing a role in determining the effective refractive index n of the optical semiconductor device. c , the refractive index of the material constituting the anti-reflection film, and the order of the various covering films constituting the anti-reflection film, it is also easy to obtain an optical semiconductor device having an anti-reflection film whose reflectivity R is minimized at a desired wavelength λ, and a method for designing an anti-reflection film for an optical semiconductor device.

[0118] Implementation 3

[0119] Figure 8 : represents the effective refractive index n of the quantum cascade laser device 130 as an example of the optical semiconductor device according to the third embodiment. c Schematic diagram of the structure of the anti-reflection film 10c when the effective refractive index n of the quantum cascade laser device is 3.3. c It varies depending on the element configuration such as the structure and composition of the core region, light confinement layer, and cladding layer.

[0120] <Structure of optical semiconductor device according to Embodiment 3>

[0121] like Figure 8 As shown, the anti-reflection film 10c is composed of an effective refractive index n c The quantum cascade laser device 130 with a refractive index of 3.3 is composed of four covering films, including a first covering film 24 composed of CeO2 with a refractive index n1 of 1.70 and a film thickness d1, a second covering film 25 composed of YF3 with a refractive index n2 of 1.40 and a film thickness d2, a third covering film 26 composed of ZnS with a refractive index n3 of 2.20 and a film thickness d3 of 300nm, and a fourth covering film 27 composed of CeF3 with a refractive index n4 of 1.45 and a film thickness d4.

[0122] In the above four-layer coating, the film thickness d3 of the ZnS third coating 26 is set to 300 nm, but it is not limited to this film thickness value, and can be set to any film thickness value. In addition, the film thickness d1 of the CeO2 first coating 24, the film thickness d2 of the YF3 second coating 25, and the film thickness d4 of the CeF3 fourth coating 27 are unknown. The desired wavelength λ is set to 10 μm.

[0123] Since there are three unknowns, if three simultaneous equations are solved in the same manner as in Embodiment 1, the thicknesses of the four-layer coating except the predetermined thickness d3 are d1 = 709.60 nm, d2 = 58.32 nm, and d4 = 357.95 nm. In the anti-reflection film 10c composed of the above four-layer coating, the reflectivity R is minimum (zero) at the desired wavelength λ = 10 μm. Fig. 9 The wavelength dependence of the reflectivity R of the antireflection film 10c composed of four layers of coatings is shown. The bandwidth where the reflectivity R becomes 0.1% or less is 614 nm. The effective refractive index n of the quantum cascade laser device is c It is not limited to 3.2 or 3.3, and other effective refractive indices n can also be applied. c The value of .

[0124] <Effects of Embodiment 3>

[0125] As described above, according to the optical semiconductor device and the design method of the anti-reflection film for the optical semiconductor device involved in the third embodiment, a four-layer covering film with a known refractive index and an unknown film thickness of any three layers and a predetermined film thickness of the remaining layer is provided on the end face of the optical semiconductor device with an effective refractive index of 3.3. f Let the effective refractive index n c The square root of the characteristic matrix of each cover film is solved by the product of the refractive index n f And the film thickness is λ / (4n f ) is equal to the characteristic matrix of the ideal single-layer cover film, and the three simultaneous equations are derived to determine the film thickness of the three layers as unknowns, thereby playing a role in determining the effective refractive index n of the optical semiconductor device. c , the refractive index of the material constituting the anti-reflection film, and the order of the various covering films constituting the anti-reflection film, it is also easy to obtain an optical semiconductor device having an anti-reflection film whose reflectivity R is minimized at a desired wavelength λ, and a method for designing an anti-reflection film for an optical semiconductor device.

[0126] Implementation 4

[0127] Fig.10 : represents the effective refractive index n of the quantum cascade laser device 140 as an example of the optical semiconductor device according to the fourth embodiment. c Schematic diagram of the structure of the anti-reflection film 10d composed of five layers of cover films in the case of 3.2. Since the quantum cascade laser device oscillates using inter-subband transitions, it can oscillate at a wavelength in the range of 3μm to 24μm. As an example of another laser wavelength different from the laser wavelength 10μm of the quantum cascade laser devices 110, 120, and 130 of embodiments 1 to 3, the quantum cascade laser device 140 has an anti-reflection film 10d corresponding to the laser wavelength 11μm.

[0128] <Structure of optical semiconductor device according to fourth embodiment>

[0129] like Fig.10 As shown, the anti-reflection film 10d is composed of an effective refractive index n cThe quantum cascade laser device 140 with a refractive index of 3.2 is composed of five covering films, including a first covering film 29 composed of CeO2 with a refractive index n1 of 1.70 and a film thickness d1 of 200nm, a second covering film 30 composed of ZnS with a refractive index n2 of 2.20 and a film thickness d2 of 100nm, a third covering film 31 composed of YF3 with a refractive index n3 of 1.40 and a film thickness d3, a fourth covering film 32 composed of ZnSe with a refractive index n4 of 2.41 and a film thickness d4, and a fifth covering film 33 composed of CeF3 with a refractive index n5 of 1.45 and a film thickness d5.

[0130] In the above five-layer coating, the film thickness d1 of the CeO2 first coating 29 is preset to 200nm and the film thickness d2 of the ZnS second coating 30 is preset to 100nm, but it is not limited to these film thickness values ​​and can be set to any film thickness value. In addition, the film thickness d3 of the YF3 third coating 31, the film thickness d4 of the ZnSe fourth coating 32, and the film thickness d5 of the CeF3 fifth coating 33 are unknown. The desired wavelength λ is set to 11μm.

[0131] Since there are three unknowns, if three simultaneous equations are solved in the same manner as in Embodiment 2, the thicknesses of the five-layer coating except for the preset thickness d1 and the thickness d2 are d3 = 522.43 nm, d4 = 286.93 nm, and d5 = 474.50 nm. In the anti-reflection film 10d composed of the five-layer coating, the reflectivity R is minimum (zero) at the desired wavelength λ = 11 μm. Fig.11 The wavelength dependence of the reflectivity R of the antireflection film 10d composed of five layers of coating is shown. The bandwidth where the reflectivity R becomes 0.1% or less is 625nm. The oscillation wavelength of the quantum cascade laser device is not limited to 10μm or 11μm, but can be any wavelength within the range of 3μm to 24μm.

[0132] <Effects of Embodiment 4>

[0133] As described above, according to the optical semiconductor device and the design method of the antireflection film for an optical semiconductor device according to the fourth embodiment, in the case of an effective refractive index n c The end face of the optical semiconductor device with a refractive index of 3.2 is provided with a five-layer cover film in which the refractive index is known and the film thickness of any three layers is unknown and the film thickness of the remaining two layers is predetermined. f Let the effective refractive index n c The square root of the characteristic matrix of each cover film is solved by the product of the refractive index n f And the film thickness is λ / (4n f) is equal to the characteristic matrix of the ideal single-layer cover film, and the three simultaneous equations are derived to determine the film thickness of the three layers as unknowns, thus playing a role in determining the effective refractive index n of the optical semiconductor device. c By changing the refractive index of the material constituting the anti-reflection film, the order of the various covering films constituting the anti-reflection film, etc., it is possible to obtain an optical semiconductor device having an anti-reflection film whose reflectivity R is minimized at a desired wavelength of 11 μm and a method for designing an anti-reflection film for an optical semiconductor device.

[0134] Implementation method 5

[0135] In Embodiments 1 to 4, quantum cascade laser devices 110, 120, 130, and 140 are described as an example of an optical semiconductor device. However, the present disclosure is not limited to quantum cascade laser devices, but is applicable to all optical semiconductor devices having an antireflection film on the end surface.

[0136] <Structure of optical semiconductor device according to Embodiment 5>

[0137] As an example of the optical semiconductor device according to the fifth embodiment, a wide-band semiconductor laser device 200 having an oscillation wavelength of 975 nm and including an antireflection film 10 e formed of a multilayer cover film will be described. Fig.12 Patent Document 3 is a schematic diagram of a wide-bandwidth semiconductor laser device 200 having an oscillation wavelength of 975 nm, the device structure of which is disclosed.

[0138] The wide-amplitude semiconductor laser device 200 is composed of an active region 41 having a width W and cladding regions 42a and 42b. The wide-amplitude semiconductor laser device 200 is composed of an n-type electrode 43, an n-type GaAs substrate 44, and an n-type Al with an Al composition ratio of 0.20 and a layer thickness of 1.3 μm. 0.20 Ga 0.80 As first cladding layer 45, n-type Al with Al composition ratio of 0.25 and layer thickness of 0.2 mm 0.25 Ga 0.75 As second cladding layer 46, n-side Al with Al composition ratio of 0.16 and layer thickness of 1.05 μm 0.16 Ga 0.84 As first guide layer 47, n-side Al with Al composition ratio of 0.14 and layer thickness of 0.1 μm 0.14 Ga 0.86 As second guide layer 48, n-side GaAs with a P composition ratio of 0.12 and a layer thickness of 8 nm 0.88 P 0.12 The barrier layer 49, In ​​composition ratio of 0.12 and thickness of 8 nm 0.12 Ga 0.88As active layer 50, p-side GaAs with a P composition ratio of 0.12 and a layer thickness of 8 nm 0.88 P 0.12 The barrier layer 51 is a p-side Al layer having an Al composition ratio of 0.14 and a layer thickness of 0.35 μm. 0.14 Ga 0.86 As first guide layer 52, p-side Al with Al composition ratio of 0.16 and layer thickness of 0.30 μm 0.16 Ga 0.84 As second guide layer 53, p-type Al with an Al composition ratio of 0.55 and a layer thickness of 40 nm 0.55 Ga 0.45 As first etching stop layer 54, p-type Al with Al composition ratio of 0.25 and layer thickness of 0.1 μm 0.25 Ga 0.75 As first cladding layer 55, p-type Al with an Al composition ratio of 0.55 and a layer thickness of 40 nm 0.55 Ga 0.45 As second etching stop layer 56, p-type Al with Al composition ratio of 0.25 and layer thickness of 1.4 μm 0.25 Ga 0.75 The SiN film 59 is composed of an As second cladding layer 57 , a p-type GaAs contact layer 58 with a thickness of 0.2 μm, a SiN film 59 , and a p-type electrode 60 .

[0139] In the wide-band semiconductor laser device 200, In 0.12 Ga 0.88 The In composition ratio and layer thickness of the As active layer 50 are such that the oscillation wavelength λ is 975 nm. In addition, the effective refractive indexes of the active region 41 and the cladding regions 42a and 42b are 3.41739 and 3.41658, respectively. Since the laser light mainly exists in the active region 41, 3.41739 is used as the effective refractive index n of the wide-bandwidth semiconductor laser device 200 in the following investigation of the anti-reflection film. c .

[0140] Fig.13 1 is a schematic diagram showing the structure of an antireflection film 10e provided on an end face of a wide-band semiconductor laser device 200 having an oscillation wavelength of 975 nm, which is an example of an optical semiconductor device according to Embodiment 5. Fig.13 As shown, the anti-reflection film 10e is composed of an effective refractive index n cThe wide-band semiconductor laser device 200 with a refractive index of 3.41739 is composed of four covering films, including a first covering film 62 composed of Al2O3 (Aluminum Oxide) with a refractive index n1 of 1.63 and a film thickness d1 from the end face side, a second covering film 63 composed of Ta2O5 (Tantalum Pentoxide) with a refractive index n2 of 2.00 and a film thickness d2, a third covering film 64 composed of Al2O3 with a refractive index n3 of 1.63 and a film thickness d3 of 100nm, and a fourth covering film 65 composed of SiO2 (Silicon Dioxide) with a refractive index n4 of 1.45 and a film thickness d4.

[0141] In the above four-layer coating, the thickness d3 of the third Al2O3 coating 64 is set to 100nm, but it is not limited to this thickness value, and can be set to any thickness value. In addition, the thickness d1 of the first Al2O3 coating 62, the thickness d2 of the second Ta2O5 coating 63, and the thickness d4 of the fourth SiO2 coating 65 are unknown. The desired wavelength λ is 0.975μm (975nm).

[0142] Since there are three unknowns, if three simultaneous equations are solved in the same manner as in Embodiment 1, the thicknesses of the four-layer coating except the predetermined thickness d3 are d1 = 310.63 nm, d2 = 77.80 nm, and d4 = 271.67 nm. In the anti-reflection film 10e composed of the above four-layer coating, the reflectivity R is minimum (zero) at the desired wavelength λ = 0.975 μm. Fig.14 The wavelength dependency of the reflectance R of the antireflection film 10 e composed of four cover films is shown.

[0143] In the fifth embodiment, Ta2O5 is used as a material having an effective refractive index n2 of the wide-band semiconductor laser device 200. c The square root of the refractive index n f A material with a large refractive index, but amorphous Si can also be used instead of Ta2O5.

[0144] <Effects of Embodiment 5>

[0145] As described above, according to the optical semiconductor device and the design method of the anti-reflection film for the optical semiconductor device involved in the fifth embodiment, a four-layer cover film with a known refractive index and an unknown film thickness of any three layers and a predetermined film thickness of the remaining layer is provided on the end face of a wide-band semiconductor laser device with an oscillation wavelength λ of 975 nm as an example of an optical semiconductor device. If the refractive index n f Let the effective refractive index n cThe square root of the characteristic matrix of each cover film is solved by the product of the refractive index n f And the film thickness is λ / (4n f ) is equal to the characteristic matrix of the ideal single-layer cover film, and the three simultaneous equations are derived to determine the film thickness of the three layers as unknowns, thus playing a role in determining the effective refractive index n of the wide-band semiconductor laser device with an oscillation wavelength of 975nm. c , the refractive index of the material constituting the anti-reflection film, and the order of the various covering films constituting the anti-reflection film, it is also easy to obtain an optical semiconductor device having an anti-reflection film whose reflectivity R is minimum at an oscillation wavelength of 975nm and a method for designing an anti-reflection film for an optical semiconductor device.

[0146] In each embodiment, the refractive index of the cover film varies depending on the film forming method, and therefore the refractive index of each material shown in each embodiment is only an example. f A material with a large refractive index, and one or more materials having a refractive index n greater than that of an ideal single-layer cover film. f The structure of a multilayer cover film of a material with a small refractive index can realize the anti-reflection film of the present disclosure. As described above, the anti-reflection film involved in the present disclosure can be applied to the entire optical semiconductor device regardless of the wavelength or device structure.

[0147] The present disclosure describes various exemplary embodiments and examples, but various features, methods, and functions described in one or more embodiments are not limited to application in specific embodiments, but can be applied to the embodiments alone or in various combinations.

[0148] Therefore, numerous modifications not shown in the examples are conceivable within the technical scope disclosed in the present specification, including, for example, the modification, addition or omission of at least one component, and the extraction and combination of at least one component with components of other embodiments.

[0149] Description of Reference Numerals

[0150] 1…back side n-type electrode; 2…n-type InP substrate; 3…n-type InP buffer layer; 4…n-type GaInAs first light confinement layer; 5…core region; 6…n-type GaInAs second light confinement layer; 7…n-type InP cladding layer; 8…n-type GaInAs contact layer; 9…surface side n-type electrode; 10, 10a, 10b, 10c, 10d, 10e…anti-reflection film; 12, 18, 24, 29…CeO2 first covering film; 13, 25…YF3 second covering film; 14, 26…ZnS third covering film; 15, 27…CeF3 fourth covering film; 19, 30…ZnS second covering film; 20, 31…YF3 third covering film; 21, 32…ZnSe fourth covering film; 22, 33…CeF3 fifth covering film; 41…active region; 42a, 42b…cladding region; 43…n-type electrode; 44…n-type GaAs substrate; 45…n-type Al 0.20 Ga 0.80 As first cladding layer; 46...n-type Al 0.25 Ga 0.75 As second cladding layer; 47...n side Al 0.16 Ga 0.84 As first guide layer; 48...n side Al 0.14 Ga 0.86 As second guide layer; 49...n-side GaAs 0.88 P 0.12 Barrier layer; 50…In 0.12 Ga 0.88 As active layer; 51…p-side GaAs 0.88 P 0.12 Barrier layer; 52…p-side Al 0.14 Ga 0.86 As first guide layer; 53...p side Al 0.16 Ga 0.84 As second guide layer; 54...p-type Al 0.55 Ga 0.45 As first etching stop layer; 55...p-type Al 0.25 Ga 0.75 As first cladding layer; 56…p-type Al 0.55 Ga 0.45 As second etching stop layer; 57...p-type Al 0.25 Ga 0.75 As second cladding layer; 58 ... p-type GaAs contact layer; 59 ... SiN film; 60 ... p-type electrode; 100 ... optical semiconductor device; 110, 120, 130, 140 ... quantum cascade laser device; 200 ... wide-band semiconductor laser device.

Claims

1. An optical semiconductor device having an effective refractive index n c , the laser wavelength is λ, and an anti-reflection film is provided on one or both end faces, characterized in that, The antireflection film is composed of a plurality of cover films, wherein the plurality of cover films are stacked from a first cover film having a refractive index of n1 and a film thickness of d1 to a first cover film having a refractive index of n1 and a film thickness of d1. i And the film thickness is d i The i-th covering film is composed of i covering films up to the i-th covering film, where i≧4, The thickness of the kth covering film of the kth layer of the multilayer covering film is set to be greater than λ / 2 / n k or less than λ / 2 / n k , where 1≦k≦i, In the multi-layer cover film, the refractive index of at least one layer of the cover film is greater than the effective refractive index n c The square root of the refractive index n f , and the refractive index of at least one layer of the cover film is less than the refractive index n f , The characteristic matrix of the multilayered film obtained by sequentially accumulating the characteristic matrix from the first cover film to the characteristic matrix of the i-th cover film and the characteristic matrix of the multilayered film having a refractive index of n f And the film thickness d f =λ / 4 / n f The properties of an ideal single-layer covering film matrix are equal, The film thickness of i-3 covering films among the i covering films is a preset film thickness, The film thicknesses of the remaining three films among the i films are determined by solving three simultaneous equations derived from the characteristic matrix of the multilayer film.

2. The optical semiconductor device according to claim 1, wherein The anti-reflection film is composed of four layers of cover films.

3. The optical semiconductor device according to claim 1, wherein The anti-reflection film is composed of five layers of cover films.

4. The optical semiconductor device according to any one of claims 1 to 3, wherein The optical semiconductor device is a semiconductor laser device.

5. The optical semiconductor device according to any one of claims 1 to 3, wherein The optical semiconductor device is a quantum cascade semiconductor laser device.

6. The optical semiconductor device according to any one of claims 1 to 5, wherein: Each of the covering films is composed of any one of CeO2, YF3, ZnS, CeF3, ZnSe, Al2O3, Ta2O5, SiO2 and amorphous Si.

7. A method for designing an anti-reflection film for an optical semiconductor device, wherein the anti-reflection film for an optical semiconductor device is formed on a substrate having an effective refractive index n c One or both end faces of an optical semiconductor device having a laser wavelength of λ, and composed of a multilayer cover film formed by stacking i cover films, where i≧4, It is characterized in that The method for designing an anti-reflection film for an optical semiconductor device comprises the following steps: For the i-th cover film, the refractive index of the first cover film is n1 and the film thickness is d1, and the refractive index of the i-th cover film is n i and the film thickness becomes d i The refractive index and film thickness of each covering film are set in sequence; The film thickness of the k-th film of the k-th layer of the multilayer film is set to be greater than λ / 2 / n k or less than λ / 2 / n k , where 1≦k≦i; So that in the multi-layer cover film, the refractive index of at least one layer of the cover film is greater than the effective refractive index n c The square root of the refractive index n f , and the refractive index of at least one layer of the cover film is less than the refractive index n f Selecting the material constituting the covering film in a manner as described above; The characteristic matrix of the multilayer film obtained by sequentially accumulating the characteristic matrix of the first cover film to the characteristic matrix of the i-th cover film is set to be equal to the refractive index n f And the film thickness d f =λ / 4 / n f The properties of the ideal single-layer covering film matrix are equal; Presetting the film thickness of i-3 covering films among the i covering films; as well as The film thicknesses of the remaining three covering films among the i covering films are determined by solving three simultaneous equations derived from the characteristic matrix of the multi-layer covering films.

8. The method for designing an antireflection film for an optical semiconductor device according to claim 7, wherein: The anti-reflection film is composed of four layers of cover films.

9. The method for designing an antireflection film for an optical semiconductor device according to claim 7, wherein: The anti-reflection film is composed of five layers of cover films.

10. The method for designing an antireflection film for an optical semiconductor device according to any one of claims 7 to 9, wherein: Each of the covering films is composed of any one of CeO2, YF3, ZnS, CeF3, ZnSe, Al2O3, Ta2O5, SiO2 and amorphous Si.

Citation Information

Patent Citations

  • Semiconductor optical element

    JP1993243689A

  • Quantum cascade laser element, quantum cascade laser device, and method for manufacturing quantum cascade laser device

    JP2021163922A

  • Semiconductor laser device

    WO2019053854A1