TiO2 / SC catalyst, preparation method thereof and application of TiO2 / SC catalyst in desulfurization
By preparing TiO2/SC catalyst with FCC oil slurry and TiO2, combined with heteropoly acid loading, the problem of difficult use of FCC oil slurry is solved, low-cost and efficient desulfurization effect is achieved, environmental pollution is reduced, and sustainable development requirements are met. .
Patent Information
- Application Number
- CN202411195805.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-11-12
AI Technical Summary
As a by-product of petroleum catalytic cracking process, FCC oil slurry is difficult to be effectively utilized, resulting in scaling and coking of catalytic cracking devices, reducing production efficiency and affecting product quality, and environmental pollution problems.
The TiO2/SC catalyst is prepared by using FCC oil slurry and TiO2 as the main raw materials, and is used for desulfurization of oil by calcining and grinding, combined with heteropoly acid support, so as to achieve low cost and good desulfurization performance.
It effectively exerts the surplus value of FCC oil slurry, reduces the production cost of desulfurization catalysts, reduces environmental pollution, and improves the oxidative and desulfurization effect of the catalysts, which is in line with the sustainable development strategy.
Smart Images

Figure CN118925765A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of heavy oil slurry treatment, and specifically relates to a TiO2 / SC catalyst and a preparation method thereof and application in desulfurization. Background Art
[0002] FCC slurry refers to a mixture of solid catalyst and liquid raw materials produced in the process of catalytic cracking (FCC). FCC slurry is the fraction at the bottom of the catalytic cracking fractionation tower and is a by-product of the catalytic cracking process.
[0003] At present, my country's chemical companies mainly use catalytic cracking units to feed heavy petroleum fractions (such as residual oil) together with catalysts into catalytic cracking units. Under high temperature and high pressure and the action of catalysts, heavy oil is converted into lighter petroleum products such as diesel, gasoline and liquefied petroleum gas, resulting in an increase in FCC slurry oil year by year. Studies have shown that my country's current FCC slurry oil production capacity is approximately 4 million tons to 5 million tons. The production of a large amount of FCC slurry oil will have an adverse effect on the catalytic cracking unit. Since crude oil contains heavy metals, S, N and other elements, it will cause scaling and coking of the catalytic cracking unit, reduce production efficiency, and affect the quality of the products produced by the catalytic cracking unit. Therefore, how to recycle FCC slurry oil in a more environmentally friendly way is crucial to the sustainable development of the refining industry.
[0004] Therefore, the present invention hopes to use FCC oil slurry as the main raw material to prepare a carbonized material with good catalytic desulfurization performance, thereby achieving effective resource utilization of FCC oil slurry materials and reducing environmental pollution. Summary of the invention
[0005] The present invention aims to solve at least one of the technical problems existing in the above-mentioned prior art. To this end, the present invention provides a TiO2 / SC catalyst and a preparation method thereof and application in desulfurization. The catalyst is prepared with FCC slurry oil and TiO2 as main raw materials, and heteropoly acid can be loaded on this basis. It is applied to oil desulfurization, has the characteristics of low cost and good desulfurization performance, effectively realizes effective resource utilization of FCC slurry oil materials and reduces environmental pollution.
[0006] The present invention provides a method for preparing a TiO2 / SC catalyst, comprising the following steps: (1) The FCC oil slurry is filtered and dried to obtain an oil slurry filter cake; (2) The oil slurry filter cake is mixed with TiO2, calcined, ground and pulverized to obtain a TiO2 / SC catalyst.
[0007] In step (2), calcination is performed in a carbonization furnace, and grinding is performed after calcination to improve the oxidative desulfurization effect of the catalyst.
[0008] Preferably, the mass ratio of the oil slurry filter cake to TiO2 in step (2) is (0.5-3):1.
[0009] More preferably, the mass ratio of the oil slurry filter cake to TiO2 in step (2) is 2: 1. Experiments show that the catalyst prepared with the mass ratio of the oil slurry filter cake to TiO2 of 2: 1 has a better desulfurization effect.
[0010] Preferably, the calcination step in step (3) is: heating to 550-700°C at a heating rate of 6-8°C and keeping the temperature for 80-150 minutes.
[0011] The present invention also provides a TiO2 / SC catalyst prepared by the above preparation method.
[0012] The present invention also provides a heteropoly acid / TiO2 / SC catalyst, which is prepared by nitrating the above TiO2 / SC catalyst and then loading the heteropoly acid.
[0013] Preferably, the nitration treatment method is: soaking the TiO2 / SC catalyst in nitric acid, and then drying it to complete the nitration treatment.
[0014] After being corroded by nitric acid, the internal pores of the TiO2 / SC catalyst are opened, so that the heteropoly acid can be better loaded on the TiO2 / SC catalyst, increasing the desulfurization effect of the catalyst.
[0015] Preferably, the heteropoly acid is selected from at least one of phosphomolybdic acid and phosphotungstic acid.
[0016] More preferably, the heteropolyacid is phosphomolybdic acid.
[0017] Preferably, the heteropolyacid is loaded by an impregnation method.
[0018] The present invention also provides the use of the TiO2 / SC catalyst or heteropolyacid / TiO2 / SC catalyst in desulfurization.
[0019] Preferably, the desulfurization is oil product desulfurization. Specifically, the oil product desulfurization can be fuel oil desulfurization.
[0020] Compared with the prior art, the beneficial effects of the present invention are as follows: FCC slurry oil is a low value-added product produced in the process of petroleum catalytic cracking, and it is difficult to be effectively utilized at present. The present invention uses FCC slurry oil as the main raw material and finally prepares a catalyst product with good desulfurization performance, which not only effectively exerts the residual value of FCC slurry oil and reduces the production cost of desulfurization catalyst, but also helps reduce environmental pollution, conforms to my country's sustainable development strategy, and has important practical significance. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 The following are Fourier transform infrared spectra of the catalysts prepared in Example 2 and Example 4.
[0022] Figure 2 The X-ray diffraction patterns of the catalysts prepared in Example 2 and Example 4 are shown.
[0023] Figure 3 Scanning electron microscope images of the catalyst prepared in Example 2 at magnifications of 2000 times and 5000 times.
[0024] Figure 4 Scanning electron microscope images of the catalyst prepared in Example 4 at magnifications of 2000 times and 5000 times.
[0025] Figure 5 The results are for the thermal catalytic oxidation desulfurization rates of the catalysts prepared in Examples 1-3. DETAILED DESCRIPTION
[0026] In order to make the technical scheme of the present invention more clearly understood by those skilled in the art, the following embodiments are listed for illustration. It should be pointed out that the following embodiments do not limit the protection scope of the present invention.
[0027] Unless otherwise specified, the raw materials, reagents or devices used in the following examples can be obtained from conventional commercial sources or by existing known methods. Example
[0028] This embodiment provides a TiO2 / SC catalyst (named as 50% TiO2 / SC), and the preparation method thereof comprises the following steps: (1) Heat the FCC oil slurry to 120°C and stir it, then use a suction filtration bottle and a Buchner funnel to filter it. After the filtration is completed, the black solid on the Buchner funnel is the oil slurry filter cake.
[0029] (2) Place the empty quartz tube in a tube furnace and set the heating program to heat to 700°C at a heating rate of 6°C / min, keep it warm for 10 minutes, and then cool it to room temperature for later use.
[0030] (3) The oil slurry filter cake was mixed with TiO2 in a mass ratio of 1:1, mixed evenly on a porcelain boat, and then placed in an air-fired quartz tube. The mixture was placed in a tube furnace and heated to 600°C at a rate of 7°C / min and kept warm for 100 min. The mixture was cooled to room temperature and ground into powder to obtain a 50% TiO2 / SC catalyst. Example
[0031] This embodiment provides a TiO2 / SC catalyst (named as 33% TiO2 / SC), and the preparation method thereof comprises the following steps: (1) Heat the FCC oil slurry to 120°C and stir it, then use a suction filtration bottle and a Buchner funnel to filter it. After the filtration is completed, the black solid on the Buchner funnel is the oil slurry filter cake.
[0032] (2) Place the empty quartz tube in a tube furnace and set the heating program to heat to 700°C at a heating rate of 6°C / min, keep it warm for 10 minutes, and then cool it to room temperature for later use.
[0033] (3) The oil slurry filter cake was mixed with TiO2 in a mass ratio of 2:1, mixed evenly on a porcelain boat, and then placed in an air-fired quartz tube. The mixture was placed in a tube furnace and heated to 600°C at a rate of 7°C / min and kept at this temperature for 100 min. The mixture was cooled to room temperature and ground into powder to obtain a 33% TiO2 / SC catalyst. Example
[0034] This embodiment provides a TiO2 / SC catalyst (named as 66% TiO2 / SC), and the preparation method thereof comprises the following steps: (1) Heat the FCC oil slurry to 120°C and stir it, then use a suction filtration bottle and a Buchner funnel to filter it. After the filtration is completed, the black solid on the Buchner funnel is the oil slurry filter cake.
[0035] (2) Place the empty quartz tube in a tube furnace and set the heating program to heat to 700°C at a heating rate of 6°C / min, keep it warm for 10 minutes, and then cool it to room temperature for later use.
[0036] (3) The oil slurry filter cake was mixed with TiO2 in a mass ratio of 1:2, placed on a porcelain boat and mixed evenly, then placed in an air-fired quartz tube, placed in a tube furnace and calcined at a heating rate of 7°C / min to 600°C, and kept warm for 100 min; cooled to room temperature, ground into powder, and a 66% TiO2 / SC catalyst was obtained. Example
[0037] This embodiment provides a heteropolyacid / TiO2 / SC catalyst (named HPMo / TiO2 / SC (nitration)), the preparation method of which comprises the following steps: (1) Take 0.8643 g of 33% TiO2 / SC prepared in Example 2, add it to 1 mol / L nitric acid solution and soak it at room temperature for 2 h (nitration treatment), and then dry it at 120°C for 5 h.
[0038] (2) Weigh 0.3451 g of phosphomolybdic acid hydrate into a beaker, add 30 mL of ultrapure water, place the beaker in an ultrasonic environment at 50 ° C for dispersion for 2 h, then add 33% TiO2 / SC treated with nitration in step (1) for impregnation, stir magnetically at room temperature for 24 h, dry at 120 ° C, and grind to obtain 0.8024 g HPMo / TiO2 / SC (nitration) catalyst.
[0039] Product features and performance testing 1. Fourier Transform Infrared Spectroscopy (FT-IR) The catalysts prepared in Example 2 and Example 4 were characterized and analyzed by Fourier transform infrared spectroscopy (FT-IR). Figure 1 shown.
[0040] from Figure 1 It can be seen that the catalysts have -1 The C=C skeleton vibration peak of the benzene ring can be observed nearby, which is one of the characteristic vibrations of aromatic ring structures such as benzene rings. The Ti-O bond vibration is at 1000~400 cm -1 In the range of 480–700 cm -1 The presence of vibration mode absorption peaks proves that these two catalyst materials contain TiO2 added before calcination. HPMo / TiO2 / SC (nitration) catalyst has a peak at 1059 cm -1 (Stretching frequency of PO in PO4 tetrahedron at HPMo center), 958 cm -1 (Mo=O band at the end of the MoO6 outer octahedron) and 786cm -1 The appearance of characteristic absorption peaks (Mo-O-Mo band) indicates that the phosphomolybdic acid on the surface of the HPMo / TiO2 / SC (nitration) catalyst is not destroyed, and after being corroded by nitric acid, the phosphomolybdic acid can be better loaded on the catalyst.
[0041] 2. X-ray diffraction (XRD) The catalysts prepared in Example 2 and Example 4 were characterized and analyzed by X-ray diffraction (XRD). Figure 2 shown.
[0042] from Figure 2It can be seen that the characteristic peak of the anatase phase usually appears at about 25.3° at 2θ, and the characteristic peak of the rutile phase appears at about 25° and 54.3° at 2θ. The prepared HPMo / TiO2 / SC (nitration) catalyst and TiO2 / SC catalyst both have diffraction peaks at 27° and 54° at 2θ. At the same time, the diffraction peak of the MoO3 unit appears in the range of 25°-30° in HPMo / TiO2 / SC (nitration), indicating that after the nitration treatment of HPMo / TiO2 / SC (nitration), the phosphomolybdic acid clusters can be well dispersed on the carrier.
[0043] 3. Scanning Electron Microscope Image (SEM) The catalysts prepared in Example 2 and Example 4 were characterized and analyzed by scanning electron microscopy (SEM), with the accelerating voltage of the SEM being 15 KV. Figure 3-4 shown.
[0044] Depend on Figure 3-4 It can be seen that the surface roughness of the two catalyst materials is relatively high. Figure 3 It can be seen that the TiO2 / SC catalyst can clearly see a nearly spherical structure, and each spherical structure is relatively dispersed. Figure 4 It can be seen that the HPMo / TiO2 / SC (nitration) catalyst has a smaller particle size, a highly dispersed structure, and uneven structures between carbon materials, which can better load phosphomolybdic acid in the pores, thereby enhancing the activity of the catalyst and increasing the desulfurization rate.
[0045] 4. Desulfurization performance test (1) Preparation of simulated oil (n-decane / tetradecane) Use a pipette to take 10 mL of tetradecane and add it to a 500 mL volumetric flask, then add 1.4395 g of solid DBT, and after it is fully dissolved, add n-decane. After adding n-decane, when the liquid level is 1-2 cm away from the scale line, use a rubber-tipped dropper to draw n-decane until the concave part of the liquid surface is tangent to the scale line. Make a fixed volume to prepare 500 mL of simulated oil (n-decane / tetradecane) with a sulfur content of 500 μg / g DBT.
[0046] (2) Thermal catalytic oxidation desulfurization detection process The prepared 500 μg / g DBT simulated oil was used as the reagent, the experimental conditions were 10 mL of simulated oil, 5 mL of acetonitrile as the extractant, 0.06 g of catalyst, the reaction temperature was set to a constant temperature of 60°C, and the reaction time was 90°C.
[0047] Before the experiment, turn on the switch of the constant temperature water bath, adjust it to 60℃, set the time and set it aside. Use a pipette to take 10mL of simulated oil and inject it into a cleaned and dried three-necked flask. Then add 5ml of acetonitrile as an extractant, add a magnetic particle, and after connecting to 60℃ circulating water and a condenser, turn on the switch of the magnetic stirrer and adjust the speed appropriately. When the reaction reaches the 10th minute, add 0.06g of catalyst and 0.12mL of 30% H2O2 (as an oxidant) in sequence, and start timing. The experiment was carried out under the conditions of 60℃ circulating water and magnetic stirring, and condensation reflux.
[0048] The experiment takes samples every 15 minutes, that is, at 15 minutes, 30 minutes, 45 minutes, 60 minutes, 75 minutes, and 90 minutes, stop the magnetic stirring, use the sampling needle to take about 0.05 mL of the upper clear liquid in the three-necked flask into the capillary tube that has been fired in advance, and cover it with a rubber sleeve. Labels should be affixed after each sampling to prevent confusion. After the experiment is completed, the capillary tube with the sample is placed in a centrifuge tube, and the centrifuge tube is balanced and placed in the centrifuge to adjust the speed and time. The sample after centrifugation is tested by gas chromatograph to detect the content of each part of the sample, and the desulfurization rate is calculated.
[0049] Calculation of desulfurization rate After the desulfurization reaction, the sample was centrifuged and analyzed on an Agilent Technologies 7820A machine to obtain the peak area of each component, which can be calculated by the following formula: Desulfurization rate = (1-C A / C0)×100% Where C0 is the initial sulfur concentration of the simulated oil, mg / L; C A is the sulfur concentration of the oil sample after the reaction, mg / L.
[0050] The catalysts prepared in Examples 1-3 and the TiO2 catalyst were respectively used to carry out thermal catalytic oxidation desulfurization tests.
[0051] Depend on Figure 5It can be seen that under the same conditions, the desulfurization rate of 33% TiO2 / SC catalyst (the mixing ratio of oil filter cake and TiO2 is 2:1) increased from 61.6% at 15min to 76.0% at 90min. Its desulfurization effect is better than that of 66% TiO2 / SC catalyst (the mixing ratio of oil filter cake and TiO2 is 1:2) and 50% TiO2 / SC catalyst (the mixing ratio of oil filter cake and TiO2 is 1:1), and is also higher than that of conventional TiO2 catalyst. This result shows that when TiO2 is mixed with oil filter cake and calcined, increasing the proportion of oil filter cake or TiO2 can enhance the catalytic effect, but the current optimal ratio is to prepare the catalyst by mixing oil filter cake and TiO2 in a ratio of 2:1. However, when oil filter cake and TiO2 are mixed and calcined in equal proportions, the effect of the catalyst will be reduced, which will reduce the desulfurization effect.
[0052] The catalyst prepared in Example 4 was further tested for thermal catalytic oxidation desulfurization. The results showed that as the reaction time increased, the desulfurization rate of the HPMo / TiO2 / SC catalyst increased from 38.7% at 15 min to 78.4% at 90 min. This result shows that the addition of the nitration step and then the loading of phosphomolybdic acid enhances the desulfurization effect of the catalyst.
[0053] 5. Calculation of production raw material cost Raw material cost: FCC oil slurry costs about 4,000 yuan / ton; TiO2 costs about 50,000 yuan / ton. Calculated based on the 33% TiO2 / SC catalyst in production example 2, the mass ratio of oil slurry filter cake to TiO2 added is 2:1, and the catalyst yield is about 65%. After conversion, when producing 1 ton of 33% TiO2 / SC catalyst, the raw material cost is only 29,743.6 yuan, which is economical.
[0054] The embodiments of the present application are described in detail above in conjunction with the accompanying drawings, but the present application is not limited to the above embodiments, and various changes can be made within the knowledge scope of ordinary technicians in the relevant technical field without departing from the purpose of the present application.
Claims
1. A method for preparing a TiO2 / SC catalyst, characterized in that: The following steps are involved: (1) The FCC oil slurry is filtered and dried to obtain an oil slurry filter cake; (2) The oil slurry filter cake is mixed with TiO2, calcined, ground and pulverized to obtain a TiO2 / SC catalyst.
2. The preparation method according to claim 1, characterized in that: The mass ratio of the oil slurry filter cake to TiO2 in step (2) is (0.5-3):1; preferably, the mass ratio of the oil slurry filter cake to TiO2 in step (2) is 2:
1.
3. The preparation method according to claim 1, characterized in that: The calcination step in step (3) is as follows: heating to 550-700°C at a heating rate of 6-8°C and keeping the temperature for 80-150 minutes.
4. A TiO2 / SC catalyst, characterized in that: Prepared by the preparation method described in any one of claims 1 to 3.
5. A heteropolyacid / TiO2 / SC catalyst, characterized in that: The catalyst is prepared by nitrating the TiO2 / SC catalyst as claimed in claim 4 and then loading a heteropoly acid.
6. The heteropolyacid / TiO2 / SC catalyst according to claim 5, characterized in that The nitration treatment method is: soaking the TiO2 / SC catalyst in nitric acid, and then drying it to complete the nitration treatment.
7. The heteropolyacid / TiO2 / SC catalyst according to claim 5, characterized in that The heteropoly acid is selected from at least one of phosphomolybdic acid and phosphotungstic acid; preferably, the heteropoly acid is phosphomolybdic acid.
8. The heteropolyacid / TiO2 / SC catalyst according to claim 5, characterized in that The heteropoly acid is loaded by an impregnation method.
9. Use of the TiO2 / SC catalyst according to claim 4 or the heteropolyacid / TiO2 / SC catalyst according to any one of claims 5 to 8 in desulfurization.