High-performance Mo-based catalyst, preparation method thereof and application of high-performance Mo-based catalyst in distributed ammonia synthesis

By preparing Mo-based catalysts, regulating the nitriding treatment conditions and pre-reduction temperature, the problem of low ammonia synthesis efficiency of existing catalysts under low temperature and low pressure is solved, and efficient and stable ammonia synthesis is achieved, suitable for renewable energy power electrolysis and hydrogen production by hydrogen system.

CN118925767APending Publication Date: 2024-11-12FUZHOU UNIV

Patent Information

Application Number
CN202310523352.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-10
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

It is difficult for existing catalysts to efficiently synthesize ammonia under low temperature and low pressure conditions, and traditional industrial catalysts are not suitable for renewable energy power electrolysis hydrogen production systems, resulting in low ammonia synthesis efficiency.

Method used

By nitriding and passivating the molybdenum-containing precursor, Mo-based catalyst is prepared, the nitriding treatment conditions and pre-reduction temperature are regulated, and the efficient molybdenum nitride crystal phase is formed to achieve efficient synthesis of ammonia under mild conditions.

Benefits of technology

It realizes efficient synthesis of ammonia under low temperature and low pressure conditions, improves the reaction performance and stability of the catalyst, reduces costs, and the N element in molybdenum nitride directly participates in the reaction cycle, optimizing the catalytic effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118925767A_ABST
    Figure CN118925767A_ABST
Patent Text Reader

Abstract

The invention provides a high-performance Mo-based catalyst, a preparation method thereof and application of the high-performance Mo-based catalyst in distributed ammonia synthesis. The preparation method specifically comprises the following steps: (1) carrying out nitrogen treatment on a molybdenum-containing precursor to obtain a nitride; and (2) passivating the nitride obtained in the step (1) to obtain the Mo-based catalyst. The molybdenum nitride catalyst provided by the invention has excellent ammonia synthesis catalytic performance under mild conditions. As the catalyst does not contain noble metal, the cost of the catalyst can be effectively reduced, the preparation method is relatively simple, the thermal stability is good, and the catalyst has obvious industrial application value.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of catalyst material preparation, and in particular to a high-performance Mo-based catalyst and a preparation method thereof and application thereof in distributed ammonia synthesis. Background Art

[0002] Hydrogen is an ideal green energy source and one of the feasible solutions to the fossil energy crisis. However, there are still key issues that need to be solved for the large-scale promotion and application of hydrogen energy. The "bottleneck" technical difficulty of hydrogen energy storage lies in the storage and transportation of hydrogen. Hydrogen storage and transportation requires a high pressure of 35-70MPa. High-pressure hydrogen is flammable and explosive, and its inherent safety is weak. In addition, the core materials and equipment for high-pressure hydrogen storage mainly rely on imports. Therefore, optimizing the hydrogen source structure and solving the problem of safe storage and transportation of hydrogen energy are the key to realizing the development of the hydrogen energy industry. Ammonia (NH3) is one of the most important bulk chemicals in the world and an efficient hydrogen storage carrier. The development of the "ammonia-hydrogen energy storage" route with NH3 as a hydrogen carrier has unique advantages: first, high energy density: 1L liquid ammonia (2.2MPa) = 2.2L hydrogen (70.0MPa) = 1200L H2 at room temperature and pressure; second, easy liquefaction storage and transportation: NH3 can be stored and transported in liquid form when pressurized to 1.0MPa; third, cross-season carbon-free energy storage: "ammonia-hydrogen energy storage" is the same as "hydrogen energy storage", which can achieve "zero loss" seasonal energy storage and carbon-free energy storage cycle; fourth, high safety: NH3 is not flammable, and its pungent smell is a reliable alarm signal. Therefore, using NH3 as an energy storage carrier and developing a technology that complements and integrates renewable energy power electrolysis hydrogen production and advanced synthetic ammonia technology is one of the most feasible ways to achieve clean and efficient utilization of renewable energy, optimize hydrogen source structure, and safely store and transport hydrogen.

[0003] However, the pressure-type water electrolysis hydrogen production system requires an output pressure of ≤5.0MPa, and the general output pressure is 1.6-3.2MPa. The temperature of the H2 obtained by electrolysis after deep dehydration and deoxygenation is about 400℃. Therefore, in order to achieve the complementary integration of renewable energy power and synthetic ammonia technology, it is urgent to develop ammonia synthesis technology under relatively mild conditions that matches the renewable energy power electrolysis hydrogen production system (reaction conditions: ~400℃, 1.6~3.2MPa). The existing industrial synthetic ammonia catalysts for fossil energy are difficult to meet the requirements under these relatively mild conditions. The design and development of new and efficient low-temperature and low-pressure synthetic ammonia catalysts has become the key to connecting the "renewable energy-ammonia-hydrogen" cycle route.

[0004] In recent years, studies have been conducted to modify the surface morphology of Co, Mo and Ni, add alkaline (earth) metals (K2O, Cs2O or BaO x) to promote the catalytic performance of synthetic ammonia at low temperature and low pressure. However, the catalysts prepared by these modification methods do not break the limiting relationship between activation energy and the bond energy of the intermediate species. Therefore, these catalysts still require higher temperatures (≥400°C) and pressures (~9.0MPa) in the synthetic ammonia reaction. Mo is located on the left side of the "volcano-type" curve. If the intermediate species N in the synthetic ammonia reaction fills the gaps in the Mo metal structure, a Mo with metallic properties, no reaction with water and high stability is formed. x N interstitial compound (interstitial compound: a metal compound formed by transition metal elements and non-metallic elements with smaller atomic radius such as nitrogen and boron). x N interstitial compounds have the characteristics of easy transfer of nitrogen ions / vacancies, electrons / holes, and N species in the bulk phase and abundant surface reaction sites. x The N in the N lattice can also be regenerated by NH3, realizing a chemical chain cycle process centered on the combination of the intermediate species "N", which is expected to achieve efficient synthesis of ammonia under mild conditions. Summary of the invention

[0005] The present invention provides a method for preparing a Mo-based catalyst, comprising the following steps:

[0006] (1) subjecting a molybdenum-containing precursor to a nitriding treatment to obtain a nitride;

[0007] (2) The nitride obtained in step (1) is passivated to obtain the Mo-based catalyst.

[0008] According to an embodiment of the present invention, in step (1), the molybdenum-containing precursor may be first subjected to an oxidation treatment and then to a nitridation treatment.

[0009] Preferably, the oxidation treatment condition is calcination in an oxygen-containing atmosphere. Further, the oxygen-containing atmosphere can be any atmosphere known in the art, such as air. Further, the calcination condition is: calcination temperature is 400-600°C, preferably 500°C; calcination time is 2-10h, preferably 4h.

[0010] According to an embodiment of the present invention, the molybdenum-containing precursor is selected from molybdenum salts and / or molybdenum precipitates.

[0011] According to an embodiment of the present invention, the molybdenum salt is selected from at least one of ammonium molybdate, molybdenum chloride and sodium molybdate, for example, two of them.

[0012] According to an embodiment of the present invention, the molybdenum precipitate is prepared by adding a precipitant to a solution containing a molybdenum salt. Preferably, the molybdenum precipitate may be dried before calcination. Further, the drying conditions include: a drying temperature of 80-120°C, preferably 120°C; a drying time of 8-24h, preferably 12h.

[0013] According to an embodiment of the present invention, the precipitating agent is preferably hexamethylenetetramine.

[0014] According to an embodiment of the present invention, the solution containing molybdenum salt further comprises a solvent, and the solvent is selected from at least one of ethanol, water and tetrahydrofuran, preferably water.

[0015] According to an embodiment of the present invention, in step (1), the nitridation treatment is carried out in a nitrogen-containing atmosphere. Preferably, the nitrogen-containing atmosphere comprises at least nitrogen and / or ammonia, and optionally comprises or does not comprise argon and hydrogen. Preferably, in the nitrogen-containing atmosphere, the volume content of nitrogen and / or ammonia is 1-100 vol%, for example, 1 vol%, 15 vol%. Exemplarily, the nitrogen-containing atmosphere is selected from NH3 and Ar, wherein NH3 is 10 vol%. Exemplarily, the nitrogen-containing atmosphere is selected from N2 and H2, and the volume ratio thereof is 15:85. Exemplarily, the nitrogen-containing atmosphere is selected from NH3.

[0016] According to an embodiment of the present invention, in step (1), the conditions of the nitridation treatment include: the nitridation temperature is 600-900°C, for example, 700°C, 800°C; the nitridation time is 2-12h, for example, 10h.

[0017] According to an embodiment of the present invention, in step (1), the heating rate of the nitridation treatment is 2-10°C min -1 , for example, 5℃ min -1 .

[0018] According to an embodiment of the present invention, in step (2), the passivation treatment is carried out in a passivation gas, and the passivation gas comprises a mixture of oxygen and an inert gas. Preferably, the inert gas is selected from any one of nitrogen, argon, helium, etc., preferably argon. Preferably, in the passivation gas, the volume concentration of oxygen is 0-10 vol%, for example, 1 vol%. Exemplarily, the passivation gas comprises oxygen and argon, and the volume concentration of oxygen is 1 vol%.

[0019] According to an embodiment of the present invention, in step (2), the conditions for the passivation treatment include: the passivation time is 6-12 hours, preferably 6 hours.

[0020] According to an embodiment of the present invention, in step (2), the Mo-based catalyst comprises molybdenum nitride, and the crystal phase of the molybdenum nitride is selected from any one of the following crystal phases: δ-Mo2N, β-Mo2N, and γ-Mo2N. In the present invention, the δ-Mo2N refers to Mo2N in the δ phase, the β-Mo2N refers to Mo2N in the β phase, and the γ-Mo2N refers to Mo2N in the γ phase.

[0021] According to an embodiment of the present invention, the preparation method further comprises: (3) subjecting the Mo-based catalyst to a pre-reduction treatment.

[0022] According to an embodiment of the present invention, after the Mo-based catalyst is pre-reduced, the crystal phase of molybdenum nitride therein does not substantially change.

[0023] According to an embodiment of the present invention, the pre-reduction treatment comprises: subjecting the Mo-based catalyst to a heat treatment in a reducing atmosphere.

[0024] According to an embodiment of the present invention, the reducing atmosphere comprises a mixture of hydrogen and argon, wherein the volume content of hydrogen is 1-10 vol%. Preferably, the reducing atmosphere comprises hydrogen and argon, wherein the volume content of hydrogen is 10 vol%.

[0025] According to an embodiment of the present invention, the temperature of the heat treatment is 300-500°C, for example, 400°C.

[0026] According to an embodiment of the present invention, the heat treatment time is 1-4 hours, for example, 2 hours or 3 hours.

[0027] According to a preferred embodiment of the present invention, the method for preparing the Mo-based catalyst comprises the following steps:

[0028] (A1) uniformly dispersing a molybdenum salt and a precipitant in a solvent, respectively, mixing, and standing for aging to obtain a molybdenum precipitate;

[0029] (A2) subjecting the molybdenum precipitate obtained in step (A1) to nitridation to obtain a nitride;

[0030] (A3) The nitride obtained in step (A2) is passivated to obtain the Mo-based catalyst.

[0031] Preferably, the static aging time is 6-24 hours, preferably 12 hours.

[0032] Preferably, the preparation method further comprises: (A4) subjecting the Mo-based catalyst to a pre-reduction treatment.

[0033] According to a preferred embodiment of the present invention, the method for preparing the Mo-based catalyst comprises the following steps:

[0034] (B1) calcining the molybdenum salt in air to form an oxide;

[0035] (B2) subjecting the oxide obtained in step (B1) to nitridation to obtain a nitride;

[0036] (B3) subjecting the nitride obtained in step (B2) to passivation treatment to obtain the Mo-based catalyst. Preferably, the preparation method further comprises: (B4) subjecting the Mo-based catalyst to a pre-reduction treatment.

[0037] According to an exemplary embodiment of the present invention, the method for preparing the Mo-based catalyst specifically includes:

[0038] (C1) dispersing ammonium molybdate and hexamethylenetetramine in deionized water respectively, mixing, standing for aging, separating and drying to obtain a molybdenum precipitate, and calcining in air to obtain an oxide;

[0039] (C2) the oxide is subjected to nitridation treatment in a mixture of ammonia and argon to obtain a nitride;

[0040] (C3) the nitride in step (C2) is then passivated in a mixture of oxygen and argon to obtain the Mo-based catalyst;

[0041] Wherein, the Mo-based catalyst comprises molybdenum nitride, the crystal phase of molybdenum nitride is γ phase, and its XRD pattern is as follows: Figure 1 As shown in a.

[0042] Preferably, the preparation method further comprises: (C4) subjecting the Mo-based catalyst to a pre-reduction treatment.

[0043] According to an exemplary embodiment of the present invention, the method for preparing the molybdenum nitride catalyst specifically includes:

[0044] (D1) Plating platinum chloride in ammonia gas and subjecting it to nitridation treatment to obtain a nitride;

[0045] (D2) passivating the nitride in step (1) in a mixed gas of oxygen and argon to obtain the Mo-based catalyst;

[0046] Wherein, the Mo-based catalyst comprises molybdenum nitride, the crystal phase of the molybdenum nitride is δ phase, and its XRD pattern is as follows: Figure 1 As shown in b.

[0047] Preferably, the preparation method further comprises: (D3) subjecting the Mo-based catalyst to a pre-reduction treatment.

[0048] According to an exemplary embodiment of the present invention, the method for preparing the molybdenum nitride catalyst specifically includes:

[0049] (E1) calcining ammonium molybdate in air to obtain an oxide;

[0050] (E2) the oxide is subjected to nitridation treatment in a mixture of ammonia and argon to obtain a nitride;

[0051] (E3) the nitride in step (E2) is then passivated in a mixture of oxygen and argon to obtain the Mo-based catalyst;

[0052] Wherein, the Mo-based catalyst comprises molybdenum nitride, the crystal phase of the molybdenum nitride is β phase, and its XRD pattern is as follows: Figure 1 As shown in c.

[0053] Preferably, the preparation method further comprises: (E4) subjecting the Mo-based catalyst to a pre-reduction treatment.

[0054] The present invention also provides a Mo-based catalyst, which is obtained by the above-mentioned preparation method.

[0055] According to an embodiment of the present invention, the Mo-based catalyst includes molybdenum nitride, and the molybdenum nitride is crystalline.

[0056] According to an embodiment of the present invention, in the Mo-based catalyst, the crystal phase of the molybdenum nitride crystal is selected from at least one of δ-Mo2N, β-Mo2N, and γ-Mo2N.

[0057] According to an exemplary embodiment of the present invention, the crystal of molybdenum nitride is selected from δ-Mo2N.

[0058] According to an exemplary embodiment of the present invention, the molybdenum nitride crystal is selected from β-Mo2N.

[0059] According to an exemplary embodiment of the present invention, the molybdenum nitride crystal is selected from γ-Mo2N.

[0060] The present invention also provides the use of the Mo-based catalyst, preferably the use in ammonia synthesis, more preferably the use in distributed ammonia synthesis.

[0061] Beneficial Effects

[0062] 1. The present invention provides a high-performance Mo-based catalyst and a method for using it for the coupled thermal catalytic "zero-carbon" synthesis of ammonia using renewable energy electric power electrolysis of water to produce hydrogen. The Mo-based catalyst has excellent catalytic reaction performance in the ammonia synthesis process, providing a new method for green ammonia synthesis.

[0063] 2. In the Mo-based catalyst synthesis method provided by the present invention, the crystal phase of molybdenum nitride can be effectively controlled by adjusting the conditions in the nitriding treatment (such as nitriding atmosphere, heating rate, etc.).

[0064] 3. In the ammonia synthesis performance test of the Mo-based catalyst provided by the present invention, the ammonia synthesis performance of the Mo-based catalyst at low temperature can be optimized by changing the pre-reduction temperature of the molybdenum nitride catalyst, thereby achieving efficient ammonia synthesis under mild conditions. The inventors found that the N element in the molybdenum nitride included in the Mo-based catalyst of the present invention can directly participate in the ammonia synthesis reaction, so that the Mo-based catalyst forms N vacancies and supplements the N element from the feed gas to complete the catalytic reaction cycle.

[0065] 4. The ammonia synthesis rate of the Mo-based catalyst provided by the present invention is better than that of the traditional Mo-based catalyst, and the preparation method of the Mo-based catalyst of the present invention is relatively simple. Since the catalyst does not contain precious metals, the catalyst cost can be effectively reduced, the thermal stability is good, and the catalyst is easy to shape, and has obvious industrial application value. BRIEF DESCRIPTION OF THE DRAWINGS

[0066] Figure 1 The X-ray diffraction (XRD) patterns of the Mo-based catalysts prepared in Examples 1 to 5.

[0067] Figure 2 The nitrogen temperature programmed desorption (N2-TPD) diagram of the Mo-based catalysts prepared in Examples 1, 4 and 5.

[0068] Figure 3 This is a graph showing the ammonia synthesis reaction rate of the Mo-based catalysts prepared in Examples 1 to 5 at 400°C and 1 MPa.

[0069] Figure 4 The Mo-based catalyst prepared in Example 5 15 N isotope tracing experiment diagram.

[0070] Figure 5 This is the XRD pattern of the comparative Mo-based catalyst of Comparative Example 1. DETAILED DESCRIPTION

[0071] The technical scheme of the present invention will be further described in detail below in conjunction with specific embodiments. It should be understood that the following embodiments are only exemplary descriptions and explanations of the present invention and should not be construed as limiting the scope of protection of the present invention. All technologies implemented based on the above content of the present invention are included in the scope that the present invention is intended to protect.

[0072] Unless otherwise specified, the raw materials and reagents used in the following examples are commercially available or can be prepared by known methods.

[0073] Example 1

[0074] The preparation method of Mo-based catalyst is as follows: ammonium molybdate (3.5 g) and hexamethylenetetramine (4 g) are dispersed in deionized water (50 mL) respectively, and after ultrasonic treatment for 10 min, a colorless, clear and transparent solution is formed; the two solutions are mixed, and then aged for 12 h to form a white precipitate, and the excess solvent is removed, and the precipitate is washed several times with a small amount of deionized water, and then dried at 120 ° C for 12 h and transferred to a muffle furnace, and heated in air at 5 ° C min -1 The oxide was then transferred to a tube furnace and heated to 500 °C and calcined for 4 h to obtain the oxide. The oxide was then transferred to a tube furnace and heated at 2 °C min in an atmosphere of 10 vol% NH3 / Ar mixed gas. -1 , heat up to 750℃, nitride for 2h to obtain nitride; after cooling to room temperature, switch to 1% O2 / Ar mixed gas for passivation for 6h to obtain black powder, which is the Mo-based catalyst, marked as γ-Mo2N.

[0075] Example 2

[0076] The preparation method of Mo-based catalyst is as follows: ammonium molybdate (3.5 g) is placed in a muffle furnace and heated at 5 °C min -1 The temperature was raised to 500 °C and calcined for 4 h to obtain the oxide. The oxide was then transferred to a tube furnace and heated at 5 °C min in a mixture of N2 and H2 with a volume ratio of 15:85. -1 , heat up to 700℃, nitride for 4h to obtain nitride; after cooling to room temperature, switch to 1% O2 / Ar mixed gas for passivation for 6h to obtain black powder, which is Mo-based catalyst, marked as β-Mo2N.

[0077] Example 3

[0078] The preparation method of Mo-based catalyst is as follows: Molybdenum chloride (3.5 g) is placed in a tube furnace and heated at 10 °C min -1 , the temperature was raised to 600°C and nitrided for 3 hours to obtain nitride; after cooling to room temperature, it was switched to 1 vol% O2 / Ar mixed gas for passivation for 6 hours to obtain a black powder, which is the Mo-based catalyst, marked as δ-Mo2N.

[0079] Example 4

[0080] The preparation method of Mo-based catalyst is as follows: ammonium molybdate (3.5 g) and hexamethylenetetramine (4 g) are dispersed in deionized water (50 mL) respectively, and after ultrasonic treatment for 10 min, a colorless, clear and transparent solution is formed; the two solutions are mixed, and then aged for 12 h to form a white precipitate, and the excess solvent is removed, and the precipitate is washed several times with a small amount of deionized water, and then dried at 120 ° C for 12 h and transferred to a muffle furnace, and heated in air at 5 ° C min -1The oxide was then transferred to a tube furnace and heated to 500 °C and calcined for 4 h to obtain the oxide. The oxide was then transferred to a tube furnace and heated at 2 °C min in an atmosphere of 10 vol% NH3 / Ar mixed gas. -1 , heat up to 750℃, nitride for 2h to obtain nitride; after cooling to room temperature, switch to 1% O2 / Ar mixed gas for passivation for 6h to obtain black powder, which is the Mo-based catalyst, marked as γ-Mo2N.

[0081] The black powder γ-Mo2N was placed in a 10% H2 / Ar mixed gas atmosphere at 5℃min -1 , heated to 400 °C, reduced for 2 h, and cooled to room temperature to obtain a pre-reduced black powder, which is the pre-reduced Mo-based catalyst, labeled as γ-Mo2N-400.

[0082] Example 5

[0083] The preparation method of Mo-based catalyst is as follows: ammonium molybdate (3.5 g) and hexamethylenetetramine (4 g) are dispersed in deionized water (50 mL) respectively, and after ultrasonic treatment for 10 min, a colorless, clear and transparent solution is formed; the two solutions are mixed, and then aged for 12 h to form a white precipitate, and the excess solvent is removed, and the precipitate is washed several times with a small amount of deionized water, and then dried at 120 ° C for 12 h and transferred to a muffle furnace, and heated in air at 5 ° C min -1 The oxide was then transferred to a tube furnace and heated to 500 °C and calcined for 4 h to obtain the oxide. The oxide was then transferred to a tube furnace and heated at 2 °C min in an atmosphere of 10 vol% NH3 / Ar mixed gas. -1 , heat up to 750℃, nitride for 2h to obtain nitride; after cooling to room temperature, switch to 1% O2 / Ar mixed gas for passivation for 6h to obtain black powder, which is the Mo-based catalyst, marked as γ-Mo2N.

[0084] The black powder γ-Mo2N was placed in a 10% H2 / Ar mixed gas atmosphere at 5℃min -1 , the temperature was raised to 500 °C, reduced for 2 h, and then cooled to room temperature to obtain a pre-reduced black powder, which was the pre-reduced Mo-based catalyst, labeled as γ-Mo2N-500.

[0085] Comparative Example 1

[0086] This comparative example is basically the same as Example 1, except that the oxide prepared in Example 1 is subjected to nitridation treatment to obtain a nitride as comparative Mo-based catalyst 1.

[0087] Since the comparative Mo-based catalyst 1 prepared in this comparative example has not been passivated, it is easily oxidized to form a partially oxidized phase after being exposed to air for 2 hours, which will lead to a decrease in the activity of synthesizing ammonia. Figure 5 Middle A.

[0088] Comparative Example 2

[0089] This comparative example is basically the same as Example 1, except that the oxide prepared in Example 1 is not subjected to nitridation treatment, but is directly calcined in an inert atmosphere (such as argon) for 2 hours to obtain a comparative Mo-based catalyst 2.

[0090] It is known from the test that the comparative Mo-based catalyst 2 includes an oxidized phase, which is not a pure phase of molybdenum nitride, and has a poor effect when used as a catalyst in the synthesis of ammonia.

[0091] Test Example 1

[0092] The catalysts prepared in Examples 1 to 5 were used to detect the crystal structure of the catalysts by X-ray diffraction. The results are as follows: Figure 1 As shown. It can be seen that the main crystal phase of the XRD spectrum of the Mo-based catalyst prepared in Example 1 is the γ phase (see Figure 1 a), indicating that the Mo-based catalyst prepared in Example 1 contains γ-phase Mo2N; the XRD pattern of the Mo2N catalyst prepared in Example 2 shows that the main crystalline phase is β-phase (see Figure 1 c), indicating that the Mo-based catalyst prepared in Example 2 contains β-phase Mo2N; the XRD spectrum of the Mo-based catalyst prepared in Example 3 shows that the main crystalline phase is δ-phase (see Figure 1 b), indicating that the Mo-based catalyst prepared in Example 3 contains δ-phase Mo2N.

[0093] The XRD patterns of the Mo-based catalysts prepared in Examples 4 and 5 are shown in Figure 1 In d and e, the main crystal phase is γ phase, which is basically the same as Example 1.

[0094] Test Example 2

[0095] The Mo-based catalysts prepared in Examples 1, 4 and 5 were tested for nitrogen adsorption and desorption capabilities by nitrogen temperature programmed desorption (N2-TPD) experiments. Figure 2 As shown. Figure 2 It can be seen that the Mo-based catalysts prepared in Examples 4 and 5 have lower nitrogen desorption temperatures and more nitrogen desorption amounts than the Mo-based catalyst prepared in Example 1, indicating that the Mo-based catalysts prepared in Examples 4 and 5 have stronger adsorption and desorption capabilities for nitrogen, proving that the pre-reduced Mo-based catalyst is beneficial to improving the nitrogen adsorption and desorption capabilities of the Mo-based catalyst; and the Mo-based catalyst prepared in Example 5 has lower nitrogen desorption temperatures and more nitrogen desorption amounts than the Mo-based catalyst prepared in Example 4, indicating that the molybdenum nitride catalyst prepared in Example 5 has stronger adsorption and desorption capabilities for nitrogen, proving that the Mo-based catalyst pretreated with a pre-reduction temperature of 500°C has better performance.

[0096] Application Example 1

[0097] The preparation method of distributed synthetic ammonia is as follows:

[0098] 0.15 g of each Mo-based catalyst prepared in Examples 1 to 5 was used as a catalyst for synthesizing ammonia. The ammonia synthesis rate was measured in a continuous flow micro fixed bed reactor. The reaction gas was introduced at a total mass space velocity of 60,000 mL g -1 h -1 The concentration change of NH3 in the tail gas was measured by ion chromatography (Thermo Scientific, DIONEX, ICS-600); wherein the reaction gas composition was: 75vol%H2+25vol%N2 mixed gas. Under the conditions of 400℃ and 1MPa, the reaction rate of synthesizing ammonia using different Mo-based catalysts was measured. The test results of the Mo-based catalysts of Examples 1 to 5 are shown in Figure 3 .

[0099] from Figure 3 It can be seen that the Mo-based catalysts of Examples 1 to 5 exhibit different ammonia synthesis activities. The activity order of the Mo-based catalysts is γ-Mo2N-500>γ-Mo2N-400>γ-Mo2N>β-Mo2N>δ-Mo2N. At 400°C and 1 MPa, the reaction rate of ammonia synthesis over the Mo catalyst containing γ-Mo2N-500 can reach 5.3 mmol g -1 h -1 .

[0100] Application Example 2

[0101] The Mo-based catalyst γ-Mo2N-500 prepared in Example 5 was used as a catalyst for synthesizing ammonia; the reaction gas composition was: 5 vol% 15 N2+95vol%Ar. 15 N isotope tracing experiments were used to detect the reaction characteristics of N element in Mo catalyst.

[0102] from Figure 4 It can be seen that when entering 15 After the reaction gas of N2, it can be detected 14 N 15 The mass spectrometry signal of N (m / z=29) indicates 15 N2 gas molecules 15 The N isotope is adsorbed on the Mo-based catalyst and dissociated, and 14N is combined with Mo and then desorbed from the surface of the Mo-based catalyst. The results show that the N element in the Mo-based catalyst can be desorbed from the surface of the Mo-based catalyst to form nitrogen vacancies, directly participating in the reaction process of synthesizing ammonia, and the N element in the reaction gas will be re-adsorbed on the nitrogen vacancies of the Mo-based catalyst to replenish the consumed N element in the Mo-based catalyst and complete the catalytic reaction cycle.

[0103] The above is a description of the exemplary embodiments of the present invention. However, the protection scope of the present application is not limited to the above embodiments. Any modification, equivalent substitution, improvement, etc. made by those skilled in the art within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a Mo-based catalyst, characterized in that: The following steps are involved: (1) subjecting a molybdenum-containing precursor to a nitriding treatment to obtain a nitride; (2) The nitride obtained in step (1) is passivated to obtain the Mo-based catalyst.

2. The preparation method according to claim 1, characterized in that: In step (1), the molybdenum-containing precursor may be first subjected to an oxidation treatment and then to a nitridation treatment. Preferably, the oxidation treatment is carried out by calcining in an oxygen-containing atmosphere.

3. The preparation method according to claim 1 or 2, characterized in that: The molybdenum-containing precursor is selected from molybdenum salts and / or molybdenum precipitates. Preferably, the molybdenum salt is selected from at least one of ammonium molybdate, molybdenum chloride and sodium molybdate. Preferably, the molybdenum precipitate is prepared by adding a precipitant to a solution containing a molybdenum salt. Preferably, the molybdenum salt-containing solution further comprises a solvent, and the solvent is selected from at least one of ethanol, water and tetrahydrofuran.

4. The preparation method according to any one of claims 1 to 3, characterized in that In step (1), the nitridation treatment is performed in a nitrogen-containing atmosphere. Preferably, the nitrogen-containing atmosphere includes at least nitrogen and / or ammonia, and optionally includes or excludes argon and hydrogen. Preferably, in step (1), the conditions of the nitriding treatment include: the nitriding temperature is 600-900° C.; and the nitriding time is 2-12 h. Preferably, in step (1), the heating rate of the nitridation treatment is 2-10°C min -1 .

5. The preparation method according to any one of claims 1 to 4, characterized in that: In step (2), the passivation treatment is carried out in a passivation gas, and the passivation gas includes a mixture of oxygen and an inert gas. Preferably, the inert gas is selected from any one of nitrogen, argon, and helium. Preferably, the volume concentration of oxygen in the passivation gas is 0-10 vol%. Preferably, in step (2), the conditions for the passivation treatment include: the passivation time is 6-12 hours. Preferably, in step (2), the Mo-based catalyst comprises molybdenum nitride, and the crystalline phase of the molybdenum nitride is selected from any one of the following crystalline phases: δ-Mo2N, β-Mo2N, and γ-Mo2N.

6. The preparation method according to any one of claims 1 to 5, characterized in that: The preparation method further comprises: (3) subjecting the Mo-based catalyst to a pre-reduction treatment. Preferably, the pre-reduction treatment comprises: heat treating the Mo-based catalyst in a reducing atmosphere. Preferably, the reducing atmosphere comprises a mixture of hydrogen and argon, wherein the volume content of hydrogen is 1-10 vol%. Preferably, the heat treatment temperature is 300-500°C. Preferably, the heat treatment time is 1-4 hours.

7. The preparation method according to any one of claims 1 to 6, characterized in that: The preparation method of the Mo-based catalyst comprises the following steps: (A1) uniformly dispersing a molybdenum salt and a precipitant in a solvent, respectively, mixing, and standing for aging to obtain a molybdenum precipitate; (A2) subjecting the molybdenum precipitate obtained in step (A1) to nitridation to obtain a nitride; (A3) The nitride obtained in step (A2) is passivated to obtain the Mo-based catalyst. Preferably, the static aging time is 6-24h. Preferably, the preparation method further comprises: (A4) subjecting the Mo-based catalyst to a pre-reduction treatment.

8. The preparation method according to any one of claims 1 to 7, characterized in that: The preparation method of the Mo-based catalyst comprises the following steps: (B1) calcining the molybdenum salt in air to form an oxide; (B2) subjecting the oxide obtained in step (B1) to nitridation to obtain a nitride; (B3) subjecting the nitride obtained in step (B2) to passivation treatment to obtain the Mo-based catalyst. Preferably, the preparation method further comprises: (B4) subjecting the Mo-based catalyst to a pre-reduction treatment.

9. A Mo-based catalyst, characterized in that The Mo-based catalyst is obtained by the preparation method according to any one of claims 1 to 8. Preferably, the Mo-based catalyst comprises molybdenum nitride, and the molybdenum nitride is crystalline. Preferably, in the Mo-based catalyst, the crystal phase of the molybdenum nitride crystal is selected from at least one of δ-Mo2N, β-Mo2N and γ-Mo2N.

10. Use of the Mo-based catalyst according to claim 9.

Citation Information

Patent Citations

  • Molybdenum-based nitrogen carrier and preparation method and application thereof

    CN114669316A

  • Long chain normal compound diene selective hydrogenation catalyst-molybdenum nitrid and molybdenum nitrooxide and preparation and use thereof

    CN1385240A

  • Process and apparatus for preparing metal nitride catalyst material

    CN1887421A

  • Ammonia-decomposition catalyst, method of producing the same, and method of treating ammonia

    JP2010094669A

Cited By

  • Alkali metal modified molybdenum nitride-based catalyst as well as preparation method and application thereof

    CN120346830A

  • Ni-based three-phase structure ammonia synthesis catalyst as well as preparation method and application thereof