Preparation method and application of oxygen vacancy-containing monatomic ruthenium-doped tungsten oxide catalyst
The preparation of oxygen-containing vacancies single-atom ruthenium doped tungsten oxide catalysts through a one-step solvothermal method has solved the problem of complex preparation of existing catalysts and low selective demethoxy activity, achieving efficient selective demethoxylation of guaiac compounds Methoxy conversion significantly improves the catalytic properties and the yield of alkyl monophenols.
Patent Information
- Application Number
- CN202410471262.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-18
- Publication Date
- 2024-11-12
AI Technical Summary
The existing catalysts have problems of complex preparation and low activity when catalyzing the selective demethoxy reaction in lignin, and it is difficult to effectively improve the yield of alkyl monophenols.
A one-step solvothermal method is used to prepare a single-atom ruthenium-doped tungsten oxide catalyst for oxygen-containing vacancy. The reaction of Ru salt, WCl6 and thioacetamide in alcohol solution is used to form an oxygen-rich catalyst for guaiac lignol. Selective demethoxy reaction of compounds.
The high yield of demethoxy conversion of guaiacol compounds with high catalytic activity and strong selectivity is achieved, which simplifies the catalyst preparation process, inhibits the hydrogenation of benzene ring and the retention of phenolic hydroxyl groups, and significantly improves the Catalytic properties.
Smart Images

Figure CN118925720A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of catalyst development and biomass conversion, and specifically relates to a preparation method and application of a ruthenium oxide catalyst doped with a single atom containing oxygen vacancies. Background Art
[0002] With the development of economy, the existing fossil energy can no longer meet the needs of current social development. Moreover, the excessive consumption of fossil energy has led to severe problems such as environmental pollution and global warming. The development of a new generation of renewable green energy has attracted much attention. As the fourth largest energy source on the earth, biomass energy has the advantages of abundant reserves, renewable, clean and environmentally friendly, zero CO2 net emission, convenient storage and transportation, etc. The important component of biomass energy is lignin, which is a complex polymer composed of basic units containing benzene rings connected by C-O bonds and C-C bonds. The monomer phenolic compounds can be used to make synthetic resins, surfactants and many other fine chemicals. It is a key source of renewable production of aromatic chemicals. At present, the research on catalytic conversion of lignin mainly focuses on the complete deoxygenation to generate aromatics or cycloalkanes. The high-value phenolic hydroxyl groups are also removed at the same time, which significantly reduces the economic efficiency of the conversion process. Therefore, the most promising way is to selectively convert lignin phenols into monophenolic high-value-added chemicals through effective catalytic technology, which not only promotes the development and utilization of low-priced and abundant biomass resources in my country, but also has a positive effect on environmental protection.
[0003] Guaiacol compounds in lignin contain C Ar –OH, C Ar –OCH3, C Ar O–CH3 three kinds of C–O bonds, among which C Ar – The bond energy of OCH3 is greater than that of C Ar O–CH3 but less than C Ar–OH, making the selective removal of methoxy groups more challenging. According to the characteristics of this reaction, if you want to increase the yield of alkyl monophenol compounds, you need to avoid hydrogenation of the benzene ring and retention of the phenolic hydroxyl group. Therefore, the hydrogenation activity and deoxygenation activity of the catalyst should not be too strong. The literature mainly reports oxides and metal-supported catalysts. Among them, literature 1 [Green Chem., 2019, 21, 3081] reported that the yield of 4-propylguaiacol selective demethoxylation product catalyzed by Au / Nb2O5 at 300°C was 84.2%; literature 2 [Fuel Process Technol., 2020, 199, 106224] reported that MoO3 / SiO2 can catalyze the selective demethoxylation of 4-propylguaiacol at 350°C to obtain a 65.2% yield of alkyl monophenol. Since the nature and content of oxygen vacancies have a great influence on the performance of catalysts, adjusting the defect structure of catalysts has become an important and effective strategy to improve the performance of catalysts. For example, reference 3 [ACS Sustainable Chem. Eng., 2021, 9, 34, 11604] studied the demethoxylation reaction mechanism of MoOx and found that its surface oxygen vacancies can enhance the adsorption and activation of guaiacol. Ar –OCH3 bond, promoting the occurrence of demethoxylation reaction; Reference 4 [Zhang Yaowen, PhD dissertation of Beijing University of Chemical Technology, 2022] also found that defective FeOx species can significantly promote C Ar The activation of the –OCH3 bond promotes the removal of the methoxy group in guaiacol. The above results show that constructing oxygen vacancies on oxide supports can improve the selective demethoxylation activity of the catalyst.
[0004] However, the current literature reports that the construction of oxygen vacancies mainly adopts methods such as element doping, etching, reduction and heat treatment. For example, reference 5 [Sep. Purif. Technol., 2022, 294: 121167] uses a solvothermal method to prepare Mo-doped W 18 O 49 Ultrathin nanowires, doping with Mo atoms will adjust W 18 O 49 The surface atomic structure and electronic state of the cerium oxide increase the concentration of oxygen vacancies; Chinese invention CN 117466326A discloses a method for etching to increase oxygen vacancies, so that the plasma is in full contact with the surface of cerium dioxide to obtain a cerium dioxide material rich in oxygen vacancies; Chinese invention CN 116375098A utilizes nitrogen and carbon dioxide generated by high-temperature heating of melamine to form a low-oxygen environment, so that the lattice oxygen of iron oxide is lost to form oxygen vacancies. However, these preparation methods are relatively complicated, and it is of great significance to continue to study simple and effective methods for increasing oxygen vacancies.
[0005] In order to increase the oxygen vacancies and selective demethoxylation activity of tungsten oxide, the present invention utilizes the reducibility of thioacetamide and adopts a one-step solvothermal method to prepare a metal ruthenium-doped tungsten oxide catalyst rich in oxygen vacancies, and applies it to the reaction of demethoxylating lignin guaiacol compounds to prepare alkyl monophenols. Summary of the invention
[0006] In view of the problems of complex preparation and low selective demethoxylation activity of existing catalysts, the present invention provides a preparation method and application of a ruthenium-doped tungsten oxide catalyst containing oxygen vacancies and single atoms. The preparation method is simple, the ruthenium content in the catalyst is very low, the oxygen vacancies are many, and the ruthenium content is single-atom dispersed. The prepared catalyst can efficiently catalyze the selective demethoxylation of guaiacol to convert it into alkyl monophenol.
[0007] The technical solution of the present invention is:
[0008] A method for preparing a ruthenium-doped tungsten oxide catalyst containing oxygen vacancies and a single atom thereof, which is prepared by a one-step solvothermal method, wherein the ruthenium content in the ruthenium-doped tungsten oxide catalyst is 0.01-0.1%. The method specifically comprises the following steps: dissolving Ru salt, WCl6 and thioacetamide in an alcohol solution, and then transferring the solution into a high-pressure reactor for solvothermal reaction, and then separating, washing and drying the precipitate to obtain the ruthenium-doped tungsten oxide catalyst.
[0009] Furthermore, the Ru salt is at least one of ruthenium chloride, ruthenium acetate, ruthenium iodide, and ruthenium acetylacetonate.
[0010] Furthermore, the alcohol solution is methanol, ethanol, propanol, isopropanol, butanol, etc.
[0011] Furthermore, the molar ratio of thioacetamide to WCl6 is 0.1 to 1:1, preferably 0.3 to 0.8:1.
[0012] Furthermore, the temperature of the solvent thermal reaction is 120 to 220° C., and the time is 6 to 24 hours.
[0013] Furthermore, the drying is vacuum drying, the drying temperature is 30 to 100° C., and the drying time is 1 to 24 hours.
[0014] Furthermore, in the ruthenium-doped tungsten oxide catalyst, ruthenium exists in the form of a single atom.
[0015] The catalyst obtained by the preparation method is applied to the selective demethoxylation reaction of guaiacol compounds, has high catalytic activity, and has a high yield of converting guaiacol compounds into monophenols through selective demethoxylation.
[0016] Furthermore, the guaiacol compound is at least one of guaiacol, 4-methylguaiacol, 4-ethylguaiacol and 4-propylguaiacol.
[0017] The beneficial effects of the present invention are:
[0018] The present invention prepares a noble metal ruthenium-doped tungsten oxide catalyst by one-pot reaction of Ru salt, WCl6 and thioacetamide, and W is reacted by a solvothermal method. 6+ The precipitate is an oxide, and in the presence of thioacetamide, the generated tungsten oxide is further deoxidized to form more oxygen vacancies, which promotes the adsorption of noble metal Ru ions on the oxygen vacancies, and then undergoes redox reactions, and Ru is fixed on the tungsten oxide in the form of a single atom. The catalyst preparation method is simple, the conditions are mild, and it is easy to operate. The Ru in the catalyst exists in the form of a single atom, which can promote the maximum activity of the noble metal component and make the Ru atom in a sulfide state. Compared with cluster or nanometal catalysts, the hydrogen dissociation activity of the single atom is significantly reduced. Therefore, in the selective demethoxylation reaction of guaiacol, the hydrogenation of the benzene ring and the removal of the phenolic hydroxyl group can be inhibited, showing good catalytic activity and selectivity. The present invention provides a simple method for the preparation of a single-atom catalyst, and the obtained catalyst can efficiently catalyze the high-value conversion of lignin biomass. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 The high angle annular dark field scanning transmission electron microscope (HAADF-STEM) image of the ruthenium-doped tungsten oxide catalyst prepared in the present invention (a) and the X-ray absorption fine structure spectrum (EXAFS) of the ruthenium-doped tungsten oxide catalyst, standard Ru and RuO2 prepared in Example 1 (b), wherein Figure 1 The white dots circled in yellow in a are Ru atoms. Figure 1 b shows that there is no Ru-Ru bond, so ruthenium is dispersed in a single-atom state on the tungsten oxide support. DETAILED DESCRIPTION
[0020] The present invention is further described in detail below with reference to specific embodiments, but the present invention is not limited thereto.
[0021] The reagents used in the examples were all analytically pure and the water was deionized water.
[0022] Example 1
[0023] According to the Ru loading amount of 0.04%, ruthenium chloride was added to 50mL ethanol, and then 1.2g WCl6 was added to dissolve, and then 0.114g thioacetamide was added to dissolve according to the sulfur / tungsten molar ratio of 0.5, and then transferred to a 200mL reactor for solvent thermal reaction at 160℃ for 24h. The resulting precipitate was washed with water, washed with alcohol, and vacuum dried at 60℃ for 6h to obtain a ruthenium-doped tungsten oxide catalyst. 0.1g of the above catalyst, 1.2g of 4-propylguaiacol and 15.0g of n-dodecane were added to a high-pressure reactor, and the air in the reactor was removed by displacement method. Then, after adjusting the hydrogen pressure to 3.0MPa, the temperature was raised to 225℃ and the reaction was continued for 8h, and the conversion rate reached 95.6%, and the selectivity of alkylphenol reached 98.3%.
[0024] Example 2
[0025] According to the Ru loading amount of 0.04%, ruthenium acetate was added to 50mL methanol, and then 1.2g WCl6 was added to dissolve, and then 0.023g thioacetamide was added to dissolve according to the sulfur / tungsten molar ratio of 0.1, and then transferred to a 200mL reactor for solvent thermal reaction at 120℃ for 24h. The obtained precipitate was washed with water, washed with alcohol, and vacuum dried at 100℃ for 1h to obtain a ruthenium-doped tungsten oxide catalyst. 0.1g of the above catalyst, 1.2g of 4-methylguaiacol and 15.0g of n-dodecane were added to a high-pressure reactor, and the air in the reactor was removed by displacement method. Then, after adjusting the hydrogen pressure to 3.0MPa, the temperature was raised to 225℃ and the reaction was continued for 8h, and the conversion rate reached 66.6%, and the selectivity of alkylphenol reached 60.9%.
[0026] Example 3
[0027] According to the Ru loading amount of 0.04%, ruthenium was added to 50mL propanol, and then 1.2g WCl6 was added to dissolve, and then 0.171g thioacetamide was added to dissolve according to the sulfur / tungsten molar ratio of 0.75, and then transferred to a 200mL reactor for solvent thermal reaction at 220℃ for 6h. The resulting precipitate was washed with water, washed with alcohol, and vacuum dried at 50℃ for 8h to obtain a ruthenium-doped tungsten oxide catalyst. 0.1g of the above catalyst, 1.2g of 4-propylguaiacol and 15.0g of n-dodecane were added to a high-pressure reactor, and the air in the reactor was removed by displacement method. Then, after adjusting the hydrogen pressure to 3.0MPa, the temperature was raised to 225℃ and the reaction was continued for 8h, and the conversion rate reached 82.8%, and the selectivity of alkylphenol reached 90.2%.
[0028] Example 4
[0029] According to the Ru loading amount of 0.1%, ruthenium acetylacetonate was added to 50mL isopropanol, and then 1.2g WCl6 was added to dissolve, and then 0.228g thioacetamide was added to dissolve according to the sulfur / tungsten molar ratio of 1, and then transferred to a 200mL reactor for solvent thermal reaction at 200℃ for 10h. The obtained precipitate was washed with water, washed with alcohol, and vacuum dried at 30℃ for 24h to obtain a ruthenium-doped tungsten oxide catalyst. 0.1g of the above catalyst, 1.2g of guaiacol and 15.0g of n-dodecane were added to a high-pressure reactor, and the air in the reactor was removed by displacement method. Then, after adjusting the hydrogen pressure to 3.0MPa, the temperature was raised to 225℃ and the reaction was continued for 8h, and the conversion rate reached 88.3%, and the selectivity of phenol reached 80.6%.
[0030] Example 5
[0031] According to the Ru loading amount of 0.05%, ruthenium chloride was added to 50mL butanol, and then 1.2g WCl6 was added to dissolve, and then 0.068g thioacetamide was added to dissolve according to the sulfur / tungsten molar ratio of 0.3, and then transferred to a 200mL reactor for solvent thermal reaction at 180℃ for 15h. The resulting precipitate was washed with water, washed with alcohol, and vacuum dried at 80℃ for 8h to obtain a ruthenium-doped tungsten oxide catalyst. 0.1g of the above catalyst, 1.2g of 4-propylguaiacol and 15.0g of n-dodecane were added to a high-pressure reactor, and the air in the reactor was removed by displacement method. Then, after adjusting the hydrogen pressure to 3.0MPa, the temperature was raised to 225℃ and the reaction was continued for 8h, and the conversion rate reached 90.1%, and the selectivity of alkylphenol reached 98.1%.
[0032] Example 6
[0033] According to the Ru loading amount of 0.03%, ruthenium chloride was added to 50mL butanol, and then 1.2g WCl6 was added to dissolve, and then 0.114g thioacetamide was added to dissolve according to the sulfur / tungsten molar ratio of 0.3, and then transferred to a 200mL reactor for solvent thermal reaction at 200℃ for 10h. The obtained precipitate was washed with water, washed with alcohol, and vacuum dried at 60℃ for 6h to obtain a ruthenium-doped tungsten oxide catalyst. 0.1g of the above catalyst, 1.2g of 4-ethylguaiacol and 15.0g of n-dodecane were added to a high-pressure reactor, and the air in the reactor was removed by displacement method. Then, after adjusting the hydrogen pressure to 3.0MPa, the temperature was raised to 225℃ and the reaction was continued for 8h, and the conversion rate reached 90.0%, and the selectivity of alkylphenol reached 96.4%.
[0034] Comparative Example 1
[0035] The same as Example 1, except that no ruthenium salt was added during the preparation of the catalyst, under the same reaction conditions, the conversion rate of 4-propylguaiacol was 87.1%, and the selectivity of alkylphenol reached 79.4%.
[0036] Comparative Example 2
[0037] The same as Example 1, except that no thioacetamide was added during the preparation of the catalyst, under the same reaction conditions, the conversion rate of 4-propylguaiacol was 29.8%, and the selectivity of alkylphenol reached 51.1%.
Claims
1. A method for preparing a ruthenium-doped tungsten oxide catalyst containing oxygen vacancies, characterized in that: The ruthenium-doped tungsten oxide catalyst is prepared by a one-step solvothermal method, and the ruthenium content in the ruthenium-doped tungsten oxide catalyst is 0.01-0.1%. The method specifically comprises the following steps: dissolving Ru salt, WCl6 and thioacetamide in an alcohol solution, and then transferring the solution into a high-pressure reactor for a solvothermal reaction, and then separating, washing and drying the precipitate to obtain the ruthenium-doped tungsten oxide catalyst.
2. The method for preparing the oxygen vacancy-containing single-atom ruthenium-doped tungsten oxide catalyst according to claim 1, characterized in that: The Ru salt is at least one of ruthenium chloride, ruthenium acetate, ruthenium iodide and ruthenium acetylacetonate.
3. The method for preparing the oxygen vacancy-containing single-atom ruthenium-doped tungsten oxide catalyst according to claim 1, characterized in that: The alcohol solution is methanol, ethanol, propanol, isopropanol or butanol.
4. The method for preparing the oxygen vacancy-containing single-atom ruthenium-doped tungsten oxide catalyst according to claim 1, characterized in that: The molar ratio of thioacetamide to WCl6 is 0.1 to 1:
1.
5. The method for preparing the oxygen vacancy-containing single-atom ruthenium-doped tungsten oxide catalyst according to claim 1, characterized in that: The temperature of the solvent thermal reaction is 120 to 220° C., and the time is 6 to 24 hours.
6. The method for preparing the oxygen vacancy-containing single-atom ruthenium-doped tungsten oxide catalyst according to claim 1, characterized in that: The drying is vacuum drying, the drying temperature is 30-100° C., and the drying time is 1-24 hours.
7. The method for preparing the oxygen vacancy-containing single-atom ruthenium-doped tungsten oxide catalyst according to claim 1, characterized in that: In the ruthenium-doped tungsten oxide catalyst, ruthenium exists in the form of single atoms.
8. Use of the oxygen vacancy-containing single-atom ruthenium-doped tungsten oxide catalyst obtained by the preparation method according to any one of claims 1 to 7 in the selective demethoxylation reaction of guaiacol compounds.
9. The use according to claim 8, characterized in that The guaiacol compound is at least one of guaiacol, 4-methylguaiacol, 4-ethylguaiacol and 4-propylguaiacol.