Modified tobacco additive as well as preparation method and application thereof
By using Fe3O4 nanoparticles coated with oleic acid in cigarettes to form ordered mesoporous graphene microspheres, combined with metal oxide catalysis, the problem of decreasing combustion and moisturizing properties caused by the reduction of tar in the prior art is solved, and the problem of reducing tar volume is achieved. Higher user experience and lower aerosol generation.
Patent Information
- Application Number
- CN202411126495.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-08-16
AI Technical Summary
While reducing the amount of cigarette tar, the prior art reduces the combustion and moisturizing properties, affects the user experience, and the additive preparation cost is high and is not suitable for large-scale production.
Fe3O4 nanoparticles coated with oleic acid are pyrolysis, calcination, etching and graphitization to form ordered mesoporous graphene microspheres as modified tobacco additives, combined with metal oxide catalytic oxide support to reduce tar oil and improve moisturization.
Improves the combustion and moisturizing properties of tobacco, reduces the generation of high-profile substances in aerosols, increases the moisture of smoke, reduces stimulation, significantly improves throat comfort, and improves the comprehensive experience score of cigarettes .
Smart Images

Figure CN118923900A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of cigarette additives and relates to a modified tobacco additive and a preparation method and application thereof. Background Art
[0002] The smoke produced when tobacco burns contains tar, nicotine, etc. The health hazards of smoking mainly come from certain components in the smoke tar produced during the burning process of cigarettes, such as benzo[α]pyrene, dibenzo[α,h]anthracene, nitrosamines and certain nitrogen heterocyclic compounds and other substances of high concern in the aerosol. Therefore, the key to reducing the harm of smoking to the human body is to reduce the amount of tar in cigarettes.
[0003] my country's cigarettes are mainly traditional flue-cured tobacco, which has a high sugar content. Reducing the tar content of cigarette products is an important part of tobacco research. With the increasing attention paid to health by cigarette consumers, the research and development of low-tar cigarette products is an inevitable trend in the development of the tobacco industry.
[0004] CN108686653A discloses a method for preparing a bimetallic nanocatalyst for reducing the CO release of cigarette smoke. The method reduces the tar content of cigarette products and reduces CO release by adding acetate fiber tow to gold / silver bimetallic nanocatalysts and rolling them into a filter. However, the preparation cost of the catalyst is high, which is not conducive to large-scale production.
[0005] CN111084405A discloses a reconstituted tobacco sheet and a preparation method thereof, wherein an emulsifier is used to emulsify aerosol generators of different solubility to obtain a uniformly dispersed aerosol generator emulsion, and then tobacco material, aerosol generator emulsion, fiber, adhesive, emulsion stabilizer, tobacco flavor and fragrance are added to medium water, and a uniform slurry is obtained by high-speed dispersion, and the slurry is spread on a receiving object by casting, and the reconstituted tobacco sheet is obtained after drying. By adding an emulsifier, the tar content is reduced, so that the tobacco sheet can continuously and stably smoke.
[0006] The above scheme reduces the tar content of cigarettes by adding additives, but the additives will reduce the combustibility and moisturizing properties of cigarettes, resulting in a reduced user experience. Summary of the invention
[0007] The purpose of the present invention is to provide a modified tobacco additive and a preparation method and application thereof. The modified tobacco additive of the present invention can not only improve the combustibility of tobacco, reduce the amount of tar in cigarettes, and reduce the generation of highly concerned substances in aerosols, but also improve the moisturizing property of tobacco, so that cigarettes can maintain their original style unchanged, increase the moisturizing feeling of smoke, reduce irritation, and significantly improve throat comfort.
[0008] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:
[0009] In a first aspect, the present invention provides a method for preparing a modified tobacco additive, the preparation method comprising the following steps:
[0010] (1) Mixing oleic acid iron, oleic acid and a first solvent, and subjecting the mixture to pyrolysis to obtain oleic acid-coated Fe 3 O 4 Nanoparticles, oleic acid-coated Fe 3 O 4 Nanoparticles are mixed with a second solvent to obtain oleic acid-coated Fe 3 O 4 Nanoparticle dispersion;
[0011] (2) Surfactant solution and oleic acid-coated Fe 3 O 4 Nanoparticle dispersions are mixed and heated to obtain Fe 3 O 4 Nano-superlattice microspheres, the Fe 3 O 4 Nano-superlattice microspheres are calcined to obtain carbonized Fe 3 O 4 Nano superlattice microspheres;
[0012] (3) Carbonized Fe 3 O 4 After the nano-superlattice microspheres are etched, they are graphitized to obtain ordered mesoporous graphene microspheres;
[0013] (4) Mixing the modified metal source solution and the ordered mesoporous graphene microspheres and stirring them to react, thereby obtaining a precursor, and hydrolyzing the precursor and then sintering it to obtain the modified tobacco additive.
[0014] The present invention uses monodisperse oleic acid coated Fe 3 O 4 Nanoparticles were used as basic building blocks to prepare Fe ions by solvent evaporation induced self-assembly (EISA) in an oil-in-water emulsion system. 3 O 4 Nano superlattice microspheres. During the solvent evaporation process, the intermolecular forces of the ligands on the surface of the nanoparticles induce the nanoparticles to be closely arranged in a face-centered cubic close-packed manner to form a superlattice structure. At the same time, since this process occurs in an oil-in-water emulsion system, it is equivalent to assembling in a confined space, so the overall morphology of the obtained product is consistent with the shape of the emulsion droplets. After calcination, the oleic acid ligands are carbonized to form amorphous carbon coated on the particle surface. The oleic acid-coated Fe inside the microspheres after etching 3 O 4The nanoparticles are etched away to obtain mesoporous carbon microspheres. After high-temperature graphitization again, the graphitization degree of the mesoporous carbon microspheres is further improved to obtain mesoporous graphene microspheres (OMGSs) with a wall thickness of only a few layers of graphene. Then, OMGSs is used as a skeleton, and the active substance precursor is adsorbed by wet impregnation, and then induced hydrolysis and high-temperature treatment are performed to obtain the modified tobacco additive. The modified tobacco additive is a composite microsphere of metal oxide and mesoporous graphene. The metal oxide is distributed on the surface of the mesoporous graphene microsphere. The mesoporous graphene microsphere has high porosity, low volume density, developed specific surface area and unique physical properties. It can have good filtering, purification and separation effects on gases and liquids, reduce the amount of tar, and improve the wettability of tobacco. At the same time, it can serve as a carrier of catalytic oxides, and the metal oxide can catalyze the decomposition of organic matter and reduce the generation of highly concerned substances in aerosols such as aldehydes, benzenes, indenes and condensed aromatic hydrocarbons. At the same time, the metal oxide has excellent oxygen storage and release function (OSC effect) and high-temperature rapid oxygen vacancy diffusion ability, which can realize the storage / release of oxygen.
[0015] Preferably, in step (1), the first solvent comprises octadecene.
[0016] Preferably, the molar ratio of iron oleate to oleic acid in step (1) is 1:(0.6-0.9), for example: 1:0.6, 1:0.65, 1:0.7, 1:0.8 or 1:0.9, etc., not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0017] Preferably, the temperature of the pyrolysis treatment in step (1) is 300-350°C, for example, 300°C, 310°C, 320°C, 330°C or 350°C, etc., and is not limited to the listed values. Other values not listed within the numerical range are also applicable.
[0018] Preferably, the time of the pyrolysis treatment in step (1) is 20 to 40 minutes, for example, 20 minutes, 25 minutes, 30 minutes, 35 minutes or 40 minutes, etc., not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0019] Preferably, in step (1), the second solvent comprises n-hexane.
[0020] Preferably, the oleic acid-coated Fe 3 O 4 The concentration of the nanoparticle dispersion is 300-800 g / L, for example, 300 g / L, 400 g / L, 500 g / L, 700 g / L or 800 g / L, etc., but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0021] Preferably, the solute of the surfactant solution in step (2) includes dodecyltrimethylammonium bromide.
[0022] Preferably, the solvent of the surfactant solution in step (2) comprises deionized water.
[0023] Preferably, the concentration of the surfactant solution in step (2) is 15 to 25 g / L, for example, 15 g / L, 18 g / L, 20 g / L, 22 g / L or 25 g / L, etc., but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0024] Preferably, the mixing in step (2) is followed by stirring.
[0025] Preferably, the stirring time is 10 to 20 min, for example, 10 min, 12 min, 15 min, 18 min or 20 min, etc., and is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0026] Preferably, the temperature of the heating treatment in step (2) is 45-55°C, for example, 45°C, 48°C, 50°C, 52°C or 55°C, etc., and is not limited to the listed values. Other values not listed within the numerical range are also applicable.
[0027] Preferably, the heating treatment time in step (2) is 1 to 3 hours, for example, 1 hour, 1.5 hours, 2 hours, 2.5 hours or 3 hours, etc., and is not limited to the listed values. Other values not listed within the numerical range are also applicable.
[0028] Preferably, the atmosphere of the calcination treatment in step (2) comprises nitrogen and / or argon.
[0029] Preferably, the temperature of the calcination treatment in step (2) is 450-550°C, for example, 450°C, 480°C, 500°C, 520°C or 550°C, etc., not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0030] Preferably, the calcination time in step (2) is 1 to 3 hours, for example, 1 hour, 1.5 hours, 2 hours, 2.5 hours or 3 hours, etc., not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0031] Preferably, the etching solution used in the etching treatment in step (3) comprises hydrochloric acid.
[0032] Preferably, the etching treatment in step (3) is followed by washing, centrifugation and drying.
[0033] Preferably, the washing detergent comprises ethanol and / or water.
[0034] Preferably, the atmosphere of the graphitization treatment in step (3) comprises nitrogen and / or argon.
[0035] Preferably, the temperature of the graphitization treatment in step (3) is 1000-1500°C, for example, 1000°C, 1100°C, 1200°C, 1400°C or 1500°C, etc., not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0036] Preferably, the time of the graphitization treatment in step (3) is 1 to 3 hours, for example: 1 hour, 1.5 hours, 2 hours, 2.5 hours or 3 hours, etc., not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0037] Preferably, the solute of the modified metal source solution in step (4) comprises a hydrolyzable germanium salt and / or a hydrolyzable tin salt.
[0038] Preferably, the hydrolyzable germanium salt comprises Ge(OEt) 4 .
[0039] Preferably, the hydrolyzable tin salt comprises SnCl 2 .
[0040] Preferably, the solvent of the modified metal source solution in step (4) comprises ethanol.
[0041] Preferably, the concentration of the modified metal source solution in step (4) is 0.05 to 0.2 g / L, for example, 0.05 g / L, 0.08 g / L, 0.1 g / L, 0.15 g / L or 0.2 g / L, etc., not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0042] Preferably, the mass volume ratio of the ordered mesoporous graphene microspheres to the modified metal source solution in step (4) is 1 to 3 g / L, for example: 1 g / L, 1.5 g / L, 2 g / L, 2.5 g / L or 3 g / L, etc., not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0043] Preferably, the stirring reaction time in step (4) is 3 to 5 h, for example, 3 h, 3.5 h, 4 h, 4.5 h or 5 h, etc., not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0044] Preferably, the hydrolysis treatment in step (4) comprises mixing the precursor with aqueous ammonia.
[0045] Preferably, the temperature of the hydrolysis treatment in step (4) is 50-70°C, for example, 50°C, 55°C, 60°C, 65°C or 70°C, etc., and is not limited to the listed values. Other values not listed within the numerical range are also applicable.
[0046] Preferably, the sintering temperature in step (4) is 300-400°C, for example, 300°C, 320°C, 350°C, 380°C or 400°C, etc., but is not limited to the listed values. Other values not listed within the range are also applicable.
[0047] Preferably, the sintering time in step (4) is 0.5 to 1.5 h, for example, 0.5 h, 0.8 h, 1 h, 1.2 h or 1.5 h, etc., and is not limited to the listed values. Other values not listed within the range are also applicable.
[0048] In a second aspect, the present invention provides a modified tobacco additive, wherein the modified tobacco additive is prepared by the preparation method described in the first aspect.
[0049] In a third aspect, the present invention provides a cigarette shredded tobacco, wherein the cigarette shredded tobacco comprises the modified tobacco additive as described in the second aspect.
[0050] Preferably, based on the mass of the cigarette tobacco being 100%, the mass fraction of the tobacco additive is 0.5-3%, for example, 0.5%, 1%, 1.5%, 2% or 3%, etc., and is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0051] Preferably, the cigarette shreds further include tobacco raw materials and a binder.
[0052] Preferably, the binder comprises sodium carboxymethylcellulose.
[0053] Compared with the prior art, the present invention has the following beneficial effects:
[0054] (1) The modified tobacco additive of the present invention can not only improve the combustibility of tobacco and reduce the generation of highly concerned substances in aerosol, but also improve the moisturizing property of tobacco, so that the cigarette can maintain its original style, increase the moist feeling of smoke, reduce irritation, and significantly improve throat comfort.
[0055] (2) The total experience score of the shredded tobacco made by adding the modified tobacco additive of the present invention in terms of gloss, aroma, harmony, miscellaneous smell, irritation and aftertaste can reach 88.5 points or more. By adjusting the conditions in the preparation process and the ratio of raw materials, the total score can reach 94.5 points or more. BRIEF DESCRIPTION OF THE DRAWINGS
[0056] Figure 1The carbonized Fe 3 O 4 SEM image of nanosuperlattice microspheres.
[0057] Figure 2 The carbonized Fe 3 O 4 SEM image of the nanosuperlattice. DETAILED DESCRIPTION
[0058] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0059] Example 1
[0060] This embodiment provides a modified tobacco additive, which is prepared by the following method:
[0061] (1) Iron oleate and oleic acid were dissolved in 400 g of octadecene at a molar ratio of 1:0.75, and the mixture was pyrolyzed at 320°C for 30 min, and then rapidly cooled. After cooling to room temperature, the mixture was washed with ethanol, isopropanol and n-hexane, and centrifuged. The resulting precipitate was oleic acid-coated Fe 3 O 4 Nanoparticles, oleic acid-coated Fe 3 O 4 Nanoparticles were mixed with n-hexane to obtain 500 g / L of oleic acid-coated Fe 3 O 4 Nanoparticle dispersion;
[0062] (2) Add 2g dodecyltrimethylammonium bromide (DTAB) and 100mL deionized water to a 250mL three-necked flask. After DTAB is completely dissolved, add 10ml Fe 3 O 4 The nanoparticle dispersion was stirred rapidly for 15 minutes to form an oil-in-water emulsion system. Then it was heated to 50°C and kept at this temperature for 2 hours to allow the n-hexane to completely evaporate. Finally, the Fe 3 O 4 The solid was sucked down and repeatedly washed with deionized water to remove the residual surfactant DTAB on the surface to obtain Fe 3 O 4 Nano superlattice microspheres, Fe 3 O 4 The nano-superlattice microspheres were placed in a tube furnace and heated to 500°C at a heating rate of 2°C / min in an argon atmosphere. The temperature was kept constant for 2 h to carbonize the oleic acid ligands and coat the particle surface in the form of amorphous carbon. The particles were cooled to room temperature to obtain a black powder, which was carbonized Fe 3O 4 Nano-superlattice microspheres, the carbonized Fe 3 O 4 SEM images of nano-superlattice microspheres are shown in Figure 1 As shown;
[0063] (3) Using hydrochloric acid to carbonize Fe 3 O 4 The nano-superlattice microspheres were etched, washed, dried, and then graphitized at 1200°C to obtain ordered mesoporous graphene microspheres (OMGSs).
[0064] (4) SnCl 2 Dissolve in ethanol to make a solution with a concentration of 0.1 g / L. Then, take 20 mg of dried OMGSs and disperse them in 10 mL of SnCl 2 ethanol solution, stirred for 4 hours. Centrifuged to obtain black powder, and washed with a small amount of ethanol to remove excess SnCl on the surface. 2 The obtained black powder was exposed to an aqueous ammonia solution at 60°C to allow the volatilized ammonia to induce SnCl 2 Hydrolyze to generate tin hydroxide. Then use deionized water to wash away the NH 4 The dried black powder was transferred to a porcelain boat and heated to 350°C in a tube furnace for 1 hour to completely convert the tin hydroxide into SnO 2 And improve its crystallization degree. Finally, the modified tobacco additive is obtained.
[0065] Example 2
[0066] This embodiment provides a modified tobacco additive, which is prepared by the following method:
[0067] (1) Iron oleate and oleic acid were dissolved in 400 g of octadecene at a molar ratio of 1:0.6, and the mixture was pyrolyzed at 300°C for 40 min and then rapidly cooled. After cooling to room temperature, the mixture was washed with ethanol, isopropanol and n-hexane, and centrifuged. The resulting precipitate was oleic acid-coated Fe 3 O 4 Nanoparticles, oleic acid-coated Fe 3 O 4 Nanoparticles were mixed with n-hexane to obtain 300 g / L of oleic acid-coated Fe 3 O 4 Nanoparticle dispersion;
[0068] (2) Add 1.5 g dodecyltrimethylammonium bromide (DTAB) and 100 mL deionized water to a 250 mL three-necked flask. After DTAB is completely dissolved, add 10 mL Fe 3 O4 The nanoparticle dispersion was stirred rapidly for 10 min to form an oil-in-water emulsion system. Then it was heated to 45 °C and kept at this temperature for 3 h to allow the n-hexane to completely evaporate. Finally, the Fe 3 O 4 The solid was sucked down and repeatedly washed with deionized water to remove the residual surfactant DTAB on the surface to obtain Fe 3 O 4 Nano superlattice microspheres, Fe 3 O 4 The nano-superlattice microspheres were placed in a tube furnace and heated to 450°C at a heating rate of 2°C / min in an argon atmosphere. The temperature was kept constant for 3 h to carbonize the oleic acid ligands and coat the particle surface in the form of amorphous carbon. The particles were cooled to room temperature to obtain a black powder, which was carbonized Fe 3 O 4 Nano superlattice microspheres;
[0069] (3) Using hydrochloric acid to carbonize Fe 3 O 4 The nano-superlattice microspheres were etched, washed, dried, and then graphitized at 1000°C to obtain ordered mesoporous graphene microspheres (OMGSs).
[0070] (4) Ge(OEt) 4 Dissolve in ethanol to a concentration of 0.05 g mL -1 Then, 20 mg of dried OMGSs were dispersed in 10 mL of Ge(OEt) 4 In ethanol solution, stir for 4 hours. After centrifugation, a black powder is obtained, and the excess Ge(OEt) on the surface is washed with a small amount of ethanol. 4 . It was exposed to an aqueous ammonia solution at 60°C to promote Ge(OEt) 4 Hydrolyze to germanium hydroxide. Then wash away the surface impurities with deionized water and dry in an oven. Repeat this step twice. After drying, place the product in a tube furnace and heat it to 350°C for 1 hour to completely convert Ge hydroxide into GeO 2 , and finally the modified tobacco additive is obtained.
[0071] Example 3
[0072] This embodiment provides a modified tobacco additive, which is prepared by the following method:
[0073] (1) Iron oleate and oleic acid were dissolved in 400 g of octadecene at a molar ratio of 1:0.9, and the mixture was pyrolyzed at 350°C for 20 min and then rapidly cooled. After cooling to room temperature, the mixture was washed with ethanol, isopropanol and n-hexane, and centrifuged. The resulting precipitate was oleic acid-coated Fe 3 O4 Nanoparticles, oleic acid-coated Fe 3 O 4 Nanoparticles were mixed with n-hexane to obtain 800 g / L of oleic acid-coated Fe 3 O 4 Nanoparticle dispersion;
[0074] (2) Add 2.5 g of dodecyltrimethylammonium bromide (DTAB) and 100 mL of deionized water to a 250 mL three-necked flask. After DTAB is completely dissolved, add 10 mL of Fe 3 O 4 The nanoparticle dispersion was stirred rapidly for 20 minutes to form an oil-in-water emulsion system. Then it was heated to 55°C and kept at this temperature for 1 hour to allow the n-hexane to completely evaporate. Finally, the Fe 3 O 4 The solid was sucked down and repeatedly washed with deionized water to remove the residual surfactant DTAB on the surface to obtain Fe 3 O 4 Nano superlattice microspheres, Fe 3 O 4 The nano-superlattice microspheres were placed in a tube furnace and heated to 500°C at a heating rate of 2°C / min in a nitrogen atmosphere. The temperature was kept constant for 1 h to carbonize the oleic acid ligands and coat the particle surface in the form of amorphous carbon. The particles were cooled to room temperature to obtain a black powder, which was carbonized Fe 3 O 4 Nano superlattice microspheres;
[0075] (3) Using hydrochloric acid to carbonize Fe 3 O 4 The nano-superlattice microspheres were etched, washed, dried, and then graphitized at 1500°C to obtain ordered mesoporous graphene microspheres (OMGSs).
[0076] (4) SnCl 2 Dissolve in ethanol to make a solution with a concentration of 0.2 g / L. Then, take 30 mg of dried OMGSs and disperse them in 10 mL of SnCl 2 ethanol solution, stirred for 5 h. Centrifuged to obtain black powder, and washed with a small amount of ethanol to remove excess SnCl on the surface. 2 The obtained black powder was exposed to an aqueous ammonia solution at 70°C to allow the volatilized ammonia to induce SnCl 2 Hydrolyze to generate tin hydroxide. Then use deionized water to wash away the NH 4 The dried black powder was transferred to a porcelain boat and heated to 400°C in a tube furnace for 0.5 h to completely convert the tin hydroxide into SnO 2And improve its crystallization degree, finally obtain the modified tobacco additive.
[0077] Example 4
[0078] The only difference between this embodiment and embodiment 1 is that the temperature of the heating treatment in step (2) is 40° C., and the other conditions and parameters are exactly the same as those in embodiment 1.
[0079] Example 5
[0080] The only difference between this embodiment and embodiment 1 is that the temperature of the heating treatment in step (2) is 60° C., and the other conditions and parameters are exactly the same as those in embodiment 1.
[0081] Example 6
[0082] The only difference between this embodiment and embodiment 1 is that the concentration of the modified metal source solution in step (4) is 0.01 g / L, and the other conditions and parameters are exactly the same as those in embodiment 1.
[0083] Example 7
[0084] The only difference between this embodiment and embodiment 1 is that the concentration of the modified metal source solution in step (4) is 0.3 g / L, and the other conditions and parameters are exactly the same as those in embodiment 1.
[0085] Comparative Example 1
[0086] The difference between this comparative example and Example 1 is that no surfactant is added in step (2), and the other conditions and parameters are exactly the same as those in Example 1. 3 O 4 SEM images of nano-superlattice Figure 1 shown.
[0087] Comparative Example 2
[0088] The only difference between this comparative example and Example 1 is that no modified metal source is added in step (4), and the other conditions and parameters are exactly the same as those in Example 1.
[0089] The tobacco additives obtained in the above examples and comparative examples were added to the cigarette tobacco formula in a flavoring and material adding manner, and formed using a cigarette making machine. The cigarettes were smoked according to the national standard GB5606.4-2005 "Technical Requirements for Sensory Properties of Cigarettes". The results of the smoking test are shown in Table 1.
[0090] Table 1
[0091]
[0092]
[0093] As can be seen from Table 1, according to Examples 1-7, the total experience score of the comprehensive gloss, aroma, harmony, miscellaneous smell, irritation and aftertaste of the cigarette made from the shredded tobacco added with the modified tobacco additive of the present invention can reach more than 88.5 points. By adjusting the conditions in the preparation process and the ratio of raw materials, the total score can reach more than 94.5 points.
[0094] By comparing Example 1 with Examples 4-5, it can be seen that in the preparation process of the modified tobacco additive of the present invention, the temperature of the heating treatment in step (2) will affect its performance. When the temperature of the heating treatment is controlled at 45-55° C., the performance of the modified tobacco additive is better. If the temperature of the heating treatment is too high, although the solvent can be evaporated quickly, the formed water-in-oil emulsion system will be destroyed, resulting in the Fe 3 O 4 The structural stability of nano-superlattice microspheres is poor, and the material morphology will be destroyed during subsequent processing. If the heating temperature is too low, the solvent will evaporate too slowly and incompletely.
[0095] By comparing Example 1 with Examples 6-7, it can be seen that in the preparation process of the modified tobacco additive of the present invention, the concentration of the modified metal source solution in step (4) will affect its performance. When the concentration of the modified metal source solution is controlled at 0.05-0.2 g / L, the performance of the modified tobacco additive is better. If the concentration of the modified metal source solution is too high, there is too much metal on the surface of the mesoporous graphene microspheres, which blocks the pores of the mesoporous graphene microspheres and causes the performance to decrease. If the concentration of the modified metal source solution is too low, it cannot effectively catalyze the decomposition of organic matter and the storage performance of oxygen decreases.
[0096] By comparing Example 1 with Comparative Example 1, it can be seen that the present invention can induce ferroferric oxide to self-assemble by adding a surfactant to form Fe 3 O 4 Nano superlattice microspheres.
[0097] By comparing Example 1 and Comparative Example 2, it can be seen that metal oxides can catalyze the decomposition of organic matter and reduce the generation of substances of high concern in aerosols such as aldehydes, benzenes, indenes and condensed ring aromatic hydrocarbons. At the same time, metal oxides have excellent oxygen storage and release functions (OSC effect) and high-temperature rapid oxygen vacancy diffusion capabilities, which can realize the storage / release of oxygen.
[0098] Application Example 1
[0099] In this application example, the modified tobacco additive obtained in Example 1 is added into the cigarette tobacco formula in the form of flavoring and adding material to prepare cigarettes.
[0100] Comparative application example 1
[0101] The only difference between this comparative application example and application example 1 is that no modified tobacco additive is added to make the cigarette.
[0102] The aerosol test bases of Application Example 1 and Comparative Application Example 1 are:
[0103] GB / T23203.1-2013; GB / T19609-2004; GB / T23356-2009; GB / T21130-2007; GB / T23355-2009; YC / T253-2019; YC / T255-2008; YC / T254-2008; YC / T377-2019; Q / CTQ5-2010 (laboratory method, determination of tobacco-specific nitrosamines in total particulate matter in mainstream smoke). The test results are shown in Table 2.
[0104] Table 2
[0105]
[0106]
[0107] It can be seen from Table 2 that the amount of substances of high concern in the aerosol of the cigarette containing the modified tobacco additive of the present invention is significantly reduced compared with the cigarette without the modified tobacco additive, and the user experience is significantly improved.
[0108] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.
Claims
1. A method for preparing a modified tobacco additive, characterized in that: The preparation method comprises the following steps: (1) mixing oleic acid iron, oleic acid and a first solvent, subjecting the mixture to pyrolysis treatment to obtain oleic acid-coated Fe3O4 nanoparticles, and mixing the oleic acid-coated Fe3O4 nanoparticles with a second solvent to obtain a dispersion of oleic acid-coated Fe3O4 nanoparticles; (2) mixing a surfactant solution with an oleic acid-coated Fe3O4 nanoparticle dispersion, heating the mixture to obtain Fe3O4 nanosuperlattice microspheres, and calcining the Fe3O4 nanosuperlattice microspheres to obtain carbonized Fe3O4 nanosuperlattice microspheres; (3) After etching the carbonized Fe3O4 nano-superlattice microspheres, the ordered mesoporous graphene microspheres are obtained by graphitization; (4) Mixing the modified metal source solution and the ordered mesoporous graphene microspheres and stirring them to react, thereby obtaining a precursor, and hydrolyzing the precursor and then sintering it to obtain the modified tobacco additive.
2. The preparation method according to claim 1, characterized in that Step (1) the first solvent comprises octadecene; Preferably, the molar ratio of iron oleate to oleic acid in step (1) is 1:(0.6-0.9); Preferably, the temperature of the pyrolysis treatment in step (1) is 300-350°C; Preferably, the pyrolysis treatment time in step (1) is 20 to 40 minutes; Preferably, the second solvent in step (1) comprises n-hexane; Preferably, the concentration of the oleic acid-coated Fe3O4 nanoparticle dispersion in step (1) is 300-800 g / L.
3. The preparation method according to claim 1 or 2, characterized in that: The solute of the surfactant solution in step (2) includes dodecyltrimethylammonium bromide; Preferably, the solvent of the surfactant solution in step (2) comprises deionized water; Preferably, the concentration of the surfactant solution in step (2) is 15 to 25 g / L; Preferably, the mixing in step (2) is followed by stirring; Preferably, the stirring time is 10 to 20 minutes; Preferably, the temperature of the heating treatment in step (2) is 45-55°C; Preferably, the heating treatment time in step (2) is 1 to 3 hours.
4. The preparation method according to any one of claims 1 to 3, characterized in that: The calcination atmosphere in step (2) includes nitrogen and / or argon; Preferably, the calcination temperature in step (2) is 450-550°C; Preferably, the calcination treatment time in step (2) is 1 to 3 hours.
5. The preparation method according to any one of claims 1 to 4, characterized in that: The etching solution of the etching treatment in step (3) comprises hydrochloric acid; Preferably, the etching treatment in step (3) is followed by washing, centrifugation and drying; Preferably, the washing detergent comprises ethanol and / or water; Preferably, the atmosphere of the graphitization treatment in step (3) comprises nitrogen and / or argon; Preferably, the temperature of the graphitization treatment in step (3) is 1000-1500°C; Preferably, the graphitization treatment time in step (3) is 1 to 3 hours.
6. The preparation method according to any one of claims 1 to 5, characterized in that: The solute of the modified metal source solution in step (4) comprises a hydrolyzable germanium salt and / or a hydrolyzable tin salt; Preferably, the hydrolyzable germanium salt comprises Ge(OEt)4; Preferably, the hydrolyzable tin salt comprises SnCl2; Preferably, the solvent of the modified metal source solution in step (4) comprises ethanol; Preferably, the concentration of the modified metal source solution in step (4) is 0.05 to 0.2 g / L; Preferably, the mass volume ratio of the ordered mesoporous graphene microspheres to the modified metal source solution in step (4) is 1 to 3 g / L; Preferably, the stirring reaction time in step (4) is 3 to 5 hours.
7. The preparation method according to any one of claims 1 to 6, characterized in that: The hydrolysis treatment in step (4) comprises mixing the precursor with aqueous ammonia; Preferably, the temperature of the hydrolysis treatment in step (4) is 50-70°C; Preferably, the sintering temperature in step (4) is 300-400°C; Preferably, the sintering time in step (4) is 0.5 to 1.5 hours.
8. A modified tobacco additive, characterized in that: The modified tobacco additive is prepared by the preparation method according to any one of claims 1-7.
9. A cigarette tobacco, characterized in that: The cigarette shreds contain the modified tobacco additive according to claim 8.
10. The cigarette shreds according to claim 9, characterized in that: Based on the mass of the cigarette tobacco being 100%, the mass fraction of the tobacco additive is 0.5 to 3%; Preferably, the cigarette shreds further include tobacco raw materials and a binder; Preferably, the binder comprises sodium carboxymethylcellulose.
Citation Information
Patent Citations
Preparation method of three-dimensional interpenetrating ordered mesoporous graphene spheres
CN105253877A
Cut tobacco additive based on graphene nanocomposite and preparation method and application thereof
CN106690404A
Lamellate graphene / metallic oxide nanocomposite and preparation method thereof
CN108946801A
Preparation method of geraniol-graphene oxide slow-release heat-conducting composite material for cigarettes
CN111743192A
Nanocomposite Multilayer Film Using Janus Layer-by-Layer Assembly and Method of Preparing the Same and Electrode Comprising the Same
KR1020160013725A