Cracking reaction catalyst with core-shell structure and preparation method thereof

Through the preparation of core-shell structure catalyst, the problems of low cracking reaction efficiency and high preparation cost of 13X molecular sieve were solved, and the efficient catalytic activity and silicon source utilization were improved, and the structure and performance of the molecular sieve were optimized.

CN118925781AActive Publication Date: 2024-11-12CHINA ENERGY GRP NINGXIA COAL IND CO LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202410976174.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-12
Estimated Expiration
2044-07-19

AI Technical Summary

Technical Problem

In the prior art, the cracking reaction efficiency is low, and the preparation of 13X molecular sieve has problems such as low silicon source utilization, difficult product size and morphology, and poor dispersion.

Method used

Using the preparation method of core-shell structure cracking reaction catalyst, waste molecular sieve is subjected to aluminum-soluble and silicon-soluble treatment to form aluminum-rich liquid and silicon-rich liquid. Then, 13X molecular sieve is obtained by gelation and hydrothermal crystallization, and silane is used to obtain The chemical reagent and nickel solution were impregnated to form a nickel nanoparticle layer, then combined with a titanium silicon molecular sieve, and finally mixed with a platinum precursor for calcination to form a core-shell structure catalyst.

Benefits of technology

Improve the mechanical strength and thermal stability of the 13X molecular sieve, increase the specific surface area and porosity, improve the catalytic activity and efficiency of the cracking reaction, reduce the preparation cost, improve the utilization rate of the silicon source, and enhance the reactants inside the molecular sieve. flow diffusion performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004954577570000111
    Figure BDA0004954577570000111
  • Figure BDA0004954577570000121
    Figure BDA0004954577570000121
Patent Text Reader

Abstract

The invention provides a cracking reaction catalyst with a core-shell structure and a preparation method thereof. The preparation method comprises the following steps: sequentially carrying out aluminum dissolving treatment and silicon dissolving treatment on a waste molecular sieve to obtain aluminum-rich liquid and silicon-rich liquid; the method comprises the following steps: sequentially carrying out gelation treatment, aging treatment and hydrothermal crystallization treatment on raw materials comprising aluminum-rich liquid, silicon-rich liquid and seed crystals to obtain the 13X molecular sieve, the method comprises the following steps: sequentially carrying out first dipping treatment and second dipping treatment on a 13X molecular sieve in a silanization reagent solution and a nickel-containing solution to obtain a nickel-modified 13X molecular sieve; the preparation method comprises the following steps: sequentially performing first hydrothermal reaction and roasting treatment on a nickel modified 13X molecular sieve and titanium silicalite molecular sieve precursor solution to obtain a core-shell structure 13X molecular sieve; the core-shell structure 13X molecular sieve and a platinum precursor solution are mixed and stirred, and then are subjected to solid-liquid separation, drying, pre-roasting treatment and first calcining treatment in sequence, and the obtained cracking reaction catalyst with the core-shell structure has relatively high catalytic activity in a catalytic cracking reaction.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of cracking reaction catalyst preparation, and in particular to a core-shell structure cracking reaction catalyst and a preparation method thereof. Background Art

[0002] Molecular sieve is a kind of aluminosilicate, which has the characteristics of uniform pore size, regular crystal structure, rich pore system, large specific surface area and good thermal stability. Therefore, molecular sieve is considered to be the preferred adsorbent material for removing oxygen-containing compounds from olefins. Among them, FAU molecular sieves include X-type molecular sieves and Y-type molecular sieves. The pore size of FAU molecular sieves is about 0.74nm. The X-type molecular sieve in FAU molecular sieves can better remove oxygen-containing compound impurities in olefins, so it has been studied more and has also been applied in industrial practice.

[0003] The 13X molecular sieve in the X-type molecular sieve has a uniform and ordered microporous structure, which enables it to achieve precise molecular screening. Specifically, the size and shape of the micropores of the 13X molecular sieve can highly specifically adsorb molecules of a specific size and shape, while excluding other molecules, which is very valuable in the separation and purification process of the chemical industry. For example, in the field of gas separation, the 13X molecular sieve can effectively separate target gases such as oxygen, nitrogen or carbon dioxide from a mixed gas flow. The 13X molecular sieve has a large specific surface area that can provide more active adsorption sites, thereby increasing the adsorption capacity of the 13X molecular sieve. This means that within the same physical volume, the 13X molecular sieve can adsorb more substances, thereby improving the processing rate and efficiency. The adsorption capacity of the 13X molecular sieve is particularly important in the fields of liquid or gas purification, catalyst carriers, and storage media.

[0004] Therefore, 13X molecular sieves with uniform and orderly micropores, large specific surface area and large pore capacity not only show great potential in the traditional fields of chemical industry, oil and gas processing, but also show broad application prospects in emerging fields such as environmental protection, clean energy, life sciences, etc. For example, in industrial waste gas treatment, 13X molecular sieves can effectively remove harmful gases and volatile organic compounds (VOCs); in the production of pharmaceuticals and refined chemicals, 13X molecular sieves can be used to improve the purity and yield of products.

[0005] However, there are problems in the prior art synthesis of 13X molecular sieves, such as low silicon source utilization, difficult control of product size and morphology, and poor dispersibility. The Chinese patent with the patent authorization announcement number CN103523796B proposes a method for preparing a submicron X-type molecular sieve, and applies it to the separation and adsorption of hydrocarbons. Specifically, silica sol is first used as a silicon source to prepare a guiding agent, water glass, sodium hydroxide, and aluminum hydroxide are used to prepare the mother liquor of the molecular sieve, and then the mother liquor of the molecular sieve is added to the guiding agent for aging, and a weak polar dispersant is added after aging, and microwave-assisted crystallization is used to finally prepare a submicron X-type molecular sieve. The X-type molecular sieve prepared by the above method has small crystals, shortened synthesis time, and low production cost. The finished adsorbent prepared by submicron X-type molecular sieve has the characteristics of large adsorption capacity and easy regeneration, which is suitable for deep removal of oxygen-containing impurities in hydrocarbon streams, and the 13X molecular sieve is made into a catalyst, which has a problem of low catalytic efficiency during catalytic cracking reactions. Summary of the invention

[0006] The main purpose of the present invention is to provide a core-shell structure cracking reaction catalyst and a preparation method thereof, so as to solve the problem of low cracking reaction efficiency in the prior art.

[0007] In order to achieve the above-mentioned purpose, according to one aspect of the present invention, a preparation method of a core-shell structure cracking reaction catalyst is provided, and the preparation method comprises the following steps: step S1, sequentially subjecting the waste molecular sieve to aluminum dissolution treatment and silicon dissolution treatment to obtain aluminum-rich liquid and silicon-rich liquid; step S2, sequentially subjecting the raw materials including the aluminum-rich liquid, the silicon-rich liquid and the seed to gelation treatment, aging treatment and hydrothermal crystallization treatment to obtain 13X molecular sieve; step S3, sequentially subjecting the 13X molecular sieve to a first impregnation treatment and a second impregnation treatment in a silanization agent solution and a nickel-containing solution to obtain a nickel-modified 13X molecular sieve; step S4, sequentially subjecting the nickel-modified 13X molecular sieve and a titanium silicon molecular sieve precursor solution to a first hydrothermal reaction and a roasting treatment to obtain a core-shell structure 13X molecular sieve; and step S5, mixing the core-shell structure 13X molecular sieve with a platinum precursor solution, and sequentially subjecting the mixture to solid-liquid separation, drying, pre-roasting treatment and a first calcination treatment to obtain a core-shell structure cracking reaction catalyst.

[0008] Further, in the above step S3: the time of the first impregnation treatment is 8 to 24 hours; and / or, the time of the second impregnation treatment is 24 to 48 hours; preferably, the molar concentration of the silanization agent solution is 0.05 to 0.2 mol / L; and / or, the molar concentration of the nickel-containing solution is 0.05 to 0.2 mol / L; preferably, the mass ratio of the 13X molecular sieve to the volume ratio of the silanization agent solution is 400 to 600:1 g / L; and / or, the mass ratio of the 13X molecular sieve to the volume ratio of the nickel-containing solution is 400 to 6 00:1g / L; preferably, the nickel-containing solution is a nickel nitrate solution and / or a nickel sulfate solution; preferably, the silanization agent is selected from any one or more of 3-aminopropyltriethoxysilane, tetraethoxysilane and tetramethoxysilane; preferably, step S3 also includes: subjecting the 13X molecular sieve obtained by the second impregnation treatment to a third calcination to obtain a nickel-modified 13X molecular sieve coated with a nickel nanoparticle layer; and / or, the atmosphere of the third calcination is hydrogen, the temperature of the third calcination is 500-600°C, and the time of the third calcination is 2-4h.

[0009] Further, in the above step S4, the temperature of the first hydrothermal reaction is 150-200° C., and the time of the first hydrothermal reaction is 12-24 h; and / or, the temperature of the calcination treatment is 450-550° C., and the time of the calcination treatment is 4-8 h; the titanium silicon molecular sieve precursor solution includes a first silicon source, a titanium source, a template, a fluorine complex and water, wherein the first silicon source, the titanium source, the template, the fluorine complex and the water are in a molar ratio of 1:0.04-0.1:0.1-0.3:0.03-0.06:20-50 Mixing; and / or, the ratio of the mass of nickel-modified 13X molecular sieve to the volume of the titanium silicon molecular sieve precursor solution is 400-600:1 g / L; preferably, the first silicon source is selected from any one or more of SiO2, Na2SiO3 and Si(OC2H5)4; preferably, the titanium source is selected from any one or more of TiO2, TiCl4 and Na2TiO3; preferably, the fluorine complex is selected from any one or more of sodium hexafluorophosphate, sodium hexafluoroacetylacetonate and ammonium fluoride; preferably, the template is an organic amine and / or a quaternary ammonium salt.

[0010] Furthermore, in the above step S5, stirring is performed during the mixing process, and the stirring time is preferably 12 to 36 hours; the mass concentration of the platinum precursor solution is preferably 2 to 3 g / L; the platinum precursor solution is preferably hexachloroplatinic acid dihydrate; the volume ratio of the mass of the core-shell structure 13X molecular sieve to the platinum precursor solution is preferably 1:5 g / L; and / or, the atmosphere of the pre-calcination treatment is an inert gas, and / or, the temperature of the pre-calcination treatment is 450 to 550° C.; and / or, the time of the pre-calcination treatment is 1 to 3 hours; and / or, the temperature of the first calcination treatment is 700 to 900° C.; and / or, the time of the first calcination treatment is 3 to 5 hours; and / or, the atmosphere of the first calcination treatment is air; and / or, the drying temperature is 90 to 130° C., and the drying time is 8 to 16 hours.

[0011] Furthermore, in the above step S2, the 13X molecular sieve contains silicon and aluminum, and the molar ratio of silicon to aluminum is 2.2 to 2.9:1; and / or the pore volume of the 13X molecular sieve is 0.3 to 0.5 cm 3 / g; and / or, the specific surface area of ​​13X molecular sieve is 700-950m 2 / g.

[0012] Furthermore, the above-mentioned seed crystals contain SiO2, Al2O3, Na2O and H2O, wherein the molar ratio of SiO2 to Al2O3 is 0.01-2.5:1, and the molar ratio of Na2O, H2O and SiO2 is 0.01-4.0:1.0-40.0:1.

[0013] Furthermore, the above-mentioned step S2 includes: step S21, gelling the aluminum-rich liquid and the silicon-rich liquid to obtain a first gel; step S22, aging the first gel and the seed crystal in turn and hydrothermal crystallization treatment to obtain a 13X molecular sieve; wherein the first gel contains SiO2, Al2O3, Na2O and H2O, wherein the molar ratio of SiO2 to Al2O3 is 0.5-6.0:1, and the molar ratio of Na2O, H2O and SiO2 is 0.5-6.0:10-100:1; preferably, the mass ratio of the seed crystal to the first gel is 5-20:100; and / or, the aging treatment temperature is 20-100°C, and the aging treatment time is 0.1-24h; and / or, the hydrothermal crystallization treatment temperature is 60-105°C, and the hydrothermal crystallization treatment time is 0.1-36h.

[0014] Furthermore, the preparation method further includes: a seed crystal preparation process, the preparation process including: stirring and mixing raw materials including an aluminum source, a second silicon source and water to obtain a second gel; adjusting the pH value of the second gel to 8.5-12.5 and then performing two-stage hydrothermal crystallization treatment to obtain a seed crystal; wherein the stirring and mixing rate is 200-800 rpm; and / or the stirring and mixing temperature is 20-100°C; and / or the stirring and mixing time is 0.1-24h; preferably, the pH value of the second gel is 11.8-12.2; preferably, the second silicon source is selected from any one or more of silica sol, tetraethyl orthosilicate and silicon powder; preferably, the aluminum source is selected from any one or more of sodium aluminate, pseudo-boehmite, aluminum sulfate and aluminum nitrate; preferably, the two-stage hydrothermal The crystallization treatment includes a first hydrothermal crystallization treatment and a second hydrothermal crystallization treatment, wherein the temperature of the first hydrothermal crystallization treatment is 20 to 60°C; and / or the time of the first hydrothermal crystallization treatment is 4 to 24 hours; preferably, the temperature of the second hydrothermal crystallization treatment is 80 to 120°C; and / or the time of the second hydrothermal crystallization treatment is 6 to 48 hours; further, preferably, the temperature of the first hydrothermal crystallization treatment is 35 to 45°C, and / or the time of the first hydrothermal crystallization treatment is 11 to 13 hours; the temperature of the second hydrothermal crystallization treatment is 90 to 100°C; and / or the time of the second hydrothermal crystallization treatment is 22 to 26 hours; the temperature of the second hydrothermal crystallization treatment is 50 to 60°C higher than the temperature of the first hydrothermal crystallization treatment.

[0015] Furthermore, the above-mentioned preparation method also includes a process of pretreating the waste molecular sieve, and the pretreatment process includes: sintering a mixture including the waste molecular sieve and the sodium salt to obtain a sintered product; using an acidic solution to sequentially perform aluminum dissolution treatment and solid-liquid separation on the sintered product to obtain an aluminum-rich liquid and a residue; using an alkaline solution to sequentially perform silicon dissolution treatment and solid-liquid separation on the residue to obtain a silicon-rich liquid; wherein the mass ratio of the waste molecular sieve to the sodium salt is 1:0.5-5; and / or the sintering temperature is 550-800°C; and / or the sintering time is 60-120 min ; and / or, the acidic solution is a monobasic acid solution, the mass fraction of the monobasic acid solution is 10-35%, preferably the monobasic acid is hydrochloric acid and / or nitric acid; and / or, the alkaline solution includes a monobasic alkali and water, the mass ratio of the residue, the monobasic alkali and water is 1.5-100:40-60:50-400; and / or, the monobasic alkali is NaOH and / or KOH; preferably, the waste molecular sieve is any one or more of waste HZSM-5 molecular sieve catalyst, waste MTO catalyst, fly ash, waste FCC catalyst, and waste VOC adsorbent; the sodium salt is Na2SO4 and / or NaCO3.

[0016] According to another aspect of the present invention, a core-shell structure cracking reaction catalyst is provided. The core-shell structure cracking reaction catalyst is prepared by the aforementioned preparation method.

[0017] Applying the technical solution of the present application, the steps S3 and S4 of the present application optimize the structure of the 13X molecular sieve, forming a core-shell structure 13X molecular sieve with the 13X molecular sieve as the core, the nickel nanoparticles as the intermediate layer, and the titanium silicon molecular sieve as the shell, in the process, the 13X molecular sieve is sequentially subjected to the first impregnation treatment and the second impregnation treatment, and the nickel nanoparticle intermediate layer and the titanium silicon molecular sieve shell can be sequentially formed on the surface of the 13X molecular sieve to form a gradient structure, which helps to improve the mechanical strength and thermal stability of the molecular sieve. And in the process, the structure of the 13X molecular sieve is greatly optimized, so that the obtained core-shell structure 13X molecular sieve has a certain range of parameters such as specific surface area and porosity. Therefore, the core-shell structure cracking reaction catalyst prepared by the core-shell structure 13X molecular sieve has excellent cracking reaction catalytic activity, and the core-shell structure cracking reaction catalyst is applied to the cracking reaction, which helps to improve the reaction efficiency of the cracking reaction. In addition, the 13X molecular sieve prepared using waste catalyst as raw material in steps S1 and S2 of the present application, on the one hand, realizes waste utilization and reduces the cost of preparing the 13X molecular sieve. On the other hand, the 13X molecular sieve prepared by the method of the present application has the characteristics of a higher silicon-to-aluminum ratio, a larger pore volume and specific surface area, and a regular morphology, which helps to improve the silicon source utilization rate of the 13X molecular sieve, provide more catalytic active sites for the cracking reaction catalytic process, and improve the flow and diffusion performance of the reactants inside the molecular sieve, thereby improving the reaction efficiency and reaction effect of the catalytic cracking reaction of materials such as petroleum. DETAILED DESCRIPTION

[0018] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present invention will be described in detail below in conjunction with the embodiments.

[0019] As analyzed in the background technology of the present application, the prior art has the problem of low cracking reaction efficiency. In order to solve this problem, the present application provides a core-shell structure cracking reaction catalyst and a preparation method thereof.

[0020] In a typical embodiment of the present application, a preparation method for a core-shell structure cracking reaction catalyst is provided, and the preparation method comprises the following steps: step S1, sequentially subjecting waste molecular sieves to aluminum dissolution treatment and silicon dissolution treatment to obtain aluminum-rich liquid and silicon-rich liquid; step S2, sequentially subjecting raw materials including aluminum-rich liquid, silicon-rich liquid and seed crystals to gelation treatment, aging treatment and hydrothermal crystallization treatment to obtain 13X molecular sieve; step S3, sequentially subjecting the 13X molecular sieve to a first impregnation treatment and a second impregnation treatment in a silanization agent solution and a nickel-containing solution to obtain a nickel-modified 13X molecular sieve; step S4, sequentially subjecting the nickel-modified 13X molecular sieve and a titanium silicon molecular sieve precursor solution to a first hydrothermal reaction and a calcination treatment to obtain a core-shell structure 13X molecular sieve; and step S5, mixing and stirring the core-shell structure 13X molecular sieve and a platinum precursor solution, and sequentially subjecting the mixture to solid-liquid separation, drying, a pre-calcination treatment and a first calcination treatment to obtain a core-shell structure cracking reaction catalyst.

[0021] The steps S3 and S4 of the present application optimize the structure of the 13X molecular sieve to form a core-shell structure 13X molecular sieve with the 13X molecular sieve as the core, the nickel nanoparticles as the intermediate layer, and the titanium silicon molecular sieve as the shell. In this process, the 13X molecular sieve is sequentially subjected to the first impregnation treatment and the second impregnation treatment, and the nickel nanoparticle intermediate layer and the titanium silicon molecular sieve shell can be sequentially formed on the surface of the 13X molecular sieve to form a gradient structure, which helps to improve the mechanical strength and thermal stability of the molecular sieve. And in this process, the structure of the 13X molecular sieve is greatly optimized, so that the obtained core-shell structure 13X molecular sieve has a certain range of parameters such as specific surface area and porosity. Therefore, the core-shell structure cracking reaction catalyst prepared by the core-shell structure 13X molecular sieve has excellent cracking reaction catalytic activity, and the core-shell structure cracking reaction catalyst is applied to the cracking reaction, which helps to improve the reaction efficiency of the cracking reaction. In addition, the 13X molecular sieve prepared using waste catalyst as raw material in steps S1 and S2 of the present application, on the one hand, realizes waste utilization and reduces the cost of preparing the 13X molecular sieve. On the other hand, the 13X molecular sieve prepared by the method of the present application has the characteristics of a higher silicon-to-aluminum ratio, a larger pore volume and specific surface area, and a regular morphology, which helps to improve the silicon source utilization rate of the 13X molecular sieve, provide more catalytic active sites for the cracking reaction catalytic process, and improve the flow and diffusion performance of the reactants inside the molecular sieve, thereby improving the reaction efficiency and reaction effect of the catalytic cracking reaction of materials such as petroleum.

[0022] In one embodiment of the present application, in the above step S3: the time of the first impregnation treatment is 8 to 24 hours, and / or the time of the second impregnation treatment is 24 to 48 hours; preferably, the molar concentration of the silanization agent solution is 0.05 to 0.2 mol / L, and / or the molar concentration of the nickel-containing solution is 0.05 to 0.2 mol / L; preferably, the mass ratio of the 13X molecular sieve to the volume ratio of the silanization agent solution is 400 to 600:1 g / L; and / or, the mass ratio of the 13X molecular sieve to the volume ratio of the nickel-containing solution is 40 0~600:1g / L; preferably, the nickel-containing solution is selected from nickel nitrate solution and / or nickel sulfate solution; preferably, the silanization agent is selected from any one or more of 3-aminopropyltriethoxysilane, tetraethoxysilane and tetramethoxysilane; preferably, step S3 also includes: subjecting the 13X molecular sieve obtained by the second impregnation treatment to a third calcination to obtain a nickel-modified 13X molecular sieve coated with a nickel nanoparticle layer; and / or the atmosphere of the third calcination is hydrogen, the temperature of the third calcination is 500~600℃, and the time of the third calcination is 2~4h.

[0023] It is preferred to control the time of the first impregnation treatment, the time of the second impregnation treatment, the molar concentration of the silanization agent solution and the molar concentration of the nickel-containing solution within the above ranges, which helps to control the quality of the nickel nanoparticles finally formed and improve the wetting effect of the silanization agent solution and the nickel-containing solution on the 13X molecular sieve; it is preferred to control the types of the nickel-containing solution and the silanization agent within the above ranges, which helps to enrich the selectivity of the nickel-containing solution and the silanization agent.

[0024] The nickel compound attached to the surface of the 13X molecular sieve in the third calcination is decomposed at high temperature to form nickel oxide, and hydrogen reduces the nickel oxide to nickel nanoparticles. Preferably, controlling the temperature and time of the third calcination within the above range helps to improve the efficiency of forming nickel nanoparticles.

[0025] In one embodiment of the present application, in the above step S4, the temperature of the first hydrothermal reaction is 150-200°C, and the time of the first hydrothermal reaction is 12-24h; and / or the temperature of the calcination treatment is 450-550°C, and the time of the calcination treatment is 4-8h; the titanium silicon molecular sieve precursor solution includes a first silicon source, a titanium source, a template, a fluorine complex and water, wherein the first silicon source, the titanium source, the template, the fluorine complex and the water are in a molar ratio of 1:0.04-0.1:0.1-0.3:0.03-0.06:20 ~50 mixed; and / or, the ratio of the mass of nickel-modified 13X molecular sieve to the volume of the titanium silicon molecular sieve precursor solution is 400~600:1g / L; preferably, the first silicon source is selected from any one or more of SiO2, Na2SiO3 and Si(OC2H5)4; preferably, the titanium source is selected from any one or more of TiO2, TiCl4 and Na2TiO3; preferably, the fluorine complex is selected from any one or more of sodium hexafluorophosphate, sodium hexafluoroacetylacetonate and ammonium fluoride; preferably, the template is an organic amine and / or a quaternary ammonium salt.

[0026] It is preferred to control the temperature and time of the first hydrothermal reaction within the above range, which helps to improve the interaction between the titanium silicon molecular sieve precursor and the nickel-modified 13X molecular sieve. It is preferred to control the temperature and time of the calcination treatment within the above range, which helps to improve the structural integrity of the core-shell structure 13X molecular sieve finally formed. It is preferred to control the molar ratio of the first silicon source, titanium source, template agent, fluorine complex and water within the above range, which helps to improve the uniformity of the pore size of the core-shell structure 13X molecular sieve. It is preferred to control the types of silicon source, titanium source, template agent and fluorine complex within the above range, which helps to improve the synergistic effect between the components, so that the coating formed on the surface of the 13X molecular sieve has higher catalytic activity and stability.

[0027] In one embodiment of the present application, in the above step S5, the mixing and stirring time is 12 to 36 hours; the weight concentration of the platinum precursor solution is 2 to 3 g / L; the preferred platinum precursor solution is hexachloroplatinic acid dihydrate; the volume ratio of the mass of the core-shell structure 13X molecular sieve to the platinum precursor solution is 1:5 g / L; the atmosphere of the pre-calcination treatment is an inert gas, the temperature of the pre-calcination treatment is 450 to 550°C, and the time of the pre-calcination treatment is 1 to 3 hours; the temperature of the first calcination treatment is 700 to 900°C, the time of the first calcination treatment is 3 to 5 hours, and the atmosphere of the first calcination treatment is air; the drying temperature is 90 to 130°C, and the drying time is 8 to 16 hours.

[0028] In order to control the amount of platinum salt attached to the core-shell structure 13X molecular sieve and improve the wetting effect of the platinum precursor solution on the core-shell structure 13X molecular sieve, thereby improving the catalytic efficiency of the core-shell structure cracking reaction catalyst, it is preferred to control the mixing and stirring time and the molar concentration of the platinum precursor solution within the above range. It is preferred to control the temperature, time and atmosphere of the pre-baking treatment and the first calcination treatment within the above range, which helps to improve the efficiency of the platinum salt on the core-shell structure 13X molecular sieve to form metal platinum oxide or platinum metal; it is preferred to control the drying temperature and time within the above range, which helps to remove moisture from the core-shell structure 13X molecular sieve.

[0029] In one embodiment of the present application, in the above step S2, the 13X molecular sieve contains silicon and aluminum, and the molar ratio of silicon to aluminum is 2.2 to 2.9:1; and / or the pore volume of the 13X molecular sieve is 0.3 to 0.5 cm 3 / g, and / or the specific surface area of ​​13X molecular sieve is 700-950m 2 / g.

[0030] Preferably, the prepared 13X molecular sieve has the above properties through steps S1 and S2 of the present application. Among them, the molar ratio of silicon element to aluminum element is preferably within the above range, which helps to improve the utilization rate of silicon source in 13X molecular sieve; the pore volume and specific surface area of ​​13X molecular sieve are preferably within the above range, which helps to provide more catalytic active sites for the cracking reaction catalytic process and is conducive to improving the circulation and diffusion performance of reactant molecules inside the molecular sieve.

[0031] In order to improve the formation and stability of the 13X molecular sieve framework structure, in one embodiment of the present application, the above-mentioned seed crystals preferably contain SiO2, Al2O3, Na2O and H2O, wherein the molar ratio of SiO2 to Al2O3 is 0.01 to 2.5:1, and the molar ratio of Na2O, H2O and SiO2 is 0.01 to 4.0:1.0 to 40.0:1.

[0032] To further promote the smooth formation of the structure of the 13X molecular sieve, in one embodiment of the present application, the above-mentioned step S2 preferably includes: step S21, gelling the aluminum-rich liquid and the silicon-rich liquid to obtain a first gel; step S22, aging the first gel and the seed crystal in turn, hydrothermal crystallization treatment, to obtain a 13X molecular sieve; wherein the first gel contains SiO2, Al2O3, Na2O and H2O, wherein the molar ratio of SiO2 to Al2O3 is 0.5-6.0:1, and the molar ratio of Na2O, H2O to SiO2 is 0.5-6.0:10-100:1; preferably, the mass ratio of the seed crystal to the first gel is 5-20:100; and / or the aging treatment temperature is 20-100°C, and the aging treatment time is 0.1-24h; and / or the hydrothermal crystallization treatment temperature is 60-105°C, and the hydrothermal crystallization treatment time is 0.1-36h.

[0033] Furthermore, it is preferred that the aging process be carried out under stirring.

[0034] In order to promote the formation of 13X molecular sieve crystals, in one embodiment of the present application, the above-mentioned preparation method preferably also includes: a seed crystal preparation process, the preparation process includes: stirring and mixing the raw materials including the aluminum source, the second silicon source and water to obtain a second gel; adjusting the pH value of the second gel to 8.5-12.5 and then performing two-stage hydrothermal crystallization treatment to obtain a seed crystal; wherein the stirring and mixing rate is 200-800 rpm, and / or the stirring and mixing temperature is 20-100°C, and / or the stirring and mixing time is 0.1-24h; preferably, the pH value of the second gel is 11.8-12.2; further preferably, the pH value of the above-mentioned second gel is 12. Preferably, the second silicon source is selected from any one or more of silica sol, tetraethyl orthosilicate and silicon powder; preferably, the aluminum source is selected from any one or more of sodium aluminate, pseudo-boehmite, aluminum sulfate and aluminum nitrate.

[0035] In order to improve the crystallization degree of 13X molecular sieve, it is preferred that the two-stage hydrothermal crystallization treatment includes a first stage hydrothermal crystallization treatment and a second stage hydrothermal crystallization treatment, wherein the temperature of the first stage hydrothermal crystallization treatment is 20-60°C, and / or the time of the first stage hydrothermal crystallization treatment is 4-24h; preferably, the temperature of the second stage hydrothermal crystallization treatment is 80-120°C, and / or the time of the second stage hydrothermal crystallization treatment is 6-48h; further, it is preferred that the temperature of the first stage hydrothermal crystallization treatment is 35-45°C, and / or the first stage hydrothermal crystallization treatment is 50-60°C. The time of thermal crystallization treatment is 11 to 13 hours; the temperature of the second hydrothermal crystallization treatment is 90 to 100°C, and / or the time of the second hydrothermal crystallization treatment is 22 to 26 hours; the temperature of the second hydrothermal crystallization treatment is 50 to 60°C higher than the temperature of the first hydrothermal crystallization treatment; it is further preferred that the temperature of the first hydrothermal crystallization treatment is 40°C, and / or the time of the first hydrothermal crystallization treatment is 12 hours; the temperature of the second hydrothermal crystallization treatment is 95°C, and / or the time of the second hydrothermal crystallization treatment is 24 hours.

[0036] In addition, in order to further improve the mixing effect of the aluminum source, the silicon source and the water, the specific steps of stirring and mixing the raw materials of the aluminum source, the second silicon source and the water preferably include: stirring and mixing the silicon source and the water, the stirring and mixing temperature is 20 to 60°C, the stirring and mixing time is 0.1 to 12h, the stirring and mixing speed is 200 to 800rpm, and a silicon-containing solution is obtained, and the concentration of the silicon-containing solution is 28% to 99wt%; stirring and mixing the aluminum source and the water, the stirring and mixing temperature is 20 to 60°C, the stirring and mixing time is 0.1 to 12h, and the stirring and mixing speed is 200 to 800rpm, and an aluminum-containing solution is obtained, and the concentration of the aluminum-containing solution is 28% to 99wt%, and the silicon-containing solution and the aluminum-containing solution are stirred and mixed to obtain a second gel.

[0037] Preferably, the pH value of the second gel is adjusted by slowly adding a solid base or an aqueous solution of the base to the second gel; preferably, the base is selected from sodium hydroxide and / or potassium hydroxide. Preferably, after the first hydrothermal crystallization treatment in step S22, the reaction product is filtered and washed to neutrality, and then dried at 80-120° C. until there is no obvious weight loss to obtain a 13X molecular sieve.

[0038] In order to remove impurities such as moisture and carbon deposits in the waste molecular sieve, and further reduce the preparation cost of 13X molecular sieve and increase the pore volume and specific surface area of ​​13X molecular sieve, in one embodiment of the present application, it is preferred that the above-mentioned preparation method also includes a process of pretreating the waste molecular sieve, and the pretreatment process includes: sintering a mixture including the waste molecular sieve and sodium salt to obtain a sintered product; using an acidic solution to sequentially perform aluminum dissolution treatment and solid-liquid separation on the sintered product to obtain an aluminum-rich liquid and a residue; using an alkaline solution to sequentially perform silicon dissolution treatment and solid-liquid separation on the residue to obtain a silicon-rich liquid; wherein the mass ratio of the waste molecular sieve to the sodium salt is 1:0.5~5; and / or sintering treatment The temperature is 550-800°C, and / or the sintering treatment time is 60-120min; and / or the acidic solution is a monobasic acid solution, and the mass fraction of the monobasic acid solution is 10-35%; preferably, the monobasic acid is hydrochloric acid and / or nitric acid; and / or the alkaline solution includes a monobasic alkali and water, and the mass ratio of the residue, the monobasic alkali and water is 1.5-100:40-60:50-400; and / or the monobasic alkali is NaOH and / or KOH; preferably, the waste molecular sieve is selected from any one or more of waste HZSM-5 molecular sieve catalyst, waste MTO catalyst, fly ash, waste FCC catalyst, and waste VOC adsorbent; the sodium salt is Na2SO4 and / or NaCO3.

[0039] Furthermore, it is preferred that the size of the spent molecular sieve is less than 200 mesh.

[0040] In another typical embodiment of the present application, a core-shell structure cracking reaction catalyst is provided. The core-shell structure cracking reaction catalyst is prepared by the aforementioned preparation method.

[0041] The core-shell structure cracking reaction catalyst obtained by the preparation method of the present application has excellent cracking reaction catalytic activity and stability, can achieve efficient cracking reaction at a lower temperature, and the core-shell structure cracking reaction catalyst is applied to the cracking reaction, which helps to improve the reaction efficiency of the cracking reaction. In addition, the core-shell structure cracking reaction catalyst prepared by the preparation method of the present application can be applied to petroleum cracking, waste plastic treatment and other complex organic matter conversion reactions, and has a wide range of application potential.

[0042] The beneficial effects of the present application will be further illustrated below in conjunction with embodiments.

[0043] Example 1

[0044] Preparation of 13X molecular sieve seed crystals: 21.0 g of silica sol (mass fraction of 30%) was dissolved in 36.0 g of deionized water, and pretreated in a closed reactor at 25°C for 1 hour to obtain a silicon-containing solution; 24 g of aluminum sulfate was dissolved in 18.0 g of deionized water, and stirred at 25°C for 1 hour to obtain an aluminum-containing solution; the aluminum-containing solution was slowly added dropwise to the silicon-containing solution, and the solution after the addition was stirred at 60°C for 8 hours to obtain a gel mixture; 6.74 g of sodium hydroxide was dissolved in 36 g of deionized water to obtain a sodium hydroxide aqueous solution. , adding sodium hydroxide aqueous solution to the gel mixture, controlling the pH value of the gel mixture to maintain at 12, obtaining a second gel, placing the second gel in a hydrothermal reactor, and performing two hydrothermal crystallization treatments, wherein the temperature of the first hydrothermal crystallization treatment is 40°C, the time of the first hydrothermal crystallization treatment is 12 hours, and the temperature of the second hydrothermal crystallization treatment is 95°C, the time of the second hydrothermal crystallization treatment is 24 hours, and a 13X molecular sieve seed solution is obtained, and the 13X molecular sieve seed solution is filtered, washed, and dried in sequence to obtain a 13X molecular sieve seed. The molar ratio of SiO2 to Al2O3 in the 13X molecular sieve seed is 1.5:1, and the molar ratio of Na2O, H2O to SiO2 is 1.6:32:1.

[0045] Preparation of 13X molecular sieve: The waste Z-5 molecular sieve catalyst is mixed with NaCO3 in a mass ratio of 1:2.5 for sintering treatment. The sintering temperature is 600°C and the sintering time is 100 min. The sintered product is then subjected to aluminum dissolution treatment with hydrochloric acid having a mass concentration of 25%, and then filtered to obtain aluminum-rich liquid and residue; the residue is mixed with NaOH and H2O in a mass ratio of 50:50:200 for silicon dissolution treatment, and then filtered to obtain silicon-rich liquid; the silicon-rich liquid and the aluminum-rich liquid are mixed to obtain a first gel; the above-mentioned 13X molecular sieve seed crystals and the first gel are mixed in a mass ratio of 10:100, and then aged and hydrothermally crystallized in sequence. The aging temperature is 50°C and the aging time is 12 h; the hydrothermal crystallization temperature is 70°C and the hydrothermal crystallization time is 24 h, and then dried to obtain 13X molecular sieve. The molar ratio of SiO2 to Al2O3 in the first gel is 3.5:1, the molar ratio of Na2O, H2O to SiO2 is 2.8:80:1, and the molar ratio of silicon to aluminum in the 13X molecular sieve is 2.60:1; the pore volume of the 13X molecular sieve is 0.4789 cm 3 / g, the specific surface area of ​​13X molecular sieve is 877.2m 2 / g.

[0046] Preparation of core-shell structure 13X molecular sieve: 300g of the above 13X molecular sieve powder is placed in 500mL of 0.2mol / L 3-aminopropyltriethoxysilane solution for a first impregnation treatment, and the first impregnation treatment time is 8 hours; then 300g of the treated 13X molecular sieve is placed in 500mL of 0.2mol / L nickel nitrate solution for a second impregnation treatment, and the second impregnation treatment time is 24 hours; the 13X molecular sieve after the second impregnation treatment is subjected to a third calcination in a hydrogen atmosphere at 500°C, and the third calcination time is 2 hours to obtain a nickel-modified 13X molecular sieve containing a nickel nanoparticle deposition layer, SiO2, TiO2, tetraethylammonium hydroxide, sodium hexafluorophosphate and water are added to the mixture. Mix to prepare a titanium silicon molecular sieve precursor solution, wherein the molar ratio of SiO2, TiO2, organic amine, sodium hexafluorophosphate and water is 1:0.06:0.15:0.04:40; add 150g of 13X molecular sieve containing a nickel nanoparticle deposition layer to 250mL of the titanium silicon molecular sieve precursor solution, mix thoroughly, and transfer to a reactor for a first hydrothermal reaction at a temperature of 150°C for 12h; after the reaction is completed, take out the solid and wash it with water, then dry it at 110°C for 12 hours, and calcine the dried solid at a temperature of 450°C for 4h to obtain a core-shell structure 13X molecular sieve.

[0047] Preparation of core-shell structure cracking reaction catalyst: Dissolve 1g of hexachloroplatinic acid dihydrate in 500mL of deionized water to form a platinum precursor solution, add 100g of core-shell structure 13X molecular sieve to the prepared platinum precursor solution, use a magnetic stirrer to fully stir for 24 hours and filter, place the filtered core-shell structure 13X molecular sieve in a drying oven, and dry it at 110°C for 12h. The dried core-shell structure 13X molecular sieve is placed in a molybdenum cloth furnace, pre-baked at 500°C in a nitrogen atmosphere for 2h, and then calcined at 800°C in an air atmosphere for 4 hours. A core-shell structure cracking reaction catalyst is obtained.

[0048] Example 2

[0049] The difference from Example 1 is that the 13X molecular sieve seed crystals are prepared as follows: 1 g of silicon powder is dissolved in 18.0 g of deionized water, and the mixture is pretreated at 25° C. for 1 hour in a sealed reactor to obtain a silicon-containing solution; 12 g of aluminum sulfate is dissolved in 18.0 g of deionized water, and the mixture is stirred at 35° C. for 1 hour to obtain an aluminum-containing solution; the aluminum-containing solution is slowly added dropwise to the silicon-containing solution, and the solution after the addition is stirred at 50° C. for 6 hours to obtain a gel mixture; 2 g of sodium hydroxide is dissolved in 36 g of deionized water to obtain a sodium hydroxide aqueous solution, and the sodium hydroxide aqueous solution is added to the mixture. In the gel mixture, the pH value of the gel mixture is controlled to be maintained at 11.8 to obtain a second gel, and the second gel is placed in a hydrothermal reactor for two-stage hydrothermal crystallization treatment, the temperature of the first stage of hydrothermal crystallization treatment is 50°C, the time of the first stage of hydrothermal crystallization treatment is 14 hours, the temperature of the second stage of hydrothermal crystallization treatment is 100°C, the time of the second stage of hydrothermal crystallization treatment is 18 hours, and a 13X molecular sieve seed solution is obtained, and the 13X molecular sieve seed solution is filtered, washed, and dried in sequence to obtain 13X molecular sieve seeds, and finally a core-shell structure cracking reaction catalyst is obtained. Among them, the molar ratio of SiO2 to Al2O3 of the 13X molecular sieve seeds is 0.6:1, the molar ratio of Na2O, H2O to SiO2 is 3:20:1, the silicon-aluminum ratio of the 13X molecular sieve is 2.40:1; the pore volume of the 13X molecular sieve is 0.4590cm 3 / g, the specific surface area of ​​13X molecular sieve is 873.2m 2 / g.

[0050] Example 3

[0051] The difference from Example 1 is that the preparation of 13X molecular sieve seed crystals is as follows: 0.17 g of silicon powder is dissolved in 6 g of deionized water, and pretreated in a closed reactor at 25° C. for 1 hour to obtain a silicon-containing solution; 12 g of aluminum sulfate is dissolved in 18 g of deionized water, and stirred at 35° C. for 1 hour to obtain an aluminum-containing solution; the aluminum-containing solution is slowly added dropwise to the silicon-containing solution, and the solution after the addition is stirred at 100° C. for 24 hours to obtain a gel mixture; 0.9 g of sodium hydroxide is dissolved in 6 g of deionized water to obtain a sodium hydroxide aqueous solution, and the sodium hydroxide aqueous solution is added In the gel mixture, the pH value of the gel mixture is controlled to be maintained at 12.5 to obtain a second gel, and the second gel is placed in a hydrothermal reactor for two-stage hydrothermal crystallization treatment, the temperature of the first stage of hydrothermal crystallization treatment is 60°C, the time of the first stage of hydrothermal crystallization treatment is 24 hours, the temperature of the second stage of hydrothermal crystallization treatment is 120°C, the time of the second stage of hydrothermal crystallization treatment is 48 hours, and a 13X molecular sieve seed solution is obtained, and the 13X molecular sieve seed solution is filtered, washed, and dried in sequence to obtain 13X molecular sieve seeds, and finally a core-shell structure cracking reaction catalyst is obtained. Among them, the molar ratio of SiO2 to Al2O3 of the 13X molecular sieve seeds is 0.1:1, the molar ratio of Na2O, H2O to SiO2 is 4:1:1, the silicon-aluminum ratio of the 13X molecular sieve is 2.23:1; the pore volume of the 13X molecular sieve is 0.3693cm 3 / g, the specific surface area of ​​13X molecular sieve is 801.2m 2 / g.

[0052] Example 4

[0053] The difference from Example 1 is that the 13X molecular sieve seed crystals are prepared as follows: 14.65 g of tetraethyl orthosilicate is dissolved in 36.0 g of deionized water, and pretreated in a closed reactor at 25° C. for 1 hour to obtain a silicon-containing solution; 12 g of aluminum sulfate is dissolved in 18.0 g of deionized water, and stirred at 35° C. for 1 hour to obtain an aluminum-containing solution; the aluminum-containing solution is slowly added dropwise to the silicon-containing solution, and the solution after the addition is stirred at 20° C. for 0.1 hour to obtain a gel mixture; 0.56 g of sodium hydroxide is dissolved in 6 g of deionized water to obtain a sodium hydroxide aqueous solution, and the sodium hydroxide solution is added dropwise to the silicon-containing solution. Sodium hydroxide aqueous solution is added to the gel mixture, and the pH value of the gel mixture is controlled to be maintained at 8.5 to obtain a second gel, which is placed in a hydrothermal reactor for two-stage hydrothermal crystallization treatment. The temperature of the first stage of hydrothermal crystallization treatment is 20°C, and the time of the first stage of hydrothermal crystallization treatment is 4 hours. The temperature of the second stage of hydrothermal crystallization treatment is 80°C, and the time of the second stage of hydrothermal crystallization treatment is 6 hours to obtain a 13X molecular sieve seed solution. The 13X molecular sieve seed solution is filtered, washed, and dried in sequence to obtain a 13X molecular sieve seed, and finally a core-shell structure cracking reaction catalyst is obtained. Among them, the molar ratio of SiO2 to Al2O3 of the 13X molecular sieve seed is 2.5:1, the molar ratio of Na2O, H2O to SiO2 is 0.01:40:1, and the silicon-aluminum ratio of the 13X molecular sieve is 2.87:1; the pore volume of the 13X molecular sieve is 0.3916cm 3 / g, the specific surface area of ​​13X molecular sieve is 821.1m 2 / g.

[0054] Example 5

[0055] The difference from Example 1 is that the time of the first impregnation treatment is 24 hours, and the time of the second impregnation treatment is 48 hours; the molar concentration of the silanization agent solution is 0.05 mol / L, and the molar concentration of the nickel-containing solution is 0.05 mol / L, and finally a core-shell structure cracking reaction catalyst is obtained.

[0056] Example 6

[0057] The difference from Example 1 is that the time of the first impregnation treatment is 7 hours, and the time of the second impregnation treatment is 20 hours; the molar concentration of the silanization agent solution is 0.04 mol / L, and the molar concentration of the nickel-containing solution is 0.04 mol / L, and finally a core-shell structure cracking reaction catalyst is obtained.

[0058] Example 7

[0059] The difference from Example 1 is that the temperature of the third calcination is 600° C., the time of the third calcination is 4 hours, and finally a core-shell structure cracking reaction catalyst is obtained.

[0060] Example 8

[0061] The difference from Example 1 is that the temperature of the third calcination is 400° C., the time of the third calcination is 1 hour, and finally a core-shell structure cracking reaction catalyst is obtained.

[0062] Example 9

[0063] The difference from Example 1 is that the temperature of the first hydrothermal reaction is 200° C., and the time of the first hydrothermal reaction is 24 h; the temperature of the calcination treatment is 550° C., and the time of the calcination treatment is 8 h, and finally a core-shell structure cracking reaction catalyst is obtained.

[0064] Example 10

[0065] The difference from Example 1 is that the temperature of the first hydrothermal reaction is 140° C., and the time of the first hydrothermal reaction is 10 h; the temperature of the calcination treatment is 400° C., and the time of the calcination treatment is 3 h, and finally a core-shell structure cracking reaction catalyst is obtained.

[0066] Embodiment 11

[0067] The difference from Example 1 is that the molar ratio of SiO2, TiO2, tetraethylammonium hydroxide, sodium hexafluorophosphate and water is 1:0.04:0.1:0.03:20, and a core-shell structure cracking reaction catalyst is finally obtained.

[0068] Example 12

[0069] The difference from Example 1 is that the molar ratio of SiO2, TiO2, tetraethylammonium hydroxide, sodium hexafluorophosphate and water is 1:0.1:0.3:0.06:50, and a core-shell structure cracking reaction catalyst is finally obtained.

[0070] Example 13

[0071] The difference from Example 1 is that the molar ratio of SiO2, TiO2, tetraethylammonium hydroxide, sodium hexafluorophosphate and water is 1:0.2:0.4:0.07:60, and a core-shell structure cracking reaction catalyst is finally obtained.

[0072] Embodiment 14

[0073] The difference from Example 1 is that the mass concentration of the platinum precursor solution is 3 g / L, and a core-shell structure cracking reaction catalyst is finally obtained.

[0074] Embodiment 15

[0075] The difference from Example 1 is that the mass concentration of the platinum precursor solution is 1 g / L, and a core-shell structure cracking reaction catalyst is finally obtained.

[0076] Comparative Example 1

[0077] The difference from Example 1 is that 13X molecular sieve is directly used for the preparation of cracking reaction catalyst, and finally a cracking reaction catalyst is obtained.

[0078] Test Method

[0079] Catalytic cracking process

[0080] The cracking reaction catalysts obtained in the above-mentioned embodiments and comparative examples were used for naphtha steam cracking reaction, and the specific reaction conditions were: reaction temperature of 550°C, reaction pressure of 80KPa, reaction time of 2 hours, and water-oil mass ratio of 0.6. The yield of trienes (ethylene, propylene, butadiene) and the selectivity of triene conversion are shown in Table 1.

[0081] Table 1

[0082]

[0083]

[0084] From the above description, it can be seen that the above embodiments of the present invention achieve the following technical effects:

[0085] The steps S3 and S4 of the present application optimize the structure of the 13X molecular sieve to form a core-shell structure 13X molecular sieve with the 13X molecular sieve as the core, the nickel nanoparticles as the intermediate layer, and the titanium silicon molecular sieve as the shell. In this process, the 13X molecular sieve is sequentially subjected to the first impregnation treatment and the second impregnation treatment, and the nickel nanoparticle intermediate layer and the titanium silicon molecular sieve shell can be sequentially formed on the surface of the 13X molecular sieve to form a gradient structure, which helps to improve the mechanical strength and thermal stability of the molecular sieve. And in this process, the structure of the 13X molecular sieve is greatly optimized, so that the obtained core-shell structure 13X molecular sieve has a certain range of parameters such as specific surface area and porosity. Therefore, the core-shell structure cracking reaction catalyst prepared by the core-shell structure 13X molecular sieve has excellent cracking reaction catalytic activity, and the core-shell structure cracking reaction catalyst is applied to the cracking reaction, which helps to improve the reaction efficiency of the cracking reaction. In addition, the 13X molecular sieve prepared using waste catalyst as raw material in steps S1 and S2 of the present application, on the one hand, realizes waste utilization and reduces the cost of preparing the 13X molecular sieve. On the other hand, the 13X molecular sieve prepared by the method of the present application has the characteristics of a higher silicon-to-aluminum ratio, a larger pore volume and specific surface area, and a regular morphology, which helps to improve the silicon source utilization rate of the 13X molecular sieve, provide more catalytic active sites for the cracking reaction catalytic process, and improve the flow and diffusion performance of the reactants inside the molecular sieve, thereby improving the reaction efficiency and reaction effect of the catalytic cracking reaction of materials such as petroleum.

[0086] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a core-shell structure cracking reaction catalyst, characterized in that: The preparation method comprises the following steps: Step S1, subjecting the waste molecular sieve to aluminum dissolution treatment and silicon dissolution treatment in sequence to obtain aluminum-rich liquid and silicon-rich liquid; Step S2, subjecting the raw materials including the aluminum-rich liquid, the silicon-rich liquid and the seed crystal to gelation treatment, aging treatment and hydrothermal crystallization treatment in sequence to obtain a 13X molecular sieve; Step S3, performing a first impregnation treatment and a second impregnation treatment on the 13X molecular sieve in a silanization agent solution and a nickel-containing solution in sequence to obtain a nickel-modified 13X molecular sieve; Step S4, subjecting the nickel-modified 13X molecular sieve and the titanium silicon molecular sieve precursor solution to a first hydrothermal reaction and a calcination treatment in sequence to obtain a core-shell structure 13X molecular sieve; and Step S5, mixing the core-shell structure 13X molecular sieve with a platinum precursor solution, and then sequentially performing solid-liquid separation, drying, pre-baking treatment, and first calcination treatment to obtain a core-shell structure cracking reaction catalyst.

2. The preparation method according to claim 1, characterized in that: In step S3: The first immersion treatment time is 8 to 24 hours; and / or the second immersion treatment time is 24 to 48 hours; Preferably, the molar concentration of the silanization agent solution is 0.05-0.2 mol / L; and / or, the molar concentration of the nickel-containing solution is 0.05-0.2 mol / L; preferably, the mass ratio of the 13X molecular sieve to the volume ratio of the silanization agent solution is 400-600:1 g / L; and / or, the mass ratio of the 13X molecular sieve to the volume ratio of the nickel-containing solution is 400-600:1 g / L; Preferably, the nickel-containing solution is a nickel nitrate solution and / or a nickel sulfate solution; Preferably, the silanization agent is selected from any one or more of 3-aminopropyltriethoxysilane, tetraethoxysilane and tetramethoxysilane; Preferably, step S3 further includes: The 13X molecular sieve obtained by the second impregnation treatment is subjected to a third calcination to obtain the nickel-modified 13X molecular sieve coated with a nickel nanoparticle layer; And / or, the atmosphere of the third calcination is hydrogen, the temperature of the third calcination is 500-600° C., and the time of the third calcination is 2-4 hours.

3. The preparation method according to claim 1 or 2, characterized in that: In the step S4, The temperature of the first hydrothermal reaction is 150-200° C., and the time of the first hydrothermal reaction is 12-24 hours; And / or, the temperature of the calcination treatment is 450-550° C., and the time of the calcination treatment is 4-8 hours; The titanium silicon molecular sieve precursor solution comprises a first silicon source, a titanium source, a template, a fluorine complex and water, wherein the first silicon source, the titanium source, the template, the fluorine complex and the water are mixed in a molar ratio of 1:0.04-0.1:0.1-0.3:0.03-0.06:20-50; and / or, the ratio of the mass of the nickel-modified 13X molecular sieve to the volume of the titanium silicon molecular sieve precursor solution is 400-600:1 g / L; Preferably, the first silicon source is selected from any one or more of SiO2, Na2SiO3 and Si(OC2H5)4; Preferably, the titanium source is selected from any one or more of TiO2, TiCl4 and Na2TiO3; Preferably, the fluorine complex is selected from any one or more of sodium hexafluorophosphate, sodium hexafluoroacetylacetonate and ammonium fluoride; Preferably, the template is an organic amine and / or a quaternary ammonium salt.

4. The preparation method according to any one of claims 1 to 3, characterized in that In the step S5, Stirring is performed during the mixing process, and the stirring time is preferably 12 to 36 hours; the mass concentration of the platinum precursor solution is preferably 2 to 3 g / L; the platinum precursor solution is preferably hexachloroplatinic acid dihydrate; the mass ratio of the core-shell structure 13X molecular sieve to the volume ratio of the platinum precursor solution is preferably 1:5 g / L; and / or, the atmosphere of the pre-calcination treatment is an inert gas, and / or, the temperature of the pre-calcination treatment is 450 to 550° C.; and / or, the time of the pre-calcination treatment is 1 to 3 hours; and / or, the temperature of the first calcination treatment is 700-900° C.; and / or, the time of the first calcination treatment is 3-5 hours; and / or, the atmosphere of the first calcination treatment is air; And / or, the drying temperature is 90-130° C., and the drying time is 8-16 hours.

5. The preparation method according to any one of claims 1 to 4, characterized in that: In step S2, the 13X molecular sieve contains silicon and aluminum, and the molar ratio of the silicon to the aluminum is 2.2 to 2.9:1; and / or the pore volume of the 13X molecular sieve is 0.3 to 0.5 cm 3 / g; and / or, the specific surface area of ​​the 13X molecular sieve is 700 to 950 m 2 / g.

6. The preparation method according to any one of claims 1 to 5, characterized in that The seed crystals contain SiO2, Al2O3, Na2O and H2O, wherein the molar ratio of the SiO2 to the Al2O3 is 0.01-2.5:1, and the molar ratio of the Na2O, the H2O and the SiO2 is 0.01-4.0:1.0-40.0:

1.

7. The preparation method according to any one of claims 1 to 6, characterized in that The step S2 comprises: Step S21, performing the gelation treatment on the aluminum-rich liquid and the silicon-rich liquid to obtain a first gel; Step S22, subjecting the first gel and the seed crystal to the aging treatment and the hydrothermal crystallization treatment in sequence to obtain the 13X molecular sieve; wherein the first gel comprises SiO2, Al2O3, Na2O and H2O, wherein the molar ratio of the SiO2 to the Al2O3 is 0.5-6.0:1, and the molar ratio of the Na2O, the H2O and the SiO2 is 0.5-6.0:10-100:1; Preferably, the mass ratio of the seed crystal to the first gel is 5 to 20:100; and / or the temperature of the aging treatment is 20 to 100°C, and the time of the aging treatment is 0.1 to 24 hours; and / or the temperature of the hydrothermal crystallization treatment is 60 to 105°C, and the time of the hydrothermal crystallization treatment is 0.1 to 36 hours.

8. The preparation method according to any one of claims 1 to 7, characterized in that The preparation method further comprises: The preparation process of the seed crystal comprises: Stirring and mixing raw materials including an aluminum source, a second silicon source and water to obtain a second gel; Adjusting the pH value of the second gel to 8.5-12.5 and then performing two-stage hydrothermal crystallization treatment to obtain the seed crystal; Wherein, the stirring and mixing speed is 200-800 rpm; and / or, the stirring and mixing temperature is 20-100° C.; and / or, the stirring and mixing time is 0.1-24 h; Preferably, the pH value of the second gel is 11.8 to 12.2; Preferably, the second silicon source is selected from any one or more of silica sol, tetraethyl orthosilicate and silicon powder; Preferably, the aluminum source is selected from any one or more of sodium aluminate, pseudo-boehmite, aluminum sulfate, and aluminum nitrate; Preferably, the two-stage hydrothermal crystallization treatment includes a first stage hydrothermal crystallization treatment and a second stage hydrothermal crystallization treatment, wherein: The temperature of the first hydrothermal crystallization treatment is 20 to 60° C.; and / or the time of the first hydrothermal crystallization treatment is 4 to 24 hours; Preferably, the temperature of the second hydrothermal crystallization treatment is 80-120°C; and / or, the time of the second hydrothermal crystallization treatment is 6-48h; Furthermore, it is preferred that the temperature of the first hydrothermal crystallization treatment is 35 to 45° C., and / or the time of the first hydrothermal crystallization treatment is 11 to 13 hours; The temperature of the second hydrothermal crystallization treatment is 90-100° C.; and / or the time of the second hydrothermal crystallization treatment is 22-26 hours; The temperature of the second hydrothermal crystallization treatment is 50-60° C. higher than the temperature of the first hydrothermal crystallization treatment.

9. The preparation method according to any one of claims 1 to 8, characterized in that: The preparation method further comprises a process of pretreating the waste molecular sieve, wherein the pretreatment process comprises: sintering a mixture of the waste molecular sieve and the sodium salt to obtain a sintered product; The sintered product is sequentially subjected to the aluminum dissolving treatment and solid-liquid separation using an acidic solution to obtain the aluminum-rich liquid and residue; Using an alkaline solution to sequentially perform the silicon dissolving treatment and solid-liquid separation on the residue to obtain the silicon-rich liquid; Wherein, the mass ratio of the waste molecular sieve to the sodium salt is 1:0.5-5; and / or, the temperature of the sintering treatment is 550-800° C.; and / or, the time of the sintering treatment is 60-120 min; And / or, the acidic solution is a monoprotic acid solution, the mass fraction of the monoprotic acid solution is 10-35%, and preferably the monoprotic acid is hydrochloric acid and / or nitric acid; And / or, the alkaline solution comprises a monobasic alkali and water, and the mass ratio of the residue, the monobasic alkali and the water is 1.5-100:40-60:50-400; and / or, the monobasic alkali is NaOH and / or KOH; Preferably, the waste molecular sieve is selected from any one or more of waste HZSM-5 molecular sieve catalyst, waste MTO catalyst, fly ash, waste FCC catalyst, and waste VOC adsorbent; The sodium salt is Na2SO4 and / or NaCO3.

10. A core-shell structure cracking reaction catalyst, characterized in that: The core-shell structure cracking reaction catalyst is prepared by the preparation method described in any one of claims 1 to 9.

Citation Information

Patent Citations

  • A method for synthesizing submicron X-type molecular sieves and its application

    CN103523796B

  • Method for preparing molecular sieve from chlorosilane

    CN102009984A

  • 13X zeolite molecular sieve, preparation method therefor and application of 13X zeolite molecular sieve

    CN106542542A

  • Nickel-based Fischer-Tropsch catalyst and application method

    CN107537500A