Lanthanum ferric cobaltate / carbon nitride quantum dot composite material as well as preparation method and application thereof
By preparing lanthanum iron cobaltate/carbon nitride quantum dot composite materials, the problems of weak photogenerated charge separation ability and small specific surface area of LaFeO3 materials were solved, achieving efficient degradation of acetaminophen, simplifying the preparation process and reducing costs.
Patent Information
- Application Number
- CN202410984049.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-11-12
AI Technical Summary
Existing LaFeO3 materials exhibit weak photogenerated charge separation ability and small specific surface area when photocatalyzing and combining with persulfate to degrade acetaminophen, which limits their application in the degradation of water pollutants.
Lanthanum iron cobaltate LaFe0.5Co0.5O3 was prepared by replacing Fe in the LaFeO3 perovskite matrix with Co component, and then combined with carbon nitride quantum dots (CNQDs) to form lanthanum iron cobaltate/carbon nitride quantum dot composite material, which enhances heterogeneous catalysis.
The photocatalytic activity and persulfate activation ability of the composite material under visible light were improved, significantly enhancing the degradation effect of acetaminophen, simplifying the preparation process and reducing costs.
Smart Images

Figure CN118925774A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of nanomaterials, and specifically relates to a lanthanum iron cobaltate / carbon nitride quantum dot composite material and a preparation method and application thereof. Background Art
[0002] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention, and should not necessarily be regarded as an admission or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art.
[0003] Acetaminophen is an antipyretic and analgesic drug, also known as paracetamol (PCM). PCM has a low bioavailability in the human body (about 5-15%) and a high solubility in water (12.78 g / L). At the same time, as the consumption increases, a large amount of drugs are discharged into water resources. The long-term accumulation of drugs in water will cause harm to aquatic organisms, thereby affecting the aquatic ecosystem. In order to inhibit the occurrence of this phenomenon and reduce the presence of harmful substances in drinking water and groundwater, researchers have developed various methods to remove drug pollutants in water. Advanced oxidation technology has become an ideal method for degrading acetaminophen due to its high efficiency, low cost, and green advantages. Photocatalysis has also been paid attention to as one of the degradation methods. However, the long reaction time required for this technology and the loss of effect caused by various water pollutants limit its practical application. In order to shorten its reaction time, photocatalysis is combined with persulfate (PMS) advanced oxidation technology to form a synergistic effect between the two, and its degradation effect is higher than that of a single photocatalytic system.
[0004] As a typical perovskite material, LaFeO3 has the advantages of simple synthesis method, low cost and non-toxicity. LaFeO3 contains Fe element, which can effectively activate hydrogen peroxide and persulfate, so it is used as a catalyst in advanced oxidation technology. LaFeO3 has excellent characteristics such as high stability, non-toxicity and narrow bandgap, and can be used in photocatalytic reactions. However, its weak photogenerated charge separation ability and small specific surface area seriously restrict the improvement of photocatalytic activity, and restrict its application in the combined degradation of photocatalysis and persulfate. Summary of the invention
[0005] In order to solve the shortcomings of the prior art, the present invention provides a lanthanum iron cobalt oxide / carbon nitride quantum dot composite material and its preparation method and application. The present invention uses Co component to replace part of Fe in LaFeO3 perovskite matrix to obtain lanthanum iron cobalt oxide LaFe 0.5 Co 0.5 O3 to enhance heterogeneous catalysis. Carbon nitride quantum dots (CNQDs) with advantages of photostability, low toxicity, tunable surface chemistry, wide visible range response and upconversion luminescence effect were combined with LaFe 0.5 Co0.5 O3 is compounded to effectively improve the photocatalytic ability and persulfate activation ability of the composite material. The composite material has a significant improvement in the degradation effect of PCM in the water environment.
[0006] In order to achieve the above technical objectives, the present invention adopts the following technical solutions:
[0007] The first aspect of the present invention provides a method for preparing a lanthanum iron cobaltate / carbon nitride quantum dot composite material, comprising the following steps:
[0008] (1) hydrothermally reacting melamine and citric acid to obtain carbon nitride quantum dots;
[0009] (2) heating lanthanum salt, iron salt, cobalt salt and citric acid to obtain a precursor, and calcining the precursor to obtain LaFe 0.5 Co 0.5 O3;
[0010] (3) Carbon nitride quantum dots and LaFe 0.5 Co 0.5 O3 was ball milled to obtain lanthanum iron cobaltate / carbon nitride quantum dot composite material.
[0011] In one or more embodiments, in step (1), the mass ratio of melamine to citric acid is 1:(0.7-0.9).
[0012] In one or more embodiments, in step (1), the temperature of the hydrothermal reaction is 170-190° C., and the time is 3-5 hours.
[0013] In one or more embodiments, in step (2), the lanthanum salt comprises lanthanum nitrate, the iron salt comprises iron nitrate, and the cobalt salt comprises cobalt nitrate;
[0014] The molar ratio of lanthanum salt, iron salt, cobalt salt and citric acid is (1.7-1.8):1:1:(5.9-6.1).
[0015] In one or more embodiments, in step (2), the heating reaction temperature is 75 to 85° C. and the time is 9 to 11 hours.
[0016] In one or more embodiments, in step (2), the calcination temperature is 650-750° C., the heating rate is 4-6° C. / min, and the calcination time is 4-6 h.
[0017] In one or more embodiments, in step (3), carbon nitride quantum dots and LaFe 0.5 Co 0.5 The mass ratio of O3 is 1:(5~20).
[0018] In one or more embodiments, in step (3), the ball milling speed is 550-650 rpm, and the ball milling time is 5-7 h.
[0019] The second aspect of the present invention provides a lanthanum iron cobaltate / carbon nitride quantum dot composite material prepared by the above preparation method.
[0020] The third aspect of the present invention provides the use of the above-mentioned lanthanum iron cobaltate / carbon nitride quantum dot composite material in the degradation of pollutants by coupling persulfate under visible light, wherein the pollutants include acetaminophen.
[0021] The beneficial effects of the present invention are:
[0022] (1) The present invention uses Co to replace part of the Fe in the LaFeO3 perovskite matrix to obtain lanthanum iron cobaltate LaFe 0.5 Co 0.5 O3 to enhance heterogeneous catalysis. Carbon nitride quantum dots (CNQDs) with advantages of photostability, low toxicity, tunable surface chemistry, wide visible range response and upconversion luminescence effect were combined with LaFe 0.5 Co 0.5 O3 is compounded to form LaFe 0.5 Co 0.5 The photocatalytic activity of O3 and the oxidative performance of carbon nitride quantum dots work together to improve the ability of lanthanum iron cobalt oxide / carbon nitride quantum dot composite materials to activate PMS to degrade PCM under visible light conditions.
[0023] (2) In the present invention, ball milling is used to mix carbon nitride quantum dots with LaFe 05 Co 05 O3 is compounded, LaFe in the composite material 0.5 Co 0.5 The crystal structure of O3 remains unchanged, maintaining the catalytic activity of the perovskite material under visible light.
[0024] (3) Carbon nitride quantum dots can be obtained by hydrothermal method, and LaFe can be obtained by sol-gel method 0.5 Co 0.5 O3, and then the carbon nitride quantum dots and LaFe 0.5 Co 0.5 O3 is compounded to obtain lanthanum iron cobaltate / carbon nitride quantum dot composite material. The whole preparation method is simple and low-cost, which is conducive to industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] The accompanying drawings in the specification, which constitute a part of the present invention, are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.
[0026] Figure 1 This is a scanning electron microscope image of carbon nitride quantum dots in Example 1;
[0027] Figure 2 The infrared spectra of LFCO of Comparative Example 1, (20) LFCO / CNQDs of Example 1, (10) LFCO / CNQDs obtained in Example 2, and (5) LFCO / CNQDs of Example 3;
[0028] Figure 3 XRD patterns of LFCO of Comparative Example 1, LFCO of Comparative Example 2, (20) LFCO / CNQDs of Example 1, (10) LFCO / CNQDs obtained in Example 2, and (5) LFCO / CNQDs of Example 3;
[0029] Figure 4 This is the efficiency diagram of catalytic degradation of PCM under the light-PMS system of LFCO of Comparative Example 1, LFCO of Comparative Example 2, (20) LFCO / CNQDs of Example 1, (10) LFCO / CNQDs obtained in Example 2, and (5) LFCO / CNQDs of Example 3. DETAILED DESCRIPTION
[0030] It should be noted that the following detailed descriptions are exemplary and are intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used in the present invention have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.
[0031] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit exemplary embodiments according to the present invention. As used herein, unless the context clearly indicates otherwise, the singular form is also intended to include the plural form. In addition, it should be understood that when the terms "comprising" and / or "including" are used in this specification, it indicates the presence of features, steps, operations, devices, components and / or combinations thereof.
[0032] In order to enable those skilled in the art to more clearly understand the technical solution of the present invention, the technical solution of the present invention will be described in detail below in combination with specific embodiments and comparative examples.
[0033] The instruments and reagents used in the examples are shown in Table 1 and Table 2, respectively.
[0034] Table 1 Instruments and equipment
[0035]
[0036] Table 2 Main reagents
[0037]
[0038]
[0039] Example 1
[0040] 0.866g La(NO3)3·6H2O, 0.404g Fe(NO3)3·9H2O, 0.291g Co(NO3)2·6H2O and 1.152g citric acid were put into a beaker, dissolved in 50mL ultrapure water, mixed evenly, heated to 80℃ in a water bath and stirred for 10h, then placed in an oven at 80℃ for drying, and then placed in a tube furnace at 700℃, calcined at a heating rate of 5℃ / min for 5h to obtain LaFe 0.5 Co 0.5 O3.
[0041] 2.0 g of melamine and 1.6 g of citric acid were added to 80 mL of ultrapure water, and the mixed liquid was transferred to a 100 mL polytetrafluoroethylene liner, and then placed in a stainless steel reactor and heated to 180 ° C for 4 hours. After cooling, the supernatant was centrifuged and freeze-dried to obtain carbon nitride quantum dots (CNQDs). The morphology of carbon nitride quantum dots is shown in Figure 2. Figure 1 shown.
[0042] 0.05g of carbon nitride quantum dots were mixed with 1g of LaFe 0.5 Co 0.5 O3 was put into a ball mill and ball milled at 600 rpm for 6 h. The obtained lanthanum iron cobalt oxide / carbon nitride quantum dot composite material was recorded as (20) LFCO / CNQDs.
[0043] Example 2
[0044] 0.866g La(NO3)3·6H2O, 0.404g Fe(NO3)3·9H2O, 0.291g Co(NO3)2·6H2O and 1.152g citric acid were put into a beaker, dissolved in 50mL ultrapure water, mixed evenly, heated to 80℃ in a water bath and stirred for 10h, then placed in an oven at 80℃ for drying, and then placed in a tube furnace at 700℃, calcined at a heating rate of 5℃ / min for 5h to obtain LaFe 0.5 Co 0.5 O3.
[0045] 2.0 g of melamine and 1.6 g of citric acid were added to 80 mL of ultrapure water, and the mixed liquid was transferred to a 100 mL polytetrafluoroethylene liner, and then placed in a stainless steel reactor and heated to 180 ° C for 4 hours. After cooling, the supernatant was centrifuged and freeze-dried to obtain carbon nitride quantum dots (CNQDs).
[0046] 0.1g of carbon nitride quantum dots were mixed with 1g of LaFe 0.5 Co 0.5 O3 was put into a ball mill and ball milled at 600 rpm for 6 h. The obtained lanthanum iron cobalt oxide / carbon nitride quantum dot composite material was recorded as (10) LFCO / CNQDs.
[0047] Example 3
[0048] 0.866g La(NO3)3·6H2O, 0.404g Fe(NO3)3·9H2O, 0.291g Co(NO3)2·6H2O and 1.152g citric acid were put into a beaker, dissolved in 50mL ultrapure water, mixed evenly, heated to 80℃ in a water bath and stirred for 10h, then placed in an oven at 80℃ for drying, and then placed in a tube furnace at 700℃, calcined at a heating rate of 5℃ / min for 5h to obtain LaFe 0.5 Co 0.5 O3.
[0049] 2.0 g of melamine and 1.6 g of citric acid were added to 80 mL of ultrapure water, and the mixed liquid was transferred to a 100 mL polytetrafluoroethylene liner, and then placed in a stainless steel reactor and heated to 180 ° C for 4 hours. After cooling, the supernatant was centrifuged and freeze-dried to obtain carbon nitride quantum dots (CNQDs).
[0050] 0.2g of carbon nitride quantum dots were mixed with 1g of LaFe 0.5 Co 0.5 O3 was put into a ball mill and ball milled at 600 rpm for 6 h. The obtained lanthanum iron cobalt oxide / carbon nitride quantum dot composite material was recorded as (5) LFCO / CNQDs.
[0051] Example 4
[0052] 0.866g La(NO3)3·6H2O, 0.404g Fe(NO3)3·9H2O, 0.291g Co(NO3)2·6H2O and 1.152g citric acid were put into a beaker, dissolved in 50mL ultrapure water, mixed evenly, heated to 75℃ in a water bath and stirred for 11h, then placed in an oven at 80℃ for drying, and then placed in a tube furnace at 750℃, calcined at a heating rate of 6℃ / min for 4h to obtain LaFe 0.5 Co 0.5 O3.
[0053] 2.0 g of melamine and 1.6 g of citric acid were added to 80 mL of ultrapure water, and the mixed liquid was transferred to a 100 mL polytetrafluoroethylene liner, and then placed in a stainless steel reactor and heated to 170 ° C for 5 hours. After cooling, the supernatant was centrifuged and freeze-dried to obtain carbon nitride quantum dots (CNQDs).
[0054] 0.05g of carbon nitride quantum dots were mixed with 1g of LaFe 0.5 Co 0.5 O3 was put into a ball mill and ball milled at 550 rpm for 7 h to obtain a lanthanum iron cobaltate / carbon nitride quantum dot composite material.
[0055] Example 3
[0056] 0.866g La(NO3)3·6H2O, 0.404g Fe(NO3)3·9H2O, 0.291g Co(NO3)2·6H2O and 1.152g citric acid were put into a beaker, dissolved in 50mL ultrapure water, mixed evenly, heated to 85℃ in a water bath and stirred for 9h, then placed in an oven at 80℃ for drying, and then placed in a tube furnace at 650℃, calcined at a heating rate of 4℃ / min for 6h to obtain LaFe 0.5 Co 0.5 O3.
[0057] 2.0 g of melamine and 1.6 g of citric acid were added to 80 mL of ultrapure water, and the mixed liquid was transferred to a 100 mL polytetrafluoroethylene liner, and then placed in a stainless steel reactor and heated to 190 ° C for 3 hours. After cooling, the supernatant was centrifuged and freeze-dried to obtain carbon nitride quantum dots (CNQDs).
[0058] 0.05g of carbon nitride quantum dots were mixed with 1g of LaFe 0.5 Co 0.5 O3 was put into a ball mill and ball milled at 650 rpm for 5 h to obtain a lanthanum iron cobaltate / carbon nitride quantum dot composite material.
[0059] Comparative Example 1
[0060] 0.866g La(NO3)3·6H2O, 0.404g Fe(NO3)3·9H2O, 0.291g Co(NO3)2·6H2O and 1.152g citric acid were put into a beaker, dissolved in 50mL ultrapure water, mixed evenly, heated to 80℃ in a water bath and stirred for 10h, then placed in an oven at 80℃ for drying, and then placed in a tube furnace at 700℃, calcined at a heating rate of 5℃ / min for 5h to obtain LaFe 0.5 Co 0.5O3, denoted as LFCO.
[0061] Comparative Example 2
[0062] 2.0 g of melamine and 1.6 g of citric acid were added to 80 mL of ultrapure water, and the mixed liquid was transferred to a 100 mL polytetrafluoroethylene liner, and then placed in a stainless steel reactor and heated to 180 ° C for 4 hours. After cooling, the supernatant was centrifuged and freeze-dried to obtain carbon nitride quantum dots, recorded as CNQDs.
[0063] The LFCO of Comparative Example 1, the CQNDs of Comparative Example 2, the (20) LFCO / CNQDs prepared in Example 1, the (10) LFCO / CNQDs prepared in Example 2, and the (5) LFCO / CNQDs prepared in Example 3 were subjected to infrared and XRD analysis. The infrared analysis results are shown in FIG. Figure 2 As shown in the figure, 571cm -1 The absorption peaks at 570 and 665 cm -1 The absorption peaks observed at 856 cm are attributed to the stretching vibrations of Co-O bonds and La-O. -1 The band at 1415 cm-1 can be attributed to Co-O-Co vibration. For (x)LFCO / CNQDs (x = 5, 10, 20), the composites have the characteristic peak of LFCO monomer and the band at 1415 cm-1 can be attributed to Co-O-Co vibration. -1 and 1315cm -1 There is a characteristic peak of C=N / CN bond at 1627cm -1 There are characteristic peaks of CO of carboxylic acid groups at 3715 and 2985 cm -1 The broad peaks between are the characteristic peaks of NH / OH groups, indicating that LFCO and CNQDs are successfully composited. Figure 3 As shown, (x)LFCO / CNQDs (x = 5, 10, 20) and LFCO have obvious diffraction peaks at 22.9nm, 32.6nm, 40.1nm, 46.9nm, 52.8nm, 58.4nm, 68.4nm and 77.9nm, which correspond to LaFe 0.5 Co 0.5 The weak diffraction peaks at about 37.1 nm on the (002), (112), (022), (004), (114), (312), (224) and (420) planes of O3 are attributed to Co3O4, indicating that Co substitution causes a slight phase transition of perovskite. Due to the low doping amount of CNQDs, weak diffraction peaks of CNQDs can be seen at 13.2° and 27.8° of (x)LFCO / CNQDs (x=5, 10, 20), and the crystal structure remains consistent with LFCO.
[0064] Experimental Example 1
[0065] 0.02 g of LFCO of Comparative Example 1, CQNDs of Comparative Example 2, (20) LFCO / CNQDs prepared in Example 1, (10) LFCO / CNQDs prepared in Example 2, and (5) LFCO / CNQDs prepared in Example 3 were weighed and dispersed in 100 ml of a 30 ppm PCM solution. After standing and stirring for 30 min in the dark, 0.02 g of PMS was added to the solution system. After dissolution, light was applied to catalyze the degradation of PCM under the light-PMS system. Figure 4 As shown in the results, the degradation efficiency of LFCO / CNQDs composites was significantly improved compared with that of LFCO and CNQDs, and the ratio of LFCO and CNQDs had an effect on the degradation effect of the composites. (20) LFCO / CNQDs had the best degradation effect on PCM, with a degradation rate of 92% within 10 min.
[0066] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a lanthanum iron cobaltate / carbon nitride quantum dot composite material, It is characterized in that The following steps are involved: (1) hydrothermally reacting melamine and citric acid to obtain carbon nitride quantum dots; (2) heating lanthanum salt, iron salt, cobalt salt and citric acid to obtain a precursor, and calcining the precursor to obtain LaFe 0.5 Co 0.5 O 3 ; (3) Carbon nitride quantum dots and LaFe 0.5 Co 0.5 O 3 Ball milling was performed to obtain a lanthanum iron cobalt oxide / carbon nitride quantum dot composite material.
2. The preparation method according to claim 1, It is characterized in that In step (1), the mass ratio of melamine to citric acid is 1:(0.7-0.9).
3. The preparation method according to claim 1, It is characterized in that In step (1), the temperature of the hydrothermal reaction is 170-190° C. and the time is 3-5 hours.
4. The preparation method according to claim 1, It is characterized in that In step (2), the lanthanum salt includes lanthanum nitrate, the iron salt includes iron nitrate, and the cobalt salt includes cobalt nitrate; The molar ratio of lanthanum salt, iron salt, cobalt salt and citric acid is (1.7-1.8):1:1:(5.9-6.1).
5. The preparation method according to claim 1, It is characterized in that In step (2), the heating reaction temperature is 75 to 85° C. and the time is 9 to 11 hours.
6. The preparation method according to claim 1, It is characterized in that In step (2), the calcination temperature is 650-750° C., the heating rate is 4-6° C. / min, and the calcination time is 4-6 hours.
7. The preparation method according to claim 1, It is characterized in that In step (3), carbon nitride quantum dots and LaFe 0.5 Co 0.5 O 3 The mass ratio is 1:(5-20); Alternatively, in step (3), the ball milling speed is 550-650 rpm, and the ball milling time is 5-7 h.
8. A lanthanum iron cobaltate / carbon nitride quantum dot composite material, It is characterized in that The method is obtained by the preparation method according to any one of claims 1 to 7.
9. Use of the lanthanum iron cobaltate / carbon nitride quantum dot composite material as claimed in claim 8 in coupling persulfate degradation of pollutants under visible light.
10. The use according to claim 9, It is characterized in that The contaminants included acetaminophen.