Flexible piezoelectric composite stent for simulating cartilage and preparation method of flexible piezoelectric composite stent

By filling chitosan/polyvinyl alcohol fibers in barium titanate-flexible resin piezoelectric scaffolds, flexible piezoelectric composite scaffolds that simulate cartilage, the problems of biomaterial absorption and immune inflammatory response are solved, and the efficient cartilage repair is achieved and safety, promoting chondrocyte proliferation and bone regeneration.

CN118924947AActive Publication Date: 2024-11-12BEIJING INST OF TECH
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411013276.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-11-12
Estimated Expiration
2044-07-26

AI Technical Summary

Technical Problem

The prior art is difficult to quickly absorb biological materials, resulting in insufficient cartilage repair ability and an immune inflammatory response, making it difficult to achieve rapid healing and effective repair.

Method used

The flexible piezoelectric composite scaffold is prepared by using barium titanate-flexible resin piezoelectric scaffolding to fill chitosan/polyvinyl alcohol fibers. It has good biocompatibility, flexible mechanical properties and degradability, and is stimulated by ultrasonic Promote cell proliferation and bone regeneration.

Benefits of technology

The flexible piezoelectric composite scaffold that simulates cartilage has good biocompatibility and flexible mechanical properties under ultrasound action, effectively stimulates osteoblast proliferation, promotes cartilage repair, and promotes bone regeneration through the absorption of natural components and reduces inflammatory response. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118924947A_ABST
    Figure CN118924947A_ABST
Patent Text Reader

Abstract

The invention provides a flexible piezoelectric composite stent for simulating cartilage and a preparation method thereof, and relates to the field of medical materials. The flexible piezoelectric composite stent for simulating cartilage is prepared by filling chitosan / polyvinyl alcohol fibers outside a barium titanate-flexible resin piezoelectric stent. The method for preparing the flexible piezoelectric composite scaffold is simple, the flexible piezoelectric composite scaffold simulating cartilage prepared by the method has good biocompatibility and good flexible mechanical property under the ultrasonic action, and meanwhile, osteoblast proliferation can be effectively stimulated to promote bone regeneration based on the electrical stimulation function of the piezoelectric scaffold.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of medical materials, and in particular to a cartilage-simulating flexible piezoelectric composite bracket and a preparation method thereof. Background Art

[0002] Osteoarthritis has always been one of the diseases that plagues humans, especially as more and more teenagers begin to gradually show problems such as knee degenerative lesions and cartilage damage. There is basically no vascular network in cartilage tissue, so it is difficult for repair cells to move to the damaged area and repair the damaged cartilage tissue. Therefore, once cartilage necrosis occurs, there is usually a serious lack of sufficient blood, nutrients and other substances, resulting in the inability of cartilage to repair itself. Under normal circumstances, damaged cartilage tissue is usually replaced by fibrous hyperplastic tissue, causing a serious decline in function or complete loss of function.

[0003] Commonly used methods for repairing cartilage damage include: conservative treatment, microfracture surgery, autologous chondrocyte implantation, autologous osteochondral transplantation, and biomaterial implantation. However, conservative treatment, microfracture surgery, autologous chondrocyte implantation, and autologous osteochondral transplantation will bring about immune inflammation, so biomaterial implantation is increasingly being used to treat cartilage damage and cartilage loss. How to solve the problem of how to make the biological implant material be absorbed by the cartilage as quickly as possible and improve the cartilage repair ability is the focus of researchers.

[0004] Electrical stimulation has been proven to promote the proliferation of chondrocytes and the synthesis of extracellular matrix molecules, thereby accelerating the healing of cartilage defects. Therefore, it is an effective means to improve cartilage repair to conduct research on cartilage scaffolds that are non-toxic, safe, minimally invasive, have high cartilage induction and angiogenesis capabilities, are degradable, promote cell proliferation, and have self-powered stimulation. Piezoelectric composites are intelligent materials with piezoelectricity and flexible mechanical properties. They have good biocompatibility, mechanical properties, low inflammatory response, etc., are conducive to cell proliferation, and have received high attention in the research of cartilage bone repair scaffolds. Summary of the invention

[0005] In view of this, the present invention provides a flexible piezoelectric composite scaffold for simulating cartilage and a preparation method thereof. The present invention is to fill chitosan / polyvinyl alcohol fiber outside the barium titanate-flexible resin piezoelectric scaffold to form a composite scaffold for simulating cartilage. The schematic diagram of the flexible piezoelectric composite scaffold for simulating cartilage is shown in FIG. Figure 1 As shown, the stent has good biocompatibility, flexible mechanical properties and degradability.

[0006] The present invention is achieved by adopting the following technical solutions:

[0007] A method for preparing a flexible piezoelectric composite scaffold for simulating cartilage comprises the following steps:

[0008] (1) Configure a flexible resin matrix

[0009] The barium titanate and the flexible resin are mixed in a volume ratio of 0.5-1:9-9.5, stirred, and then a curing agent is added. After stirring evenly, the mixture is molded, defoamed, and cured to obtain the flexible resin matrix, i.e., the barium titanate-flexible resin piezoelectric support;

[0010] (2) Preparation of chitosan / polyvinyl alcohol fiber gel prefabricated solution

[0011] The polyvinyl alcohol fiber is dissolved in deionized water, heated and stirred at 75°C-80°C for 25min-30min to obtain a polyvinyl alcohol fiber solution; chitosan is then dissolved in deionized water and stirred to obtain a chitosan solution; finally, the polyvinyl alcohol fiber solution and the chitosan solution are mixed in a volume ratio of 5-7:3-5, and stirred to obtain a chitosan / polyvinyl alcohol fiber gel prefabricated solution;

[0012] (3) Preparation of flexible piezoelectric composite scaffolds simulating cartilage

[0013] First, the chitosan / polyvinyl alcohol fiber gel prefabricated solution and the cross-linking agent are mixed in a mass ratio of 10:0.1-0.3, and stirred for 30 minutes to obtain a gel prefabricated solution / cross-linking agent mixed solution; then, the barium titanate-flexible resin piezoelectric scaffold is immersed in the gel prefabricated solution / cross-linking agent mixed solution, and freeze-dried after standing for 24 hours, and cut to obtain the flexible piezoelectric composite scaffold simulating cartilage.

[0014] Furthermore, the flexible resin is polydimethylsiloxane (PDMS).

[0015] Preferably, the viscosity of the flexible resin is 1500 mpa·s-1800 mpa·s.

[0016] Preferably, the particle diameter of the barium titanate is 200nm-800nm.

[0017] Preferably, the piezoelectric constant of the barium titanate is 100 pC / N-120 pC / N.

[0018] Furthermore, the curing agent is a dimer acid polyamide curing agent, preferably a hydrogenated C18 unsaturated fatty acid dimer acid.

[0019] Preferably, the mass ratio of the curing agent to the flexible resin is 0.01-0.1:1.

[0020] Preferably, the mass fraction of the polyvinyl alcohol fiber in the polyvinyl alcohol fiber solution is 10%-15%.

[0021] Preferably, the mass fraction of chitosan in the chitosan solution is 1%-5%.

[0022] Furthermore, the cross-linking agent is glutaraldehyde.

[0023] Preferably, the freeze-drying process is to cool the temperature from room temperature to -40°C at a cooling rate of 3°C / min and then freeze for 48 hours.

[0024] Another object of the present invention is to provide a flexible piezoelectric composite scaffold for simulating cartilage, which is prepared by the above-mentioned method for preparing the flexible piezoelectric composite scaffold for simulating cartilage.

[0025] Furthermore, the porosity of the cartilage-simulating flexible piezoelectric composite scaffold is 60%-80%, and the fracture strength is 1.94MPa-2.11MPa.

[0026] Furthermore, the ultrasonic intensity of the flexible piezoelectric composite stent simulating cartilage is 0.8W / cm 2 -1.6W / cm 2 , a charge signal is generated under the condition of a duty cycle of 60%-100%.

[0027] Compared with the prior art, the present invention has the following beneficial effects:

[0028] 1. The preparation method of the flexible piezoelectric composite scaffold for simulating cartilage of the present invention is simple, and the prepared flexible piezoelectric composite scaffold for simulating cartilage has good biocompatibility and good flexible mechanical properties under the action of ultrasound.

[0029] 2. The flexible piezoelectric composite scaffold prepared by the present invention not only has mechanical properties close to those of human cartilage, but can also effectively stimulate the proliferation of osteoblasts based on the electrical stimulation function of the piezoelectric scaffold.

[0030] 3. In the process of preparing a flexible piezoelectric composite scaffold that simulates cartilage of the present invention, the prepared gel prefabricated solution is formed by mixing a chitosan solution and a polyvinyl alcohol fiber solution, wherein chitosan and polyvinyl alcohol fiber are both natural osteogenic materials that can be absorbed by the human body, and the polysaccharide mixture can effectively promote bone regeneration and can be absorbed by the human body. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 Schematic diagram of the flexible piezoelectric composite stent for simulating cartilage of the present invention;

[0032] Figure 2 The tensile mechanical properties of the flexible piezoelectric composite bracket prepared in Examples 1-3 are shown in Figure 1, (a) is a bar graph of elongation at break, and (b) is a bar graph of tensile fracture strength;

[0033] Figure 3 This is a schematic diagram of a cell experiment under ultrasound action of the present invention;

[0034] Figure 4The figure is a cell live-death experiment result after the flexible piezoelectric composite scaffold prepared in Example 1-3 was co-cultured with mouse cells for 3 days;

[0035] Figure 5 This is a graph showing the ALP activity detection results after the flexible piezoelectric composite scaffold prepared in Example 1-3 was co-cultured with mouse cells for 7 days. DETAILED DESCRIPTION

[0036] The present invention will be further described below in conjunction with the embodiments.

[0037] Example 1

[0038] A method for preparing a flexible piezoelectric composite scaffold for simulating cartilage comprises the following steps:

[0039] (1) Preparation of flexible resin matrix

[0040] 30.7 g of barium titanate powder was added to 50 g of polydimethylsiloxane (PDMS, density 1.1 g / cm 3 , volume 45.45ml), stirring, mixing evenly, adding 2.5g hydrogenated C18 unsaturated fatty acid dimer acid, and then quickly stirring and mixing evenly, pouring into the bracket mold, and then putting the bracket mold into a defoaming machine for defoaming and curing for 24h to obtain a flexible resin matrix, i.e., barium titanate-polydimethylsiloxane piezoelectric bracket;

[0041] (2) Preparation of chitosan / polyvinyl alcohol fiber gel prefabricated solution

[0042] First, 10 g of polyvinyl alcohol fiber was dissolved in 90 g of deionized water, and heated and stirred at 80° C. for 30 min to obtain a polyvinyl alcohol fiber solution; then, 2 g of chitosan was dissolved in 8 g of deionized water, and stirred to obtain a chitosan solution; then, the polyvinyl alcohol fiber solution and the chitosan solution were mixed in a volume ratio of 5:5, and stirred evenly to obtain a chitosan / polyvinyl alcohol fiber gel prefabricated solution;

[0043] (3) Preparation of flexible piezoelectric composite scaffolds simulating cartilage

[0044] First, weigh 30g of chitosan / polyvinyl alcohol fiber gel prefabricated solution, add 0.9g of glutaraldehyde, and stir for 30 minutes to obtain a gel prefabricated solution / cross-linking agent mixed solution; then soak the barium titanate-polydimethylsiloxane piezoelectric scaffold in the gel prefabricated solution / cross-linking agent mixed solution, put it into a freeze-drying treatment box after 24 hours, cool it from room temperature to -40℃ at a cooling rate of 3℃ / min, and then freeze it for 48 hours; then cut off the excess gel at the edge of the barium titanate-polydimethylsiloxane piezoelectric scaffold to obtain a flexible piezoelectric composite scaffold that simulates cartilage.

[0045] Example 2

[0046] A method for preparing a flexible piezoelectric composite scaffold for simulating cartilage comprises the following steps:

[0047] (1) Configure a flexible resin matrix

[0048] 30.7 g of barium titanate powder was added to 50 g of polydimethylsiloxane (PDMS, density 1.1 g / cm 3 , volume 45.45ml), stirring, mixing evenly, adding 2.5g hydrogenated C18 unsaturated fatty acid dimer acid, and then quickly stirring and mixing evenly, pouring into the bracket mold, and then putting the bracket mold into a defoaming machine for defoaming and curing for 24h to obtain a flexible resin matrix, i.e., barium titanate-polydimethylsiloxane piezoelectric bracket;

[0049] (2) Preparation of chitosan / polyvinyl alcohol fiber gel prefabricated solution

[0050] First, 10 g of polyvinyl alcohol fiber was dissolved in 90 g of deionized water, heated and stirred at 80° C. for 30 min to obtain a polyvinyl alcohol fiber solution; then 2 g of chitosan was dissolved in 8 g of deionized water and stirred to obtain a chitosan solution; then the polyvinyl alcohol fiber solution and the chitosan solution were mixed in a volume ratio of 6:4, and stirred evenly to obtain a chitosan / polyvinyl alcohol fiber gel prefabricated solution;

[0051] (3) Preparation of flexible piezoelectric composite scaffolds simulating cartilage

[0052] First, weigh 30g of chitosan / polyvinyl alcohol fiber gel prefabricated solution, add 0.9g of glutaraldehyde, and stir for 30 minutes to obtain a gel prefabricated solution / cross-linking agent mixed solution; then soak the barium titanate-polydimethylsiloxane piezoelectric scaffold in the gel prefabricated solution / cross-linking agent mixed solution, put it into a freeze-drying treatment box after 24 hours, cool it from room temperature to -40℃ at a cooling rate of 3℃ / min, and then freeze it for 48 hours; then cut off the excess gel at the edge of the barium titanate-polydimethylsiloxane piezoelectric scaffold to obtain a flexible piezoelectric composite scaffold that simulates cartilage.

[0053] Example 3

[0054] A method for preparing a flexible piezoelectric composite scaffold for simulating cartilage comprises the following steps:

[0055] (1) Configure a flexible resin matrix

[0056] 30.7 g of barium titanate powder was added to 50 g of polydimethylsiloxane (PDMS, density 1.1 g / cm 3 , volume 45.45ml), stirring, mixing evenly, adding 2.5g hydrogenated C18 unsaturated fatty acid dimer acid, and then quickly stirring and mixing evenly, pouring into the bracket mold, and then putting the bracket mold into a defoaming machine for defoaming and curing for 24h to obtain a flexible resin matrix, i.e., barium titanate-polydimethylsiloxane piezoelectric bracket;

[0057] (2) Preparation of chitosan / polyvinyl alcohol fiber gel prefabricated solution

[0058] First, 10 g of polyvinyl alcohol fiber was dissolved in 90 g of deionized water, and heated and stirred at 80° C. for 30 min to obtain a polyvinyl alcohol fiber solution; then, 2 g of chitosan was dissolved in 8 g of deionized water, and stirred to obtain a chitosan solution; then, the polyvinyl alcohol fiber solution and the chitosan solution were mixed in a volume ratio of 7:3, and stirred evenly to obtain a chitosan / polyvinyl alcohol fiber gel prefabricated solution;

[0059] (3) Preparation of flexible piezoelectric composite scaffolds simulating cartilage

[0060] First, weigh 30g of chitosan / polyvinyl alcohol fiber gel prefabricated solution, add 0.9g of glutaraldehyde, and stir for 30 minutes to obtain a gel prefabricated solution / cross-linking agent mixed solution; then soak the barium titanate-polydimethylsiloxane piezoelectric scaffold in the gel prefabricated solution / cross-linking agent mixed solution, put it into a freeze-drying treatment box after 24 hours, cool it from room temperature to -40℃ at a cooling rate of 3℃ / min, and then freeze it for 48 hours; then cut off the excess gel at the edge of the barium titanate-polydimethylsiloxane piezoelectric scaffold to obtain a flexible piezoelectric composite scaffold that simulates cartilage.

[0061] Figure 2 The tensile mechanical properties of the flexible piezoelectric composite bracket prepared in Example 1-3 are shown in FIG. Figure 2 (b) The tensile fracture strength bar chart shows that the tensile fracture strengths of the flexible piezoelectric composite brackets prepared in Example 1, Example 2, and Example 3 are 2.11 MPa, 2.01 MPa, and 1.94 MPa, respectively. The difference is not obvious, but according to Figure 2 (a) From the elongation at break bar graph, it can be seen that the elongation at break corresponding to Example 1, Example 2 and Example 3 are 74%, 67% and 49% respectively. It can be seen that as the volume ratio of the polyvinyl alcohol fiber solution and the chitosan solution decreases, the tensile strength of the scaffold does not decrease much, but the elongation at break has a significant difference.

[0062] The schematic diagram of the cell experiment under ultrasound of the present invention is as follows Figure 3 Reference Figure 3 The cell live / death experiment and alkaline phosphatase (ALP) activity detection experiment were carried out using the flexible piezoelectric composite scaffolds prepared in Examples 1-3 to verify the biological cell compatibility and osteogenic performance of each bone scaffold (mouse MC3T3-E1 cells were used to carry out cell live / death experiment and alkaline phosphatase (ALP) activity detection).

[0063] The results of the cell live-death experiment after culturing the flexible piezoelectric composite scaffold prepared in Example 1-3 with mouse cells for 3 days are shown in FIG. Figure 4The ALP activity detection result after 7 days of co-culture of the flexible piezoelectric composite scaffold prepared in Example 1-3 and mouse cells is shown in FIG. Figure 5 As shown. Among them, the cell live / dead experimental detection method is to use mouse osteoblasts (MC3T3-E1, national identification cell culture system, China) as experimental materials, co-culture with the flexible piezoelectric composite scaffold prepared in Example 1-3, and after 72 hours, the dye is prepared by Calcein / PI cell live / dead kit, the scaffold after co-culture is treated, and then the live / dead ratio of cells on the scaffold is counted by software; the alkaline phosphatase (ALP) quantitative analysis experimental method is to use mouse osteoblasts (MC3T3-E1, national identification cell culture system, China) as experimental materials, co-culture with a blank scaffold-free group and the flexible piezoelectric composite scaffold prepared in Example 1-3, and apply ultrasonic waves with an intensity of 0.8W / cm every day. 2 -1.6W / cm 2 , ultrasound with a duty cycle of 60%-100% for 1 min. After 7 days, the protein expression on the scaffold was monitored by an alkaline phosphatase (ALP) detection kit to obtain the ALP activity test results, such as Figure 5 shown.

[0064] Depend on Figure 4 It can be seen that the cell survival rates of the flexible piezoelectric composite scaffolds prepared by Example 1, Example 2 and Example 3 are all greater than 89%, proving that the flexible piezoelectric composite scaffold has good cell compatibility. Figure 5 Compared with the blank control group, the ALP activity of the flexible piezoelectric composite scaffold prepared in Example 1-3 under ultrasound was significantly improved, proving that the scaffold has a good osteogenic effect.

[0065] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing a flexible piezoelectric composite scaffold simulating cartilage, characterized in that: The following steps are involved: (1) Preparation of flexible resin matrix The barium titanate and the flexible resin are mixed in a volume ratio of 0.5-1:9-9.5, stirred, and then a curing agent is added. After stirring evenly, the mixture is molded, defoamed, and cured to obtain the flexible resin matrix, i.e., the barium titanate-flexible resin piezoelectric support; (2) Preparation of chitosan / polyvinyl alcohol fiber gel prefabricated solution The polyvinyl alcohol fiber is dissolved in deionized water, heated and stirred at 75°C-80°C for 25min-30min to obtain a polyvinyl alcohol fiber solution; chitosan is then dissolved in deionized water and stirred to obtain a chitosan solution; the polyvinyl alcohol fiber solution and the chitosan solution are then mixed in a volume ratio of 5-7:3-5, and stirred to obtain a chitosan / polyvinyl alcohol fiber gel prefabricated solution; (3) Preparation of flexible piezoelectric composite scaffolds simulating cartilage First, the chitosan / polyvinyl alcohol fiber gel prefabricated solution and the cross-linking agent are mixed in a mass ratio of 10:0.1-0.3, and stirred for 30 minutes to obtain a gel prefabricated solution / cross-linking agent mixed solution; then, the barium titanate-flexible resin piezoelectric scaffold is immersed in the gel prefabricated solution / cross-linking agent mixed solution, and freeze-dried after standing for 24 hours, and cut to obtain the flexible piezoelectric composite scaffold simulating cartilage.

2. The method for preparing the flexible piezoelectric composite scaffold for simulating cartilage according to claim 1, characterized in that: The flexible resin is polydimethylsiloxane.

3. The method for preparing the flexible piezoelectric composite scaffold for simulating cartilage according to claim 1, characterized in that: The viscosity of the flexible resin is 1500 mpa·s-1800 mpa·s.

4. The method for preparing the flexible piezoelectric composite scaffold for simulating cartilage according to claim 1, characterized in that: The particle diameter of the barium titanate is 200nm-800nm, and the piezoelectric constant is 100pC / N-120pC / N.

5. The method for preparing the flexible piezoelectric composite scaffold for simulating cartilage according to claim 1, characterized in that: The curing agent is a dimer acid polyamide curing agent.

6. The method for preparing the flexible piezoelectric composite scaffold for simulating cartilage according to claim 1, characterized in that: The mass ratio of the curing agent to the flexible resin is 0.01-0.1:

1.

7. The method for preparing the flexible piezoelectric composite scaffold for simulating cartilage according to claim 1, characterized in that: The mass fraction of the polyvinyl alcohol fiber in the polyvinyl alcohol fiber solution is 10%-15%; the mass fraction of chitosan in the chitosan solution is 1%-5%.

8. The method for preparing the flexible piezoelectric composite scaffold for simulating cartilage according to claim 1, characterized in that: The cross-linking agent is glutaraldehyde.

9. The method for preparing the flexible piezoelectric composite scaffold for simulating cartilage according to claim 1, characterized in that: The freeze-drying process is to cool the temperature from room temperature to -40°C at a cooling rate of 3°C / min and then freeze for 48 hours.

10. A flexible piezoelectric composite stent simulating cartilage, characterized in that: The flexible piezoelectric composite scaffold for simulating cartilage is prepared by the preparation method of any one of claims 1 to 9; the flexible piezoelectric composite scaffold for simulating cartilage has a porosity of 60%-80%, a fracture strength of 1.94MPa-2.11MPa, and an ultrasonic intensity of 0.8W / cm 2 -1.6W / cm 2 , a charge signal is generated under the condition of a duty cycle of 60%-100%.

Citation Information

Patent Citations

  • Preparation method of cartilage repair scaffold material

    CN103690991A

  • Piezoelectric ceramic ultra-high filling silicone rubber composite ink material for ink direct writing printing and preparation method and application of piezoelectric ceramic ultra-high filling silicone rubber composite ink material

    CN113621238A

  • Bone tissue engineering scaffold 3D printing material with piezoelectric property

    CN113968731A

  • Hydrogel coated scaffold

    US20150250923A1