Hydrofining catalyst, preparation method and application thereof, composite carrier and preparation method thereof

Through the combination of cheap biomass charcoal coated with alumina composite support and Group VIII and Group VIB metal components, the existing hydrorefining catalyst activity improvement problem is solved, efficient desulfurization and nitrogen removal effects are achieved, and the preparation cost is reduced. and complexity.

CN118925740APending Publication Date: 2024-11-12CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310539376.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-12
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The activity improvement of existing hydrorefining catalysts is difficult to achieve, and traditional carbon precursors are costly and complex in preparation processes, making it difficult to effectively regulate the surface properties of the carrier.

Method used

The biomass carbon-coated alumina composite carrier is prepared by mixing, calcining and hydrothermal treatment of biomass raw materials and alumina precursors, and the group VIII and group VIB metal components are used as Active metal component, regulates the interaction force of the active metal and the support in the catalyst.

Benefits of technology

It significantly improves the desulfurization and nitrogen removal performance of the catalyst, reduces the preparation cost and process complexity, realizes effective regulation of the surface properties of the carrier, and improves the activity of the catalyst.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118925740A_ABST
    Figure CN118925740A_ABST
Patent Text Reader

Abstract

The invention relates to a hydrofining catalyst, a preparation method and application thereof, a composite carrier and a preparation method thereof, and the hydrofining catalyst comprises 40-80 wt% of a carrier and 18-50 wt% of an active metal component based on the total weight of the hydrofining catalyst; the carrier comprises a biomass charcoal coated aluminum oxide composite carrier; the active metal components comprise a first active metal component and a second active metal component, and the first active metal component is selected from one or more of VIII group metal elements; and the second active metal component is selected from one or more of VIB group metal elements. The biomass charcoal coated aluminum oxide composite carrier can be simply and cheaply prepared, and the surface property of the composite carrier is effectively regulated and controlled; and the desulfurization and denitrification performances of the catalyst are effectively improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to the technical field of petrochemical engineering, and in particular, to a hydrorefining catalyst and a preparation method and application thereof, a composite carrier and a preparation method thereof. Background Art

[0002] As the blood of industry, oil is known as "black gold". However, the sulfur and nitrogen compounds contained in oil release SOx and NOx after combustion, which can cause serious environmental pollution. Therefore, countries around the world have successively formulated increasingly stringent environmental regulations to limit the content of sulfur and nitrogen in refined oil products, promote the upgrading of oil quality, and produce clean oil products. In modern oil processing, hydrodesulfurization process is the key technology for producing clean oil products, and its core lies in the development of supported sulfurized Co(Ni)Mo(W) catalyst.

[0003] γ-Al2O3 is a common carrier of traditional hydrorefining catalysts. Its surface has a large number of active -OH sites, which makes it interact strongly with active metals. Although this is beneficial to the dispersion of active metals to a certain extent, it also reduces the reduction performance of active metals and makes them difficult to be sulfided / activated, resulting in a decrease in the degree of sulfidation of the sulfided Co(Ni)Mo(W) catalyst (reduction in active phase), and the active phase is mainly composed of Co-Mo-SI type active phases with low activity and low stacking layers, which ultimately limits the improvement of catalyst activity. Therefore, how to achieve the modulation of the properties of γ-Al2O3 carriers is very important for the preparation of highly active hydrorefining catalysts. Carbon materials, as a typical surface inert material, are used to modify the surface properties of traditional γ-Al2O3 carriers to improve the activity of hydrogenation catalysts, which has great development prospects.

[0004] CN 100406122C discloses a method for preparing an Al2O3 carrier with large pore size, concentrated pore distribution, good strength, etc. by using rice husk powder, peanut shell powder, and coconut shell powder as pore expanders, and the carrier is applied to the hydrogenation process of heavy oil and residual oil, and finally the hydrodesulfurization rate of the catalyst is only increased by about 4%, and the effect is average. In addition, in the process, only crop stem shell powder is used as a pore expander, and the surface properties of the Al2O3 carrier cannot be regulated.

[0005] CN 101733151A discloses a method for preparing a carbon-containing γ-Al2O3 carrier by using organic carboxylic acid and organic carboxylic acid ammonium salt as carbon precursors, introducing the carbon precursors on a formed γ-Al2O3 carrier by an impregnation method, and then calcining the carrier under an inert atmosphere, so that the desulfurization rate of the catalyst is increased by about 6%. However, the process uses organic acid as a carbon precursor, which is costly.

[0006] CN 105688924B discloses a method for preparing a carbon γ-Al2O3 carrier by mechanical kneading using alcohol, sugar and organic acid as carbon sources. At the same time, an impregnation method is further used and P and organic matter are added as additives to finally prepare a hydrorefining catalyst. Although the activity of the catalyst is improved to a certain extent, the cost of the carbon precursor used is relatively high and the preparation process is complicated.

[0007] In summary, the currently disclosed technologies still have deficiencies in improving the activity of catalysts. At the same time, the relatively expensive carbon precursors and cumbersome preparation processes also hinder the development of the technology. Therefore, finding a simple and inexpensive method for preparing carbon@Al2O3 composite carriers to improve the activity of hydrotreating catalysts is a key technical problem that needs to be solved in this field. Summary of the invention

[0008] The purpose of the present disclosure is to provide a hydrorefining catalyst and its preparation method and application, a composite carrier and its preparation method, which can simply and cheaply prepare a biomass carbon-coated alumina composite carrier, and the surface properties of the composite carrier are effectively regulated; and the desulfurization and denitrification performance of the catalyst are effectively improved.

[0009] In order to achieve the above-mentioned objectives, the first aspect of the present disclosure provides a hydrotreating catalyst, which, based on the total weight of the hydrotreating catalyst, comprises 40 to 80 weight percent of a carrier and 18 to 50 weight percent of an active metal component; the carrier comprises a biochar-coated alumina composite carrier; the active metal component comprises a first active metal component and a second active metal component, the first active metal component being selected from one or more of the Group VIII metal elements; the second active metal component being selected from one or more of the Group VIB metal elements.

[0010] Optionally, based on the total weight of the carrier, the carrier comprises 0.1 to 10 weight % of biochar and 90 to 99.9 weight % of alumina;

[0011] Optionally, based on the total weight of the hydrotreating catalyst, the content of the first active metal component in the form of oxide is 3 to 10 wt %; the content of the second active metal component is 15 to 40 wt %.

[0012] Optionally, the total acid content of the biochar-coated alumina composite carrier measured by pyridine infrared is 100-200 μmol / g, and the BET specific surface area of ​​the biochar-coated alumina composite carrier is 300-450 m 2 / g.

[0013] Optionally, the first active metal component is selected from one or both of Ni and Co; the second active metal component is selected from one or both of Mo and W.

[0014] The second aspect of the present disclosure provides a method for preparing a biomass carbon-coated alumina composite carrier, comprising the following steps:

[0015] S1, mixing the biomass raw material with the alumina precursor to obtain a composite carrier precursor;

[0016] S2, subjecting the composite carrier precursor to a first calcination treatment to obtain a composite carrier intermediate;

[0017] S3, subjecting the composite carrier intermediate to hydrothermal treatment.

[0018] Optionally, in step S1, based on the total weight of the composite carrier precursor, the content of the biomass raw material is 5 to 40 weight %; and the content of the alumina precursor is 60 to 95 weight %.

[0019] Optionally, in step S1, the biomass raw material is selected from one or more of corn stalks, wheat stalks, rice stalks and sorghum stalks;

[0020] The aluminum oxide precursor is selected from one or more of pseudo-boehmite, aluminum hydroxide and aluminum nitrate; preferably pseudo-boehmite.

[0021] Optionally, the method further comprises: subjecting the biomass raw material to a first drying process, a crushing process, and a sieving process to obtain a biomass powder having a particle size of less than 60 meshes, and then mixing and grinding the biomass powder with the alumina precursor to a particle size of less than 200 meshes to obtain a composite carrier precursor;

[0022] Optionally, the conditions of the first drying treatment include: drying at 60 to 150° C. for 12 to 36 hours;

[0023] Optionally, the grinding treatment conditions include: grinding at 1000-10000 r / min for 12-36 hours.

[0024] Optionally, in step S2, the conditions of the first calcination treatment include: a calcination temperature of 300 to 700° C., a calcination time of 3 to 8 hours; a calcination atmosphere of one or more of air, nitrogen, oxygen, argon and water vapor;

[0025] Preferably, before the first calcination treatment, the composite carrier precursor is dried at 60 to 150° C. for 4 to 15 hours.

[0026] Optionally, in step S3, the conditions of the hydrothermal treatment include: a hydrothermal temperature of 150 to 350° C., a hydrothermal time of 2 to 8 hours, and an atmosphere of the hydrothermal treatment selected from one or more of oxygen, nitrogen, ammonia and carbon dioxide;

[0027] Preferably, step S3 further comprises: adding deionized water dropwise to the composite carrier intermediate until it reaches a saturated water absorption state, and then performing the hydrothermal treatment;

[0028] Optionally, the method further comprises: cooling the hydrothermal treatment product and drying it at 60 to 150° C. for 4 to 15 hours.

[0029] A third aspect of the present disclosure provides a biomass carbon-coated alumina composite carrier prepared according to the method of the second aspect.

[0030] A fourth aspect of the present disclosure provides a method for preparing a hydrotreating catalyst, comprising the following steps:

[0031] An active metal precursor, a carrier and an additive are mixed, and then subjected to a molding treatment and a second calcination treatment; wherein the carrier comprises the biomass carbon-coated alumina composite carrier of the third aspect; wherein the active metal precursor comprises a first active metal precursor and a second active metal precursor; the first active metal precursor is selected from one or more of the Group VIII metal precursors; and the second active metal precursor is selected from one or more of the Group VIB metal precursors.

[0032] Optionally, the method comprises: impregnating a solution of an active metal precursor with a support;

[0033] Optionally, the first active metal precursor is selected from one or more of a nickel metal precursor and a cobalt metal precursor; preferably, the nickel metal precursor is selected from one or more of nickel nitrate, basic nickel carbonate and nickel sulfate, preferably basic nickel carbonate and / or nickel nitrate; the cobalt metal precursor is selected from one or more of cobalt sulfate, cobalt carbonate, cobalt oxalate and cobalt nitrate, preferably cobalt nitrate and / or cobalt oxalate;

[0034] The second active metal precursor is selected from one or more of a molybdenum metal precursor and a tungsten metal precursor; preferably, the molybdenum metal precursor is selected from one or more of sodium molybdate, ammonium molybdate, molybdenum chloride and molybdic acid, preferably ammonium molybdate; the tungsten metal precursor is selected from one or more of ammonium metatungstate, phosphotungstic acid and silicotungstic acid, preferably ammonium metatungstate and / or phosphotungstic acid;

[0035] Preferably, the weight ratio of the first active metal precursor: the second active metal precursor: the biomass carbon-coated alumina composite carrier is 0.2-0.6:0.3-0.7:1.

[0036] Optionally, the conditions of the second calcination treatment include: a calcination temperature of 300-600°C, a calcination time of 3-6 hours; a calcination atmosphere of one or more of air, nitrogen, oxygen, argon and water vapor; optionally, before performing the second calcination treatment, the product obtained by the molding treatment is dried at 80-160°C for 4-12 hours.

[0037] A fifth aspect of the present disclosure provides a hydrotreating catalyst prepared according to the method of the fourth aspect of the present disclosure.

[0038] A sixth aspect of the present disclosure provides use of the hydrotreating catalyst of the first aspect or the fifth aspect in a feedstock oil hydrotreating reaction.

[0039] Optionally, the method comprises the following steps: contacting the crude oil with the hydrofining catalyst under hydrogenation conditions to carry out a hydrofining reaction;

[0040] Optionally, the conditions of the hydrofining reaction include: reaction temperature of 260-380°C; hydrogen pressure of 2-10 MPa; hydrogen-oil volume ratio of 200-800:1; feed oil mass space velocity of 0.5-6h -1 ;

[0041] Optionally, the feedstock oil is selected from gasoline and / or diesel fractions;

[0042] Preferably, the method further comprises: performing a sulfidation treatment on the hydrotreating catalyst before carrying out the hydrotreating reaction.

[0043] Through the above technical scheme, the present disclosure provides a hydrorefining catalyst and its preparation method and application, a composite carrier and its preparation method. The present disclosure uses cheap biomass raw materials to prepare a biomass carbon-coated alumina composite carrier with a "tree root"-like structure, and uses at least one metal component of Group VIII and at least one metal component of Group VIB as an active metal component to prepare a hydrorefining catalyst. The biomass carbon-coated alumina composite carrier provided by the present disclosure can effectively regulate the interaction force between the active metal and the carrier in the catalyst, modify the microscopic stacking structure of the metal active phase, and significantly improve the activity of the catalyst.

[0044] Other features and advantages of the present disclosure will be described in detail in the following detailed description. BRIEF DESCRIPTION OF THE DRAWINGS

[0045] The accompanying drawings are used to provide a further understanding of the present disclosure and constitute a part of the specification. Together with the following specific embodiments, they are used to explain the present disclosure but do not constitute a limitation of the present disclosure. In the accompanying drawings:

[0046] Figure 1This is a scanning electron microscope photograph of the biomass carbon-coated alumina composite carrier prepared in Example 4. DETAILED DESCRIPTION

[0047] The specific embodiments of the present disclosure are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present disclosure, and are not used to limit the present disclosure.

[0048] A first aspect of the present disclosure provides a hydrotreating catalyst, which comprises 40 to 80 weight percent of a carrier and 18 to 50 weight percent of an active metal component based on the total weight of the hydrotreating catalyst; the carrier comprises a biochar-coated alumina composite carrier; the active metal component comprises a first active metal component and a second active metal component, the first active metal component being selected from one or more of the Group VIII metal elements; the second active metal component being selected from one or more of the Group VIB metal elements.

[0049] The present invention uses cheap biomass raw materials to prepare a biomass carbon-coated alumina composite carrier with a "tree root"-like structure, and uses at least one metal component of Group VIII and at least one metal component of Group VIB as an active metal component to prepare a hydrorefining catalyst. The biomass carbon-coated alumina composite carrier provided by the present invention can effectively regulate the interaction force between the active metal and the carrier in the catalyst, modify the microscopic stacking structure of the metal active phase, and significantly improve the activity of the catalyst.

[0050] In the present disclosure, the symbol "@" indicates that the substance before the symbol is coated on the surface of the substance after the symbol, that is, "biomass carbon coated alumina composite carrier" can be represented by "biomass carbon@alumina composite carrier" or "biomass C@alumina composite carrier".

[0051] In the present disclosure, biomass charcoal refers to a product prepared from biomass raw materials through a process including roasting, etc. Biomass raw materials include common raw materials such as corn stalks, wheat stalks, rice stalks and sorghum stalks.

[0052] In one embodiment, based on the total weight of the carrier, the carrier includes 0.1 to 10 weight % of biochar and 90 to 99.9 weight % of alumina; preferably, the carrier includes 1 to 7 weight % of biochar and 93 to 99 weight % of alumina. In the present disclosure, the content of alumina and biochar in the carrier is determined by thermogravimetric method. Using a carrier having the component composition in this embodiment, the hydrorefining catalyst can have a better catalytic effect.

[0053] In one embodiment, based on the total weight of the hydrotreating catalyst, the metal active components are in the form of oxides, and the content of the first active metal component is 3 to 10 weight %; the content of the second active metal component is 15 to 40 weight %.

[0054] In a preferred embodiment, the total acid content of the biochar-coated alumina composite carrier measured by pyridine infrared is 100-200 μmol / g; preferably 140-180 μmol / g. The composite carrier provided by the present disclosure has a lower acid content than ordinary γ-Al2O3, indicating that the introduction of biochar on the surface of the composite carrier of the present disclosure achieves effective regulation of the surface properties of the carrier.

[0055] In one embodiment, the BET specific surface area of ​​the biomass carbon-coated alumina composite carrier is 300 to 450 m 2 / g.

[0056] In a specific embodiment, the first active metal component is selected from one or both of nickel (Ni) and cobalt (Co); the second active metal component is selected from one or both of molybdenum (Mo) and tungsten (W).

[0057] The second aspect of the present disclosure provides a method for preparing a biomass carbon-coated alumina composite carrier, comprising the following steps:

[0058] S1, mixing the biomass raw material with the alumina precursor to obtain a composite carrier precursor;

[0059] S2, subjecting the composite carrier precursor to a first calcination treatment to obtain a composite carrier intermediate;

[0060] S3, subjecting the composite carrier intermediate to hydrothermal treatment.

[0061] In the present disclosure, the biomass raw material is mixed with an alumina precursor and then subjected to a first calcination treatment, which allows the biochar and alumina to interact with each other during the calcination process to form an intermediate of a biochar-coated alumina composite carrier; the composite carrier intermediate obtained by calcination is then subjected to a hydrothermal treatment, and the hydrothermal treatment environment can be used to improve the properties of the interface between the biochar and alumina, thereby promoting the formation of a "tree root"-like surface structure.

[0062] In one embodiment, in step S1, based on the total weight of the composite carrier precursor, the content of the biomass raw material is 5 to 40% by weight; and the content of the alumina precursor is 60 to 95% by weight.

[0063] In a specific embodiment, in step S1, the biomass raw material is selected from one or more of corn stalks, wheat stalks, rice stalks and sorghum stalks;

[0064] The alumina precursor is selected from one or more of pseudo-boehmite, aluminum hydroxide and aluminum nitrate.

[0065] In a preferred embodiment, the method further comprises:

[0066] The biomass raw material is subjected to a first drying treatment, a crushing treatment, and a sieving treatment to obtain a biomass powder with a particle size of less than 60 meshes, and then mixed with the alumina precursor and ground to a particle size of less than 200 meshes to obtain a composite carrier precursor;

[0067] Optionally, the conditions of the first drying treatment include: drying at 60 to 150° C. for 12 to 36 hours;

[0068] Optionally, the grinding treatment conditions include: grinding at 1000-10000 r / min for 12-36 hours.

[0069] In one embodiment, in step S2, the conditions of the first calcination treatment include: a calcination temperature of 300 to 700° C., a calcination time of 3 to 8 hours; and a calcination atmosphere of one or more of air, nitrogen, oxygen, argon and water vapor;

[0070] Preferably, before the first calcination treatment, the composite carrier precursor is dried at 60 to 150° C. for 4 to 15 hours.

[0071] In one embodiment, in step S3, the conditions of the hydrothermal treatment include: the hydrothermal temperature is 150-350° C., the hydrothermal time is 2-8 hours; and the atmosphere of the hydrothermal treatment is selected from one or more of oxygen, nitrogen, ammonia and carbon dioxide.

[0072] In a specific embodiment, step S3 further includes: adding deionized water dropwise to the composite carrier intermediate until it reaches a saturated water absorption state, and then performing a hydrothermal treatment.

[0073] In a specific embodiment, the method further comprises: cooling the hydrothermal treatment product and then drying it at 60 to 150° C. for 4 to 15 hours.

[0074] The devices used in the preparation process of the composite carrier disclosed in the present invention are all conventional devices in the art.

[0075] A third aspect of the present disclosure provides a biomass carbon-coated alumina composite carrier prepared according to the method of the second aspect.

[0076] A fourth aspect of the present disclosure provides a method for preparing a hydrotreating catalyst, comprising the following steps:

[0077] An active metal precursor, a carrier and an auxiliary agent are mixed, and then subjected to a molding treatment and a second calcination treatment; wherein the carrier comprises the biomass carbon-coated alumina composite carrier of the third aspect of the present disclosure; wherein the active metal precursor comprises a first active metal precursor and a second active metal precursor; the first active metal precursor is selected from one or more of the Group VIII metal precursors; and the second active metal precursor is selected from one or more of the Group VIB metal precursors.

[0078] In the present disclosure, the mixing and molding processes can adopt conventional processes and conditions in the art.

[0079] In a preferred embodiment, the weight ratio of the first active metal precursor: the second active metal precursor: the biomass carbon coated alumina composite carrier is 0.2-0.6: 0.3-0.7: 1. By preparing the catalyst according to the mass ratio in this embodiment, a hydrorefining catalyst with better catalytic performance can be obtained.

[0080] In one embodiment, the method includes: impregnating a solution of an active metal precursor with a support;

[0081] Optionally, the conditions for the immersion treatment include: the immersion time is 0.5 to 4 hours, preferably 0.5 to 2.5 hours.

[0082] In a specific embodiment, the first active metal precursor is one or more of a nickel metal precursor and a cobalt metal precursor; preferably, the nickel metal precursor is one or more selected from nickel nitrate, basic nickel carbonate and nickel sulfate, preferably basic nickel carbonate and / or nickel nitrate; the cobalt metal precursor is one or more selected from cobalt sulfate, cobalt carbonate, cobalt oxalate and cobalt nitrate, preferably cobalt nitrate and / or cobalt oxalate;

[0083] The second active metal precursor is selected from one or more of a molybdenum metal precursor and a tungsten metal precursor; preferably, the molybdenum metal precursor is selected from one or more of sodium molybdate, ammonium molybdate, molybdenum chloride and molybdic acid, preferably ammonium molybdate; the tungsten metal precursor is selected from one or more of ammonium metatungstate, phosphotungstic acid and silicotungstic acid, preferably ammonium metatungstate and / or phosphotungstic acid.

[0084] In the present disclosure, the molding process includes one of extrusion molding and reverse molding, preferably extrusion molding. The specific process and device of extrusion molding are well known to those skilled in the art.

[0085] In one embodiment, the auxiliary agent includes an extrusion aid and a binder;

[0086] The extrusion aid is selected from one or more of starch, sesbania powder, polyethylene glycol and methyl cellulose; preferably, the amount of the extrusion aid added is 1 to 10% by weight, preferably 3 to 8% by weight, based on the total weight of each component;

[0087] The binder is selected from one or more of nitric acid, citric acid, tartaric acid, oxalic acid and oxalic acid; preferably, the addition amount of the binder is 1 to 10 weight %, preferably 3 to 8 weight %, based on the total weight of each component.

[0088] The reagents used in the present disclosure can be purchased through conventional channels or prepared by known methods.

[0089] In a specific embodiment, the catalyst product obtained by the molding process may have a strip shape, a clover shape, a granular shape, or a toothed ball shape.

[0090] In one embodiment, the conditions of the second calcination treatment include: a calcination temperature of 300 to 600° C., a calcination time of 3 to 6 hours; a calcination atmosphere of one or more of air, nitrogen, oxygen, argon and water vapor;

[0091] Optionally, before the second calcination process, the product obtained by the molding process is dried at 80 to 160° C. for 4 to 12 hours.

[0092] A fifth aspect of the present disclosure provides a hydrotreating catalyst prepared according to the method of the fourth aspect of the present disclosure.

[0093] A sixth aspect of the present disclosure provides use of the hydrotreating catalyst of the first aspect or the fifth aspect in a feedstock oil hydrotreating reaction.

[0094] In one embodiment, the method comprises the following steps: contacting the feedstock oil with the hydrofining catalyst under hydrogenation conditions to carry out a hydrofining reaction;

[0095] Optionally, the conditions of the hydrofining reaction include: reaction temperature of 260-380°C; hydrogen pressure of 2-10 MPa; hydrogen-oil volume ratio of 200-800:1; feed oil mass space velocity of 0.5-6h -1 ;

[0096] Optionally, the feedstock oil is selected from gasoline and / or diesel fractions.

[0097] In a preferred embodiment, the method further comprises: performing a sulfidation treatment on the hydrotreating catalyst before performing the hydrotreating reaction;

[0098] Optionally, the temperature of the vulcanization treatment is 200-500°C, the pressure is 0.1-10 MPa, the time of the vulcanization treatment is 1-60 hours, and the mass space velocity of the pre-vulcanized oil is 0.1-20 hours. -1 , the volume ratio of hydrogen to oil is 100-800.

[0099] The present disclosure is further described in detail by way of examples. The raw materials used in the examples can all be obtained through commercial channels. The instruments used for the performance tests are also the detection instruments of conventional manufacturers in the field.

[0100] The determination and calculation methods of the total content of the oxides of the active component metals in the catalyst are all known determination and calculation methods in the art, specifically including XRF and ICP methods.

[0101] The test method for the acid content of the biochar-coated alumina composite carrier includes a pyridine infrared method.

[0102] The test methods for the content of biomass char and alumina in the composite support include thermogravimetric analysis.

[0103] The BET specific surface area of ​​the sample was determined by nitrogen physical adsorption at low temperature.

[0104] In the following examples and comparative examples, “C@Al2O3” means carbon-coated alumina.

[0105] Example 1

[0106] This embodiment provides a hydrotreating catalyst, and the specific preparation method includes the following steps:

[0107] Preparation of composite carrier:

[0108] (1) Take an appropriate amount of wheat straw, dry it at 80°C for 24 hours, crush it with a pulverizer, and sieve it. Take 20g of biomass powder with a particle size of less than 60 mesh after sieving and mix it with 80g of pseudo-boehmite, place it in a ball mill and grind it at a speed of 5000 rpm for 24 hours to obtain a composite carrier precursor with a particle size of less than 200 mesh, wherein the content of the biomass raw material is 20% by weight based on the total weight of the composite carrier precursor; the content of the alumina precursor is 80% by weight.

[0109] (2) The composite support precursor was dried at 100°C for 6 h, and then calcined at 500°C in a 10 vol% O2 / Ar atmosphere for 5 h. After natural cooling, a C@Al2O3 composite support intermediate was obtained.

[0110] (3) The composite carrier intermediate was placed in a hydrothermal kettle and 115.6 g of deionized water was added dropwise. The hydrothermal kettle was replaced with nitrogen. The intermediate was hydrothermally treated at 200 °C for 4 h. After natural cooling, the intermediate was dried at 80 °C for 6 h to obtain a biomass C@Al2O3 composite carrier, which was labeled as C-1. The composition of the carrier is listed in Table 1.

[0111] Preparation of catalyst:

[0112] (4) 4.67 g of nickel nitrate and 8.02 g of ammonium metatungstate were dissolved in 65.7 g of deionized water to prepare a mixed impregnation solution. The mixed impregnation solution was added dropwise onto 21.90 g of the above C@Al2O3 composite carrier powder and mixed evenly (the weight ratio of the first active metal precursor: the second active metal precursor: the biochar-coated alumina composite carrier was 0.21:0.37:1), and then dried at 100°C for 8 hours, and then evenly mixed with 0.5 g of Tianqing powder, 0.4 g of nitric acid, 0.6 g of citric acid and an appropriate amount of deionized water, and extruded into a clover-shaped catalyst with a diameter of 1.5 mm.

[0113] (5) The obtained cloverleaf-shaped catalyst was dried at 80°C for 12 h, calcined at 500°C for 4 h, and naturally cooled to obtain a hydrotreating catalyst, which was labeled as AC-1.

[0114] It was measured that the total content of active metal components of nickel oxide and tungsten oxide in the AC-1 catalyst was 27.0 weight % (based on the total weight of the catalyst), of which the content of the first active metal component (nickel oxide) was 4.0 weight %; the content of the second active metal component (tungsten oxide) was 23.0 weight %; and the carrier content was 73.0 weight %.

[0115] Comparative Example 1

[0116] This comparative example adopts a preparation method similar to that of Example 1, and the difference from Example 1 is that the biomass C@Al2O3 composite carrier is replaced with a conventional γ-Al2O3 carrier, specifically comprising:

[0117] (1) Take 100 g of pseudo-boehmite, calcine it at 500°C in air atmosphere for 4 h, and then cool it naturally to obtain a γ-Al2O3 carrier.

[0118] (2) 4.67 g of nickel nitrate and 8.02 g of ammonium metatungstate were dissolved in 95.62 g of deionized water to prepare a mixed impregnation solution. The mixed impregnation solution was added dropwise onto 30.85 g of γ-Al2O3 carrier and mixed evenly, then dried at 100°C for 8 hours, and then mixed evenly with 0.5 g of Tianqing powder, 0.4 g of nitric acid, 0.6 g of citric acid and an appropriate amount of deionized water, and extruded into a clover-shaped catalyst with a diameter of 1.5 mm;

[0119] (3) The prepared cloverleaf-shaped catalyst was dried at 80°C for 12 h, and then calcined at 500°C for 4 h. After natural cooling, a comparative catalyst was obtained, which was marked as R-1.

[0120] The total content of nickel oxide and tungsten oxide in the R-1 catalyst was measured to be 27.0 wt % (based on the total weight of the catalyst), of which the content of nickel oxide was 4.0 wt %; the content of tungsten oxide was 23.0 wt %; and the content of the carrier was 73.0 wt %.

[0121] Example 2

[0122] This embodiment provides a hydrotreating catalyst, and the specific preparation method includes the following steps:

[0123] Preparation of composite carrier:

[0124] (1) Take appropriate amounts of wheat straw and corn stalk, dry them at 70°C for 24 hours, and then crush them with a grinder and sieve them. Take 30g of biomass powder with a particle size of less than 60 mesh after sieving and mix it with 70g of pseudo-boehmite, place it in a ball mill and grind it at a speed of 4000 rpm for 18 hours to obtain a composite carrier precursor with a particle size of less than 200 mesh, wherein the content of the biomass raw material is 30% by weight based on the total weight of the composite carrier precursor; the content of the alumina precursor is 70% by weight;

[0125] (2) drying the composite support precursor at 100° C. for 8 h, and then calcining at 400° C. in a 15 vol% O2 / Ar atmosphere for 5 h, and cooling naturally to obtain a C@Al2O3 composite support intermediate;

[0126] (3) The composite carrier intermediate was placed in a hydrothermal kettle and 123.4 g of deionized water was added dropwise. The hydrothermal kettle was replaced with carbon dioxide and hydrothermally treated at 250 °C for 4 h. After natural cooling, it was dried at 80 °C for 6 h to obtain a biomass C@Al2O3 composite carrier, which was labeled as C-2. The composition of the carrier is listed in Table 1.

[0127] Preparation of catalyst:

[0128] (4) Take 5.84g of nickel nitrate and 9.77g of ammonium metatungstate and dissolve them in 60.30g of deionized water to prepare a mixed impregnation solution (the weight ratio of the first active metal precursor: the second active metal precursor: the biomass carbon-coated alumina composite carrier is 0.29:0.49:1). The mixed impregnation solution is added drop by drop onto 20.10g of the above C@Al2O3 composite carrier and mixed evenly, then dried at 120°C for 6 hours, and then evenly mixed with 0.4g of methyl cellulose, 0.2g of Tianqing powder, 0.3g of nitric acid, 0.4g of citric acid and an appropriate amount of deionized water, and extruded into a strip catalyst with a diameter of 1.5mm;

[0129] (5) The obtained strip catalyst was dried at 100°C for 8 h, and then calcined at 450°C for 6 h. After natural cooling, a hydrotreating catalyst was obtained, which was labeled as AC-2.

[0130] It was measured that the total content of active metal components of nickel oxide and tungsten oxide in the AC-2 catalyst was 33.0 weight % (based on the total weight of the catalyst), of which the content of the first active metal component (nickel oxide) was 5.0 weight %; the content of the second active metal component (tungsten oxide) was 28.0 weight %; and the carrier content was 67.0 weight %.

[0131] Comparative Example 2

[0132] This comparative example provides a hydrogenation catalyst. This comparative example adopts a preparation method similar to that of Example 2, and the difference from Example 2 is that the biomass C@Al2O3 composite carrier is replaced with a conventional γ-Al2O3 carrier, specifically comprising:

[0133] (1) Take 100 g of pseudo-boehmite, calcine it at 500°C in air atmosphere for 4 h, and then cool it naturally to obtain a γ-Al2O3 carrier.

[0134] (2) 5.84 g of nickel nitrate and 9.77 g of ammonium metatungstate were dissolved in 87.76 g of deionized water to prepare a mixed impregnation solution. The mixed impregnation solution was added dropwise to 28.31 g of γ-Al2O3 carrier and mixed evenly, then dried at 120°C for 6 hours, and then mixed evenly with 0.4 g of methyl cellulose, 0.2 g of Tianqing powder, 0.3 g of nitric acid, 0.4 g of citric acid and an appropriate amount of deionized water, and extruded into a strip catalyst with a diameter of 1.5 mm;

[0135] (3) The obtained strip catalyst was dried at 100°C for 8 hours, and then calcined at 450°C for 6 hours. After natural cooling, a hydrotreating catalyst was obtained, which was marked as R-2.

[0136] The total content of nickel oxide and tungsten oxide in the R-2 catalyst was measured to be 33.0 wt% (based on the total weight of the catalyst), of which the content of nickel oxide was 5.0 wt%; the content of tungsten oxide was 28.0 wt%; and the content of the carrier was 67.0 wt%.

[0137] Example 3

[0138] This embodiment provides a hydrotreating catalyst, and the specific preparation method includes the following steps:

[0139] Preparation of composite carrier:

[0140] (1) Take appropriate amounts of wheat straw, corn straw and rice straw respectively, dry them at 70°C for 24 hours, and then crush them with a grinder and sieve them. Take 30g of biomass powder with a particle size of less than 60 mesh after sieving and mix it with 70g of pseudo-boehmite, place it in a ball mill and grind it at a speed of 4000 rpm for 18 hours to obtain a composite carrier precursor with a particle size of less than 200 mesh, wherein the content of the biomass raw material is 30% by weight based on the total weight of the composite carrier precursor; the content of the alumina precursor is 70% by weight;

[0141] (2) drying the composite support precursor at 100° C. for 8 h, and then calcining at 400° C. in a 20 vol% O2 / N2 atmosphere for 5 h, and cooling naturally to obtain a C@Al2O3 composite support intermediate;

[0142] (3) The composite carrier intermediate was placed in a hydrothermal kettle and 130.2 g of deionized water was added dropwise. The hydrothermal kettle was replaced with carbon dioxide. The intermediate was hydrothermally treated at 300 °C for 4 h. After natural cooling, the intermediate was dried at 80 °C for 6 h to obtain a biomass C@Al2O3 composite carrier, which was labeled as C-3. The composition of the carrier is listed in Table 1.

[0143] Preparation of catalyst:

[0144] (4) Take 9.34g of nickel nitrate and 11.86g of ammonium metatungstate and dissolve them in 52.20g of deionized water to prepare a mixed impregnation solution. Add the mixed impregnation solution drop by drop onto 17.40g of the above C@Al2O3 composite carrier powder and mix them evenly (the weight ratio of the first active metal precursor: the second active metal precursor: the biochar-coated alumina composite carrier is 0.54:0.68:1), then dry it at 120°C for 5 hours, and then mix it evenly with 0.7g of methyl cellulose, 0.4g of nitric acid, 0.3g of tartaric acid and an appropriate amount of deionized water, and extrude it into a granular catalyst with a diameter of 1.5mm;

[0145] (5) The obtained granular catalyst was dried at 120°C for 7 h, and then calcined at 600°C for 4 h. After natural cooling, a hydrotreating catalyst was obtained, which was labeled as AC-3.

[0146] It was measured that the total active metal content of nickel oxide and tungsten oxide in the AC-3 catalyst was 42.0 weight % (based on the total weight of the catalyst), of which the content of the first active metal component (nickel oxide) was 8.0 weight %; the content of the second active metal component (tungsten oxide) was 34.0 weight %; and the carrier content was 58.0 weight %.

[0147] Comparative Example 3

[0148] This comparative example provides a hydrogenation catalyst. This comparative example adopts a preparation method similar to that of Example 3, and the difference from Example 3 is that the biomass C@Al2O3 composite carrier is replaced with a conventional γ-Al2O3 carrier, specifically comprising:

[0149] (1) Take 100 g of pseudo-boehmite, calcine it at 500°C in air atmosphere for 4 h, and then cool it naturally to obtain a γ-Al2O3 carrier.

[0150] (2) 9.34 g of nickel nitrate and 11.86 g of ammonium metatungstate were dissolved in 75.97 g of deionized water to prepare a mixed impregnation solution. The mixed impregnation solution was added dropwise onto 24.51 g of γ-Al2O3 carrier and mixed evenly, then dried at 120°C for 5 hours, and then mixed evenly with 0.7 g of methyl cellulose, 0.4 g of nitric acid, 0.3 g of tartaric acid and an appropriate amount of deionized water, and extruded to form a granular catalyst with a diameter of 1.5 mm;

[0151] (3) The obtained granular catalyst was dried at 120°C for 7 hours, and then calcined at 600°C for 4 hours. After natural cooling, a hydrotreating catalyst was obtained, which was marked as R-3.

[0152] The total content of nickel oxide and tungsten oxide in the R-3 catalyst was measured to be 42.0 wt% (based on the total weight of the catalyst), of which the content of nickel oxide was 8.0 wt%; the content of tungsten oxide was 34.0 wt%; and the content of the carrier was 58.0 wt%.

[0153] Example 4

[0154] This embodiment provides a hydrotreating catalyst, and the specific preparation method includes the following steps:

[0155] Preparation of composite carrier:

[0156] (1) Take appropriate amounts of corn stalks and rice stalks, dry them at 70°C for 24 hours, and then crush them with a pulverizer and sieve them. Take 35g of biomass powder with a particle size of less than 60 mesh after sieving and mix it with 65g of pseudo-boehmite, place it in a ball mill and grind it at a speed of 4000 rpm for 18 hours to obtain a composite carrier precursor with a particle size of less than 200 mesh, wherein the content of the biomass raw material is 35% by weight based on the total weight of the composite carrier precursor; the content of the alumina precursor is 65% by weight;

[0157] (2) drying the composite support precursor at 100° C. for 8 h, and then calcining at 400° C. in a 10 vol% O2 / Ar atmosphere for 5 h, and cooling naturally to obtain a C@Al2O3 composite support intermediate;

[0158] (3) The composite carrier intermediate was placed in a hydrothermal kettle and 124.7 g of deionized water was added dropwise. The hydrothermal kettle was replaced with ammonia gas. The intermediate was hydrothermally treated at 300 °C for 4 h. After natural cooling, the intermediate was dried at 80 °C for 6 h to obtain a biomass C@Al2O3 composite carrier, which was labeled as C-4. The composition of the carrier is listed in Table 1.

[0159] Preparation of catalyst:

[0160] (4) Take 5.83g of cobalt nitrate and 10.67g of ammonium molybdate and dissolve them in 59.40g of deionized water to prepare a mixed impregnation solution. Add the mixed impregnation solution drop by drop onto 19.80g of C@Al2O3 composite carrier and mix them evenly (the weight ratio of the first active metal precursor: the second active metal precursor: the biochar-coated alumina composite carrier is 0.29:0.54:1), then dry at 120°C for 4 hours, and then mix them evenly with 0.7g of polyethylene glycol, 0.4g of nitric acid, 0.3g of citric acid and an appropriate amount of deionized water, and extrude them into strip catalysts with a diameter of 1.5mm;

[0161] (5) The obtained strip catalyst was dried at 120°C for 7 h, and then calcined at 500°C for 4 h. After natural cooling, a hydrotreating catalyst was obtained, which was labeled as AC-4.

[0162] It was measured that the total content of cobalt oxide and molybdenum oxide in the AC-4 catalyst was 34.0 wt% (based on the total weight of the catalyst), of which the content of the first active metal component (cobalt oxide) was 5.0 wt%; the content of the second active metal component (molybdenum oxide) was 29.0 wt%; and the carrier content was 66.0 wt%.

[0163] The scanning electron microscope photo of the biomass C@alumina composite carrier prepared in this example is shown in FIG. Figure 1 As shown by Figure 1 It can be seen that the biochar-coated alumina composite carrier prepared by the method provided in the present application has a large number of "tree root-like" structures (which can also be regarded as "grid" structures).

[0164] Comparative Example 4

[0165] This comparative example provides a hydrogenation catalyst. This comparative example adopts a preparation method similar to that of Example 4, and the difference from Example 4 is that the biomass C@Al2O3 composite carrier is replaced with a conventional γ-Al2O3 carrier, specifically comprising:

[0166] (1) Take 100 g of pseudo-boehmite, calcine it at 500°C in air atmosphere for 4 h, and then cool it naturally to obtain a γ-Al2O3 carrier.

[0167] (2) 5.83 g of cobalt nitrate and 10.67 g of ammonium molybdate were dissolved in 86.45 g of deionized water to prepare a mixed impregnation solution. The mixed impregnation solution was added dropwise onto the 27.89 γ-Al2O3 carrier and mixed evenly, then dried at 120°C for 4 hours, and then mixed evenly with 0.7 g of polyethylene glycol, 0.4 g of nitric acid, 0.3 g of citric acid and an appropriate amount of deionized water, and extruded to form a strip catalyst with a diameter of 1.5 mm;

[0168] (3) The obtained strip catalyst was dried at 120°C for 7 hours, and then calcined at 500°C for 4 hours. After natural cooling, a hydrotreating catalyst was obtained, which was marked as R-4.

[0169] The total content of cobalt oxide and molybdenum oxide in the R-4 catalyst was measured to be 34.0 wt % (based on the total weight of the catalyst), of which the content of cobalt oxide was 5.0 wt %; the content of molybdenum oxide was 29.0 wt %; and the content of the carrier was 66.0 wt %.

[0170] Example 5

[0171] This embodiment provides a hydrotreating catalyst, and the specific preparation method includes the following steps:

[0172] Preparation of composite carrier:

[0173] (1) Take an appropriate amount of rice straw and dry it at 70°C for 24 hours, then crush it with a grinder and sieve it. Take 10g of biomass powder with a particle size of less than 60 mesh after sieving and mix it with 90g of pseudo-boehmite, place it in a ball mill and grind it at a speed of 4000 rpm for 18 hours to obtain a composite carrier precursor with a particle size of less than 200 mesh, wherein the content of the biomass raw material is 10% by weight based on the total weight of the composite carrier precursor; the content of the alumina precursor is 90% by weight;

[0174] (3) drying the composite support precursor at 100° C. for 8 h, and then calcining at 400° C. in a 5 vol% O2 / N2 atmosphere for 5 h, and cooling naturally to obtain a C@Al2O3 composite support intermediate;

[0175] (3) The composite carrier intermediate was placed in a hydrothermal kettle and 145.3 g of deionized water was added dropwise. The hydrothermal kettle was replaced with carbon dioxide. The intermediate was hydrothermally treated at 280 °C for 4 h. After natural cooling, it was dried at 80 °C for 6 h to obtain a biomass C@Al2O3 composite carrier, which was labeled as C-5. The composition of the carrier is listed in Table 1.

[0176] Preparation of catalyst:

[0177] (4) Take 4.67g nickel nitrate, 1.47g molybdenum nitrate and 9.42g ammonium metatungstate and dissolve them in 58.50g deionized water to prepare a mixed impregnation solution. The mixed impregnation solution is added drop by drop onto 19.50g of the above C@Al2O3 composite carrier and mixed evenly (the weight ratio of the first active metal precursor: the second active metal precursor: the biochar-coated alumina composite carrier is 0.24:0.56:1), and then dried at 90°C for 6 hours, and then evenly mixed with 0.6g sesbania powder, 0.4g nitric acid, 0.3g citric acid and an appropriate amount of deionized water, and extruded into a clover-shaped catalyst with a diameter of 1.5mm;

[0178] (5) The obtained cloverleaf-shaped catalyst was dried at 100°C for 8 h, and then calcined at 450°C for 5 h. After natural cooling, a hydrotreating catalyst was obtained, which was labeled as AC-5.

[0179] It was measured that the total content of nickel oxide, molybdenum oxide and tungsten oxide in the AC-5 catalyst was 35.0 weight % (based on the total weight of the catalyst), of which the content of the first active metal component (nickel oxide) was 4.0 weight %; the content of the second active metal component was 31.0 weight % (of which the content of molybdenum oxide was 4.0 weight % and the content of tungsten oxide was 27.0 weight %); and the carrier content was 65.0 weight %.

[0180] Comparative Example 5

[0181] This comparative example provides a hydrogenation catalyst. This comparative example adopts a preparation method similar to that of Example 5, and the difference from Example 5 is that the biomass C@Al2O3 composite carrier is replaced with a conventional γ-Al2O3 carrier, specifically comprising:

[0182] (1) Take 100 g of pseudo-boehmite, calcine it at 500°C in air atmosphere for 4 h, and then cool it naturally to obtain a γ-Al2O3 carrier.

[0183] (2) 4.67 g of nickel nitrate, 1.47 g of molybdenum nitrate and 9.42 g of ammonium metatungstate were dissolved in 85.14 g of deionized water to prepare a mixed impregnation solution. The mixed impregnation solution was added dropwise onto 27.40 g of γ-Al2O3 carrier and mixed evenly, then dried at 90°C for 6 hours, and then mixed evenly with 0.6 g of sesbania powder, 0.4 g of nitric acid, 0.3 g of citric acid and an appropriate amount of deionized water, and extruded to form a clover-shaped catalyst with a diameter of 1.5 mm;

[0184] (3) The obtained cloverleaf-shaped catalyst was dried at 100°C for 8 hours, and then calcined at 450°C for 5 hours. After natural cooling, a hydrotreating catalyst was obtained, which was marked as R-5.

[0185] It was measured that the total content of nickel oxide, molybdenum oxide and tungsten oxide in the R-5 catalyst was 35.0 weight % (based on the total weight of the catalyst), of which the content of nickel oxide was 4.0 weight %; the content of molybdenum oxide was 4.0 weight %; the content of tungsten oxide was 27.0 weight %; and the carrier content was 65.0 weight %.

[0186] Comparative Example 6

[0187] This comparative example refers to the preparation method in Example 1, and the difference from Example 1 is that the quality of raw material addition is changed, specifically including:

[0188] Preparation of composite carrier:

[0189] (1) Take an appropriate amount of wheat straw and dry it at 80°C for 24 hours, then crush it with a grinder and sieve it. Take 70g of biomass powder with a particle size of less than 60 mesh after sieving and mix it with 30g of pseudo-boehmite, place it in a ball mill and grind it at a speed of 5000 rpm for 24 hours to obtain a composite carrier precursor with a particle size of less than 200 mesh, wherein the content of the biomass raw material is 70% by weight based on the total weight of the composite carrier precursor; the content of the alumina precursor is 30% by weight.

[0190] (2) The composite support precursor was dried at 100°C for 6 h, and then calcined at 500°C in a 10 vol% O2 / Ar atmosphere for 5 h. After natural cooling, a C@Al2O3 composite support intermediate was obtained.

[0191] (3) The composite carrier intermediate was placed in a hydrothermal kettle and 115.6 g of deionized water was added dropwise. The hydrothermal kettle was replaced with nitrogen. The intermediate was hydrothermally treated at 200 °C for 4 h. After natural cooling, the intermediate was dried at 80 °C for 6 h to obtain a biomass C@Al2O3 composite carrier, which was labeled as DC-6. The composition of the carrier is listed in Table 1.

[0192] Preparation of catalyst:

[0193] (4) 1.17 g of nickel nitrate and 5.23 g of ammonium metatungstate were dissolved in 88.73 g of deionized water to prepare a mixed impregnation solution. The mixed impregnation solution was dripped onto 25.20 g of the above C@Al2O3 composite carrier powder and mixed evenly (the weight ratio of the first active metal precursor: the second active metal precursor: the biochar-coated alumina composite carrier was 0.046:0.21:1), then dried at 100°C for 8 hours, and then evenly mixed with 0.5 g of Tianqing powder, 0.4 g of nitric acid, 0.6 g of citric acid and an appropriate amount of deionized water, and extruded into a clover-shaped catalyst with a diameter of 1.5 mm.

[0194] (5) The obtained cloverleaf-shaped catalyst was dried at 80°C for 12 h, and then calcined at 500°C for 4 h. After natural cooling, a hydrotreating catalyst was obtained, which was labeled as R-6.

[0195] It was measured that the total content of active metal components of nickel oxide and tungsten oxide in the R-6 catalyst was 16.0 wt% (based on the total weight of the catalyst), of which the content of nickel oxide was 1.0 wt%; the content of tungsten oxide was 15.0 wt%; and the content of the carrier was 84.0 wt%.

[0196] Comparative Example 7

[0197] This comparative example refers to the preparation method in Example 1, and the difference from Example 1 is that the preparation conditions are changed, specifically including:

[0198] The first calcination temperature is 200°C and the calcination time is 10h;

[0199] The temperature of the hydrothermal reaction was 450 °C and the hydrothermal time was 1 h;

[0200] The second calcination temperature is 200°C and the calcination time is 8h;

[0201] The rest of the process is the same as in Example 1. The obtained carrier is marked as DC-7, and the obtained hydrotreating catalyst is marked as R-7.

[0202] The biomass char content, alumina content, total acid content measured by 150°C pyridine infrared and BET specific surface area data of the carrier products (biomass C@Al2O3 composite carrier and conventional γ-Al2O3 carrier) obtained in the above examples and comparative examples are listed in the following Table 1.

[0203] Table 1

[0204]

[0205] From Table 1 above, we can see that:

[0206] Compared with the conventional γ-Al2O3 carriers obtained by calcining pseudo-boehmite in Comparative Examples 1 to 5, the biomass C@Al2O3 composite carriers C-1 to C-5 prepared by the method provided in the present disclosure have higher BET specific surface areas and lower total acid content;

[0207] Compared with Comparative Examples 6 to 7, the biomass C@Al2O3 composite supports C-1 to C-5 have both high BET specific surface area and appropriate acid content.

[0208] Reaction test case

[0209] This test example provides a test experiment of using the catalysts prepared in the above examples and comparative examples to perform hydrogenation treatment on coked diesel.

[0210] The catalysts of the examples and comparative examples with the same active metal content were compared, and the reaction process was as follows: they were pre-sulfurized before application to give the catalyst a better hydrogenation effect. The pre-sulfurization was carried out using a 10mL high-temperature and high-pressure hydrogenation micro-reactor, which was a wet in-situ pre-sulfurization, i.e., wet pre-sulfurization was used, and the catalyst was not unloaded after pre-sulfurization, and the hydrogenation reaction continued directly in the reactor. The pre-sulfurized oil was a n-decane solution containing 5 wt% CS2, the pre-sulfurization temperature was 320°C, the pressure was 4MPa, and the liquid hourly space velocity was 1.5h -1 , the hydrogen to oil volume ratio is 300.

[0211] The hydroprocessing of this test example was carried out using a 10mL high temperature and high pressure hydroprocessing microreactor. The raw material used for evaluation was Daqing coking diesel, which has a specific gravity (d4 20 ) is 0.8274, sulfur content is 1104ppm, and total nitrogen content is 924ppm. The raw materials are pumped in by a plunger pump. The oil sample after reaction is cooled in a high separator and collected and analyzed in a low separator. The temperature of the hydrotreating is 300℃, the pressure is 4MPa, and the liquid hourly space velocity (mass space velocity) is 5.0h -1 , the volume ratio of hydrogen to oil is 500. Under the condition of the same active metal content, the evaluation results of the hydrogenation catalyst are shown in Table 2.

[0212] The sulfur and nitrogen contents of the reactants and products were tested by ultraviolet fluorescence detection and chemiluminescence detection methods.

[0213] Desulfurization rate (mol%) = (raw material sulfur content - product sulfur content) / raw material sulfur content × 100%;

[0214] Denitrification rate (mol %) = (nitrogen content of raw material - nitrogen content of product) / nitrogen content of raw material × 100%.

[0215] Table 2

[0216]

[0217]

[0218] From the data in Table 2, it can be seen that compared with the catalysts R1 to R5 in Comparative Examples 1 to 5 using the traditional γ-Al2O3 as the carrier, the catalysts AC-1 to AC-5 prepared using the biomass C@Al2O3 composite carrier exhibited better desulfurization and denitrification activities. This is mainly because the introduction of biomass carbon effectively modified the surface properties of the carrier Al2O3, increased the BET specific surface area of ​​the carrier, and formed many "root-like" species on the carrier surface (see Figure 1), so that the active metal can be better dispersed on the surface of the carrier. At the same time, the biochar covers some of the -OH sites on the surface of Al2O3, making the catalyst have a suitable acid site distribution (the specific acid value of the carrier is listed in Table 1), which helps to reduce the interaction between the active metal and the carrier and improve the reduction performance of the catalyst. Under the dual effect of the two, the catalyst activity is finally improved.

[0219] In the preparation process of Comparative Example 6, the raw material addition ratio (for example, the content of biomass raw material and alumina precursor in the total weight of the composite carrier precursor; the weight ratio of the first active metal precursor: the second active metal precursor: the biomass carbon-coated alumina composite carrier) is not within the ratio specified in the embodiment of the present disclosure, and the composition of the carrier and the active metal component in the prepared catalyst is also not within the range of "the hydrorefining catalyst includes 40 to 80 weight% of the carrier and 18 to 50 weight% of the active metal component". The desulfurization rate and denitrification rate of catalyst R-6 are lower than those of catalysts AC-1 to AC-5, indicating that the catalyst prepared by the method provided by the present disclosure has better desulfurization and denitrification effects;

[0220] The preparation conditions of Comparative Example 7 during the preparation process (such as the conditions of the first calcination, the hydrothermal reaction, and the second calcination) are not within the scope provided in the embodiments of the present disclosure. The desulfurization rate and denitrification rate of the obtained catalyst R-7 are lower than those of the catalysts AC-1 to AC-5, indicating that the desulfurization and denitrification effects of the catalyst prepared by the method provided in the present disclosure are better.

[0221] The present disclosure is not limited to the specific details of the above-mentioned embodiments. Within the technical concept of the present disclosure, a variety of simple modifications can be made to the technical solution of the present disclosure, and these simple modifications all belong to the protection scope of the present disclosure.

[0222] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present disclosure will not further describe various possible combinations.

[0223] In addition, various embodiments of the present disclosure may be arbitrarily combined, and as long as they do not violate the concept of the present disclosure, they should also be regarded as the contents disclosed by the present disclosure.

Claims

1. A hydrotreating catalyst, characterized in that: Based on the total weight of the hydrotreating catalyst, the hydrotreating catalyst includes 40 to 80 weight percent of a carrier and 18 to 50 weight percent of an active metal component, wherein the active metal component is in the form of a metal oxide; the carrier includes a biomass carbon-coated alumina composite carrier; the active metal component includes a first active metal component and a second active metal component, wherein the first active metal component is selected from one or more of the metal elements of Group VIII; and the second active metal component is selected from one or more of the metal elements of Group VIB.

2. The hydrotreating catalyst according to claim 1, characterized in that Based on the total weight of the carrier, the carrier comprises 0.1 to 10 weight percent of biochar and 90 to 99.9 weight percent of alumina; Optionally, based on the total weight of the hydrotreating catalyst, the content of the first active metal component in the form of oxide is 3 to 10 wt %; the content of the second active metal component is 15 to 40 wt %.

3. The hydrotreating catalyst according to claim 1, characterized in that The total acid content of the biomass carbon-coated alumina composite carrier measured by pyridine infrared is 100-200 μmol / g, and the BET specific surface area of ​​the biomass carbon-coated alumina composite carrier is 300-450 m 2 / g.

4. The hydrotreating catalyst according to claim 1, characterized in that The first active metal component is selected from one or both of Ni and Co; the second active metal component is selected from one or both of Mo and W.

5. A method for preparing a biomass carbon-coated alumina composite carrier, characterized in that: The following steps are involved: S1, mixing the biomass raw material with the alumina precursor to obtain a composite carrier precursor; S2, subjecting the composite carrier precursor to a first calcination treatment to obtain a composite carrier intermediate; S3, subjecting the composite carrier intermediate to hydrothermal treatment.

6. The method according to claim 5, characterized in that In step S1, based on the total weight of the composite carrier precursor, the content of the biomass raw material is 5 to 40% by weight; and the content of the alumina precursor is 60 to 95% by weight.

7. The method according to claim 5, characterized in that In step S1, the biomass raw material is selected from one or more of corn stalks, wheat stalks, rice stalks and sorghum stalks; The aluminum oxide precursor is selected from one or more of pseudo-boehmite, aluminum hydroxide and aluminum nitrate; preferably pseudo-boehmite.

8. The method according to claim 5, characterized in that The method further includes: The biomass raw material is subjected to a first drying treatment, a crushing treatment, and a sieving treatment to obtain a biomass powder with a particle size of less than 60 meshes, and then mixed with the alumina precursor and ground to a particle size of less than 200 meshes to obtain a composite carrier precursor; Optionally, the conditions of the first drying treatment include: drying at 60 to 150° C. for 12 to 36 hours; Optionally, the grinding treatment conditions include: grinding at 1000-10000 r / min for 12-36 hours.

9. The method according to claim 5, characterized in that In step S2, the conditions of the first calcination treatment include: a calcination temperature of 300 to 700° C., a calcination time of 3 to 8 hours; a calcination atmosphere of one or more of air, nitrogen, oxygen, argon and water vapor; Preferably, before the first calcination treatment, the composite carrier precursor is dried at 60 to 150° C. for 4 to 15 hours.

10. The method according to claim 5, characterized in that In step S3, the conditions of the hydrothermal treatment include: a hydrothermal temperature of 150 to 350° C., a hydrothermal time of 2 to 8 hours, and an atmosphere of the hydrothermal treatment selected from one or more of oxygen, nitrogen, ammonia and carbon dioxide; Preferably, step S3 further comprises: adding deionized water dropwise to the composite carrier intermediate until it reaches a saturated water absorption state, and then performing the hydrothermal treatment; Optionally, the method further comprises: cooling the hydrothermal treatment product and drying it at 60 to 150° C. for 4 to 15 hours.

11. A biomass carbon-coated alumina composite carrier prepared according to the method of any one of claims 5 to 10.

12. A method for preparing a hydrotreating catalyst, characterized in that: The following steps are involved: An active metal precursor, a carrier and an additive are mixed, and then subjected to a molding treatment and a second calcination treatment; wherein the carrier comprises the biochar-coated alumina composite carrier described in claim 11; wherein the active metal precursor comprises a first active metal precursor and a second active metal precursor; the first active metal precursor is selected from one or more of the Group VIII metal precursors; the second active metal precursor is selected from one or more of the Group VIB metal precursors.

13. The method according to claim 12, characterized in that The method comprises: impregnating a solution of an active metal precursor with a carrier; Optionally, the first active metal precursor is selected from one or more of a nickel metal precursor and a cobalt metal precursor; preferably, the nickel metal precursor is selected from one or more of nickel nitrate, basic nickel carbonate and nickel sulfate, preferably basic nickel carbonate and / or nickel nitrate; the cobalt metal precursor is selected from one or more of cobalt sulfate, cobalt carbonate, cobalt oxalate and cobalt nitrate, preferably cobalt nitrate and / or cobalt oxalate; The second active metal precursor is selected from one or more of a molybdenum metal precursor and a tungsten metal precursor; preferably, the molybdenum metal precursor is selected from one or more of sodium molybdate, ammonium molybdate, molybdenum chloride and molybdic acid, preferably ammonium molybdate; the tungsten metal precursor is selected from one or more of ammonium metatungstate, phosphotungstic acid and silicotungstic acid, preferably ammonium metatungstate and / or phosphotungstic acid; Preferably, the weight ratio of the first active metal precursor: the second active metal precursor: the biomass carbon-coated alumina composite carrier is 0.2-0.6:0.3-0.7:

1.

14. The method according to claim 12, characterized in that The conditions of the second calcination treatment include: a calcination temperature of 300-600°C, a calcination time of 3-6 hours; a calcination atmosphere of one or more of air, nitrogen, oxygen, argon and water vapor; optionally, before the second calcination treatment, the product obtained by the molding treatment is dried at 80-160°C for 4-12 hours.

15. A hydrotreating catalyst prepared according to the method according to any one of claims 12 to 14.

16. Use of the hydrotreating catalyst according to any one of claims 1 to 4 and claim 15 in a hydrotreating reaction of crude oil.

17. The use according to claim 16, characterized in that The following steps are involved: Under hydrogenation conditions, the crude oil is brought into contact with the hydrotreating catalyst to perform a hydrotreating reaction; Optionally, the conditions of the hydrofining reaction include: reaction temperature of 260-380°C; hydrogen pressure of 2-10 MPa; hydrogen-oil volume ratio of 200-800:1; feed oil mass space velocity of 0.5-6h -1 ; Optionally, the feedstock oil is selected from gasoline and / or diesel fractions; Preferably, the method further comprises: performing a sulfidation treatment on the hydrotreating catalyst before carrying out the hydrotreating reaction.