Modified adsorption material as well as preparation method and application thereof

Through gas-phase grafting modification technology, the functional groups and photothermal effects of the adsorbent materials are increased, and the problem of insufficient adsorption performance of adsorbent materials in light-free environments is solved, and efficient metal ion adsorption in light-free and light-free environments is achieved, which significantly improves the Adsorption capacity and affinity.

CN118925686APending Publication Date: 2024-11-12SHANGHAI UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411130359.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

There are bottlenecks in the efficiency of adsorption of metal ions in existing adsorption materials, especially in light-free environments, which are difficult to significantly improve adsorption performance.

Method used

Through one-step gas-phase grafting modification technology, multifunctional groups and photothermal effects are introduced to form modified adsorption materials, so that they can significantly improve adsorption performance in both light and light environments. The specific steps include soaking the adsorbed substrate in a redox polymerization initiator solution, performing gas-phase redox graft polymerization, forming a graft layer, and increasing the functional groups and photothermal conversion ability of the adsorbed substrate.

Benefits of technology

It realizes efficient adsorption of metal ions in light-free and light-free environments, improves the adsorption capacity and affinity of adsorbent materials, and reduces production and environmental treatment costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118925686A_ABST
    Figure CN118925686A_ABST
Patent Text Reader

Abstract

The invention relates to a modified adsorption material and a preparation method and application thereof.The preparation method comprises the following preparation steps that S1, an adsorption base material is soaked in an initiator solution, and the initiator solution is subjected to redox polymerization in advance for subsequent gas-phase redox graft polymerization; and S2, contacting the adsorption base material treated in the step S1 with a grafting monomer to perform gas-phase redox graft polymerization, and forming a grafting layer on the adsorption base material to obtain the modified adsorption material. Compared with the prior art, the modified adsorption material prepared by the invention can further improve the adsorption performance of an adsorption base material in a dark environment, and can further improve the adsorption performance of the adsorption base material by utilizing a photothermal effect endowed by modification in an illumination environment, so that the synergistic effect of the grafted functional monomer is fully exerted, and high adsorption capacity is realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer materials, and in particular to a modified adsorption material and a preparation method and application thereof. Background Art

[0002] The functional groups in the adsorbent material and the temperature of the solid-liquid interface of the adsorbent material are two key factors affecting the metal ion adsorption efficiency. According to the law of material action (Formula 1) and the Arrhenius formula (Formula 2):

[0003] ν=k × C M m ×C N n (1)

[0004]

[0005] Where ν represents the reaction rate, k is the reaction rate constant at temperature T, C M and C N are the initial concentrations of substrates M and N, respectively, m and n are the chemical equilibrium coefficients of substrates M and N, A is the Arrhenius constant, e is the base of the natural logarithm, Ea (unit: J / mol) is the experimental activation energy, which can be regarded as a constant independent of temperature, R (unit: J / mol / K) is the molar gas constant, and T (K) is the absolute temperature during the reaction.

[0006] Therefore, the increase in metal ion concentration or the increase in ambient temperature can enhance the chemical coordination between metal ions and the functional groups of the adsorbent material. Therefore, for solutions with specific metal ion concentrations, increasing the temperature of the adsorption microenvironment, or rationally designing the adsorbent material such as using additional functional groups to cooperate, can significantly improve the adsorption performance of the adsorbent material for metal ions. For example, the amidoxime-based uranium extraction photothermal water gel prepared by combining polydopamine with amidoxime-based hydrogel; the photothermal uranium extraction hydrogel that simulates plant transpiration by photothermal means; and the photothermal uranium extraction adsorbent material combined with MXene and amidoxime-based fibers; these materials increase the temperature of the adsorption microenvironment under light drive, and all show excellent adsorption performance for uranyl ions.

[0007] The present invention is to further enhance the adsorption performance of the adsorption material to break through the bottleneck of the adsorption performance of the adsorption material. Through one-step grafting modification, the adsorption synergy of multiple functional groups and the enhancement of the material adsorption performance under the photothermal effect are simultaneously achieved. Summary of the invention

[0008] The purpose of the present invention is to provide a modified adsorbent material and its preparation method and application in order to improve the adsorption performance of the adsorbent material. On the basis that the original adsorbent material has a certain adsorption capacity, the adsorption performance of the adsorbent material is further enhanced through gas phase grafting modification in a lightless and light environment through the synergy of functional groups and photothermal effect.

[0009] The purpose of the present invention can be achieved by the following technical solutions:

[0010] One of the technical solutions of the present invention is to provide a method for preparing a modified adsorbent material, comprising the following steps:

[0011] S1, soaking the adsorption substrate in an initiator solution, pre-adsorbing the redox polymerization initiator solution for subsequent gas-phase redox graft polymerization;

[0012] S2. The adsorption substrate obtained by the treatment in step S1 is contacted with a grafting monomer to carry out gas phase redox grafting polymerization to form a grafting layer on the adsorption substrate to obtain a modified adsorption material.

[0013] In some specific embodiments, in step S1, the adsorption substrate is selected from any one of cotton cloth, non-woven fabric, fiber or film containing adsorption functional groups.

[0014] In some specific embodiments, the adsorption functional group includes any one or more of a carboxyl group, a hydroxyl group, an amino group, and an amidoxime group.

[0015] In some specific embodiments, in step S1, the initiator solution includes an initiator and a solvent, wherein the initiator is selected from any one of ammonium cerium nitrate, ammonium persulfate, potassium persulfate or sodium persulfate; and the solvent is selected from any one of hydrochloric acid solution, nitric acid solution or sulfuric acid solution.

[0016] In some specific embodiments, in step S1, the final concentration of the initiator in the initiator solution is 1-10 wt %, and the acid concentration of the solvent in the initiator solution is 0.01%-1%.

[0017] In some specific embodiments, in step S1, the temperature of the adsorption redox polymerization initiator solution is 0-45° C. and the time is 10-15 min.

[0018] In some specific embodiments, in step S2, the grafting monomer is selected from aniline or pyrrole, and the concentration of the grafting monomer in the grafting monomer aqueous solution is 50%-100%.

[0019] In some specific embodiments, in step S2, the gas phase redox graft polymerization is carried out by contacting the adsorption substrate obtained by the treatment in step S1 with the vapor of the grafting monomer to carry out graft polymerization.

[0020] In some specific embodiments, in step S2, the temperature of the graft polymerization is 0-50°C; and the time of the graft polymerization is 1-60 min.

[0021] In some specific embodiments, washing is further performed after graft polymerization to remove excess initiator solution, and the washing solution used is selected from any one of hydrochloric acid solution, sulfuric acid solution or nitric acid solution, and the final concentration of the acid in the washing solution is 0.01-0.5M.

[0022] In some embodiments, the washing time is 1-5 hours.

[0023] The second technical solution of the present invention is to provide a modified adsorption material, which is obtained based on the preparation method described in one of the above technical solutions.

[0024] The third technical solution of the present invention is to provide an application of the modified adsorption material as described in the second technical solution above, wherein the modified adsorption material is used to adsorb metal ions in the presence or absence of light.

[0025] In some specific embodiments, the modified adsorption material can be used for the adsorption, extraction and treatment of metal ions such as seawater, salt lake brine, low- and medium-level radioactive wastewater, and other industrial water bodies containing metal ions.

[0026] In some embodiments, the metal ions include uranium, iron, zinc, molybdenum, lead, magnesium, or copper ions.

[0027] The present invention improves the adsorption performance of the adsorbent material for metal ions by gas phase grafting modification. In the adsorption substrate, functional groups such as carboxyl, hydroxyl, amino and amidoxime groups show significant adsorption capacity for metal ions because the oxygen, nitrogen and sulfur atoms therein can provide lone pairs of electrons, and are considered to be effective chelating functional groups for capturing metal ions. The present invention combines the adsorbent material with these functional groups to synergistically enhance the adsorption performance of the adsorbent material for metal ions.

[0028] Introducing additional functional groups into the adsorption substrate containing chelating functional ligands enables the functional groups to exert photothermal conversion performance under light conditions, increase the temperature of the interface microenvironment of the modified adsorbent material under sunlight, and promote the adsorption and extraction of target metal ions by the modified adsorbent material. Under light-free conditions, the functional groups have oxygen, nitrogen, and sulfur atoms that provide lone pairs of electrons, so that the lone pairs of electrons coordinate with metal ions and play a role in active synergistic adsorption, ultimately enabling the modified adsorbent material to effectively enhance its adsorption performance in both light and dark environments.

[0029] During the preparation process, the present invention modifies the adsorption substrate by subjecting it to gas-phase redox graft polymerization, and the prepared modified adsorption material can achieve improved adsorption performance in both lightless and light environments. Among them, in a lightless environment, the grafted layer modified by gas-phase graft polymerization technology has an adsorption functional group, and the nitrogen atom on the group can provide a lone pair of electrons to coordinate with the metal ions. In a light environment, since the grafted layer also has excellent photothermal conversion capabilities, the use of solar energy to drive the change of the material interface microenvironment temperature under illumination conditions can once again improve the adsorption performance of the material. The present invention gives full play to the synergistic effect of the grafted functional monomers, improves the affinity of the modified adsorption material for metal ions in the solution, and improves the adsorption performance of the modified adsorption material.

[0030] Compared with the prior art, the present invention has the following beneficial effects:

[0031] (1) The present invention adopts gas phase grafting polymerization technology to directly contact the adsorption substrate with the vapor of the grafting monomer to carry out the grafting polymerization reaction. The internal microphase of the grafting-modified adsorption substrate is separated into smaller polymer particles and a slit nanopore structure is constructed, thereby improving the utilization rate of the grafting monomer. In addition, the unevaporated grafting monomer and the evaporated but unreacted grafting monomer can be condensed and recovered, thereby reducing the production cost and environmental treatment cost.

[0032] (2) The modified adsorption material prepared by the present invention can further improve the adsorption performance of the adsorption substrate in a lightless environment, and utilize the photothermal effect imparted by the modification in a light environment to further improve the adsorption performance of the adsorption substrate by solar-driven interface evaporation, thereby giving full play to the synergistic effect of the grafted functional monomers to achieve a high adsorption capacity.

[0033] (3) The modified adsorption material prepared by the present invention can not only expose the chelating sites to the maximum extent, but also modify the obtained nanoparticles and slit nanopores, thereby greatly improving the affinity of the adsorption substrate for metal ions. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 Scanning electron micrographs of the surface (a) and cross-section (b) of the modified adsorbent material in Example 1 of the present invention.

[0035] Figure 2 This is a photothermal infrared image of the modified adsorption material in Example 2 of the present invention.

[0036] Figure 3 This is a surface scanning electron microscope image of the modified adsorption material in Example 3 of the present invention.

[0037] Figure 4 This is a surface scanning electron micrograph of the modified adsorbent material in Example 4 of the present invention.

[0038] Figure 5 This is a surface scanning electron micrograph of the modified adsorbent material in Example 5 of the present invention. DETAILED DESCRIPTION

[0039] The present invention is described in detail below in conjunction with the accompanying drawings and specific embodiments. This embodiment is implemented based on the technical solution of the present invention, and provides a detailed implementation method and specific operation process, but the protection scope of the present invention is not limited to the following embodiments.

[0040] In the following embodiments and test examples, unless otherwise specified, raw materials or processing techniques are conventional commercially available raw materials or conventional processing techniques in the art.

[0041] Embodiment 1:

[0042] (1) Dissolve ammonium cerium nitrate (final concentration: 1 wt%) in 0.01% nitric acid to obtain an initiator solution.

[0043] (2) Take 0.2 g of polyvinyl alcohol fiber containing carboxyl and hydroxyl adsorption functional groups and soak it in the above initiator solution. The temperature of the initiator solution is 0° C. and soak for 10 minutes.

[0044] Among them, polyvinyl alcohol fibers containing carboxyl and hydroxyl adsorption functional groups are obtained by radiation-induced graft polymerization technology. Mainly, 1g of water-resistant polyvinyl alcohol fibers containing hydroxyl groups purchased from Kuraray Co., Ltd. are immersed in 20mL of an aqueous solution with a concentration of 20wt% of acrylic acid. Secondly, they are sealed in an electron beam with an absorbed dose of 100kGy to induce radiation polymerization of acrylic acid on the polyvinyl alcohol fibers. After the grafting is completed, the material is placed in N,N-dimethylformamide to clean the excess homopolymer. After the completion, the excess solvent on the surface of the material is cleaned with deionized water and then dried at 60°C. The polyacrylic acid grafting rate is calculated to be 110% by the mass difference before and after grafting, and the density of carboxyl groups on the material is 7.5mmol / g.

[0045] (3) The polyvinyl alcohol fiber treated in step (2) is placed in a chamber filled with aniline vapor, the concentration of aniline is 100%, and the grafting reaction is carried out at 0°C for 1 minute.

[0046] (4) After the grafting is completed, the excess initiator solution on the material is cleaned with 0.01M hydrochloric acid for 1 hour, and then the material is washed with deionized water until it is neutral to obtain a modified adsorption material.

[0047] like Figure 1 As shown, the average diameter of the modified adsorption material is 600 nm, the interior is filled with particle structures with a diameter of 1 nm, and the internal pore diameter is 0.1 nm.

[0048] Embodiment 2:

[0049] (1) Dissolve ammonium persulfate (final concentration: 10 wt%) in 1% hydrochloric acid to obtain an initiator solution.

[0050] (2) Take 0.2 g of cotton cloth containing amidoxime adsorption functional groups and soak it in the above initiator solution at a temperature of 45° C. for 10 min.

[0051] Among them, the cotton cloth containing amidoxime adsorption functional groups is prepared by directly reacting cotton cloth containing 30wt% cyanide groups with amidoxime. Specifically, 1g of cotton cloth containing cyanide groups is immersed in a 10wt% neutral hydroxylamine hydrochloride aqueous solution, reacted at 70°C for 24 hours, taken out, and the excess reaction solution is washed with deionized water and then dried at 60°C to prepare cotton cloth containing amidoxime adsorption functional groups with an amidoxime group density of 5mmol / g.

[0052] (3) The cotton cloth treated in step (2) is placed in a chamber filled with pyrrole vapor, where the pyrrole vapor comes from an aqueous solution containing 50% pyrrole, and the grafting reaction is carried out at 50° C. for 60 minutes.

[0053] (4) After the grafting is completed, the excess initiator on the material is cleaned with 0.5M sulfuric acid for 5 hours, and then the material is washed with deionized water until it is neutral to obtain a modified adsorption material.

[0054] like Figure 2 As shown, under light conditions, the modified adsorbent material has obvious heat generation in water, indicating that the modified adsorbent material has excellent photothermal properties.

[0055] Embodiment 3:

[0056] (1) Potassium persulfate (final concentration: 5 wt%) was dissolved in 0.5% sulfuric acid to obtain an initiator solution.

[0057] (2) Take 0.2 g of the non-woven fabric containing amino adsorption functional groups and soak it in the above initiator solution. The temperature of the initiator solution is 25° C. and soak for 10 minutes.

[0058] The non-woven fabric containing amino adsorption functional groups is prepared by the following process: 1g of non-woven fabric is placed in a polyethylene bag and vacuum sealed, and irradiated with an electron beam with an absorption dose of 30kGy. After completion, the non-woven fabric is placed in an aqueous solution containing 5wt% 4-hydroxybutyl acrylate glycidyl ether and 0.5wt% Span-20, and reacted in a water bath at 40°C for 2h. After completion, the non-woven fabric is taken out and washed with methanol to remove excess solvent and homopolymer on the surface, and then deionized and washed and dried at 60°C to obtain a non-woven fabric with a 4-hydroxybutyl acrylate glycidyl ether grafting rate of 150wt%. Then, it is immersed in a 70wt% ethylenediamine isopropanol solution, reacted at 60°C for 4h, and then taken out and washed with deionized water to remove excess solvent on the surface, and dried at 60°C to obtain a non-woven fabric with an amino content of 4.0mmol / g.

[0059] (3) The nonwoven fabric treated in step (2) is placed in a chamber filled with pyrrole vapor, where the pyrrole vapor comes from an aqueous solution containing 75% pyrrole, and the grafting reaction is carried out at 25° C. for 30 minutes.

[0060] (4) After the grafting is completed, the excess initiator on the material is cleaned with 0.2 M nitric acid for 4 h, and then the material is washed with deionized water until it is neutral to obtain a modified adsorption material.

[0061] like Figure 3 As shown, the average diameter of the modified adsorption material is 200 μm, the interior is filled with particle structures with a diameter of 2 nm, and the internal pore diameter is 0.5 nm.

[0062] Embodiment 4:

[0063] (1) Sodium persulfate (final concentration: 2 wt%) was dissolved in 0.1% nitric acid to obtain an initiator solution.

[0064] (2) Take 0.2 g of the film containing amidoxime and carboxyl adsorption functional groups and immerse it in the above initiator solution at a temperature of 25° C. for 10 min.

[0065] The film containing amidoxime and carboxyl adsorption functional groups is prepared by the following process: 1 g of the film is placed in 20 mL of an aqueous solution containing 20 wt% acrylonitrile and 20 wt% acrylic acid, and then sealed and irradiated with an electron beam with an absorbed dose of 100 kGy, and acrylonitrile and acrylic acid are grafted on the film surface by radiation-induced graft polymerization technology, and then the excess solvent and homopolymer on the surface are washed with deionized water, and after drying at 60° C., the grafting rate of polyacrylonitrile and polyacrylic acid is calculated to be 150 wt% by mass difference. Then, the material is subjected to the amidoxime reaction in step (2) of Example 2 to convert the grafted polyacrylonitrile into amidoxime.

[0066] (3) The film treated in step (2) is placed in a chamber filled with aniline vapor, where the aniline vapor comes from an aqueous solution containing 98% aniline, and the grafting reaction is carried out at 30° C. for 10 minutes.

[0067] (4) After the grafting is completed, the excess initiator on the material is cleaned with 0.1 M nitric acid for 3 h, and then the material is washed with deionized water until it is neutral to obtain a modified adsorption material.

[0068] like Figure 4 As shown, the average diameter of the modified adsorbent material is 1 μm, the interior is filled with particle structures with a diameter of 1 nm, and the internal pore diameter is 0.5 nm.

[0069] Embodiment 5:

[0070] (1) Dissolve ammonium cerium nitrate (final concentration: 2 wt%) in 0.1% hydrochloric acid to obtain an initiator solution.

[0071] (2) 0.2 g of ethylene vinyl alcohol copolymer fiber felt containing amidoxime and hydroxyl adsorption functional groups was soaked in the above initiator solution at a temperature of 20° C. for 10 min.

[0072] The ethylene vinyl alcohol copolymer fiber felt containing amidoxime groups and hydroxyl adsorption functional groups is prepared by the following process: 1g of ethylene vinyl alcohol copolymer containing hydroxyl groups is dissolved in N,N-dimethylformamide, and the mixture is uniformly dissolved by magnetic stirring at 80°C and then electrostatically spun into ethylene vinyl alcohol copolymer fiber felt. Then, 1g of ethylene vinyl alcohol copolymer fiber felt is placed in 20mL of an aqueous solution containing 40wt% acrylonitrile and sealed, and then irradiated with an electron beam with an absorbed dose of 100kGy. Acrylonitrile is grafted onto the fiber felt by radiation-induced graft polymerization technology. After completion, the excess solvent and homopolymer on the surface are washed with deionized water, and the grafting rate of polyacrylonitrile is calculated to be 95wt% by mass difference after drying at 60°C. Then, the material is subjected to the amidoxime reaction in step (2) of Example 2 to convert the grafted polyacrylonitrile into amidoxime groups, and the amidoxime content on the material is calculated to be 6.3mmol / g.

[0073] (3) placing the ethylene vinyl alcohol copolymer fiber felt treated in step (2) above in a chamber filled with aniline vapor, the aniline vapor being derived from an aqueous solution containing 88% aniline, and performing a grafting reaction at 30° C. for 20 minutes.

[0074] (4) After the grafting is completed, the excess initiator on the material is cleaned with 0.1 M nitric acid for 4 h, and then the material is washed with deionized water until it is neutral to obtain a modified adsorption material.

[0075] like Figure 5As shown, the average diameter of the modified adsorption material is 25 μm, the interior is filled with particle structures with a diameter of 3 nm, and the internal pore diameter is 1 nm.

[0076] The modified adsorption materials prepared in the above Examples 1-5 were subjected to the following performance tests:

[0077] Test Example 1:

[0078] Using the adsorption substrate as a control, the modified adsorption material and the adsorption substrate were respectively put into 1000L seawater in a pumping circulation mode to adsorb uranium ions under light and dark conditions. The uranium concentration in seawater was 3.3ppb, and the main form of uranium in seawater was uranyl ion UO2 2+ The input material mass was 0.2 g, and the adsorption was carried out at 100 rpm for 24 h at room temperature. The adsorption capacity was calculated and the results are shown in Table 1.

[0079] Table 1 Modified adsorption materials in dark and light (1sun, 1kw / m 2 ) Adsorption capacity of uranium in seawater (mg / g)

[0080]

[0081]

[0082] Test Example 2:

[0083] Taking the adsorption substrate as a control, the modified adsorption material and the adsorption substrate were put into 1L salt lake brine under light and lightless conditions to adsorb iron ions. The iron concentration in the salt lake brine was 5ppm, and the main form of iron in the salt lake brine was Fe(OH) + or Fe(OH)2 + The input material mass was 0.2 g, and the adsorption was carried out at 100 rpm for 24 h at room temperature. The adsorption capacity was calculated and the results are shown in Table 2.

[0084] Table 2 Adsorption capacity of modified adsorbent materials for iron ions in salt lake brine under lightless and light conditions (mg / g)

[0085]

[0086] Test Example 3:

[0087] Taking the adsorption substrate as a control, the modified adsorption material and the adsorption substrate were put into 100L of low- and medium-level wastewater under light and dark conditions for molybdenum ion adsorption. The molybdenum concentration in the low- and medium-level wastewater was 10ppm, and the main form of molybdenum in the low- and medium-level wastewater was MoO4. 2-The input material mass was 0.2 g, and the adsorption was carried out at 100 rpm at room temperature for 24 h. The adsorption capacity was calculated and the results are shown in Table 3.

[0088] Table 3 Adsorption capacity of modified adsorbent materials for molybdenum ions in low- and medium-level wastewater under lightless and light conditions (mg / g)

[0089]

[0090] Test Example 4:

[0091] Taking the adsorption substrate as a control, the modified adsorption material and the adsorption substrate were put into 2L of industrial wastewater under light and dark conditions for copper ion adsorption. The copper concentration in the industrial wastewater was 7ppm, and the main form of copper in the industrial wastewater was [Cu(NH3)4] 2+ The input material mass was 0.2 g, and the adsorption was carried out at 100 rpm for 24 h at room temperature. The adsorption capacity was calculated and the results are shown in Table 4.

[0092] Table 4 Adsorption capacity of modified adsorbent materials for copper ions in industrial wastewater under lightless and light conditions (mg / g)

[0093]

[0094] Test Example 5:

[0095] Using the unmodified adsorbent material as a control, the modified adsorbent material and the adsorbent substrate were placed in 500 mL of industrial wastewater under light and dark conditions for zinc ion adsorption. The zinc concentration in the industrial wastewater was 77 ppm, and the main form of zinc in the industrial wastewater was [Zn(NH3)4] 2+ The input material mass was 0.2 g, and the adsorption was carried out at 100 rpm for 24 h at room temperature. The adsorption capacity was calculated and the results are shown in Table 5.

[0096] Table 5 Adsorption capacity of modified adsorbent materials for zinc ions in industrial wastewater under lightless and light conditions (mg / g)

[0097]

[0098] Test Example 6:

[0099] Using the unmodified adsorbent material as a control, the modified adsorbent material and the adsorbent substrate were placed in 5L of industrial wastewater under light and dark conditions for lead ion adsorption. The lead concentration in the industrial wastewater was 0.5ppm, and the main form of lead in the industrial wastewater was PbCl4. 2- The input material mass was 0.2 g, and the adsorption was carried out at 100 rpm for 24 h at room temperature. The adsorption capacity was calculated and the results are shown in Table 6.

[0100] Table 6 Adsorption capacity of modified adsorbent materials for lead ions in industrial wastewater under lightless and light conditions (mg / g)

[0101]

[0102] Test Example 7:

[0103] Taking the adsorption substrate as a control, the modified adsorption material and the adsorption substrate were respectively put into 3L of industrial wastewater for magnesium ion adsorption under light and dark conditions, wherein the magnesium concentration in the industrial wastewater was 1ppm, and the main form of magnesium in the industrial wastewater was Mg(OH)2. The input material mass was 0.2g, and the adsorption was carried out at 100rpm for 24h at room temperature. The adsorption capacity was calculated, and the results are shown in Table 7.

[0104] Table 7 Adsorption capacity of modified adsorbent materials for magnesium ions in industrial wastewater under lightless and light conditions (mg / g)

[0105]

[0106] In summary, the modified adsorption material prepared by the present invention can more effectively adsorb metal ions in both light and dark environments, and has at least 20% improvement in adsorption performance compared to the adsorption substrate.

[0107] The above description of the embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the scope of protection of the present invention.

Claims

1. A method for preparing a modified adsorbent material, characterized in that: The steps include: S1, soaking the adsorption substrate in an initiator solution to pre-absorb the redox polymerization initiator solution; S2. The adsorption substrate obtained by the treatment in step S1 is contacted with a grafting monomer to carry out gas phase redox grafting polymerization to form a grafting layer on the adsorption substrate to obtain a modified adsorption material.

2. The method for preparing the modified adsorbent material according to claim 1, characterized in that: In step S1, the adsorption substrate is selected from any one of cotton cloth, non-woven fabric, fiber or film containing adsorption functional groups.

3. The method for preparing the modified adsorbent material according to claim 2, characterized in that: The adsorption functional groups include any one or more of carboxyl, hydroxyl, amino or amidoxime groups.

4. The method for preparing the modified adsorbent material according to claim 1, characterized in that: In step S1, the initiator solution includes an initiator and a solvent, wherein the initiator is selected from any one of ammonium cerium nitrate, ammonium persulfate, potassium persulfate or sodium persulfate; and the solvent is selected from any one of hydrochloric acid solution, nitric acid solution or sulfuric acid solution.

5. The method for preparing the modified adsorbent material according to claim 4, characterized in that: In step S1, the final concentration of the initiator in the initiator solution is 1-10 wt %, and the acid concentration of the solvent in the initiator solution is 0.01%-1%.

6. The method for preparing the modified adsorbent material according to claim 1, characterized in that: In step S1, the temperature of the adsorption redox polymerization initiator solution is 0-45°C and the time is 10-15 minutes.

7. The method for preparing the modified adsorbent material according to claim 1, characterized in that: In step S2, the grafting monomer is selected from aniline or pyrrole, and the concentration of the grafting monomer is 50%-100%.

8. The method for preparing the modified adsorbent material according to claim 1, characterized in that: In step S2, the method of gas phase redox graft polymerization is: the adsorption substrate obtained by the treatment in step S1 is contacted with the steam of the grafting monomer for graft polymerization, the graft polymerization temperature is 0-50°C; the graft polymerization time is 1-60min.

9. A modified adsorbent material, characterized in that: Obtained based on the preparation method described in any one of claims 1-8.

10. A use of the modified adsorption material according to claim 9, characterized in that: The modified adsorption material adsorbs metal ions in the presence or absence of light.