Ammonia purification composite molecular sieve catalyst as well as preparation method and application thereof

By using a composite molecular sieve catalyst loaded with copper and platinum in the exhaust gas of ammonia internal combustion engine, the problems of high catalyst cost and secondary pollution in the prior art are solved, efficient ammonia purification and nitrogen selectivity are achieved, and the amount of precious metal platinum is reduced, which meets the satisfaction of Purification requirements under high temperature and high humidity conditions.

CN118925791AActive Publication Date: 2024-11-12RES CENT FOR ECO ENVIRONMENTAL SCI THE CHINESE ACAD OF SCI
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410989271.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-12
Estimated Expiration
2044-07-23

AI Technical Summary

Technical Problem

Existing ammonia internal combustion engine exhaust purification catalysts are expensive and have secondary pollution problems. Excessive amount of precious metal platinum leads to a degradation of catalyst performance and cannot effectively purify ammonia.

Method used

Using ammonia purification composite molecular sieve catalyst, the copper ions and platinum are uniformly loaded into the molecular sieve carrier and combined with multi-stage ball mill to form a dual-function site that couples ammonia oxidation and nitrogen oxide reduction, reducing the amount of platinum in precious metals while maintaining high activity. and selective.

Benefits of technology

Under the low platinum content of precious metals, high-efficiency ammonia purification and nitrogen selectivity are achieved, catalyst costs are reduced, secondary pollution is avoided, and purification needs of ammonia internal combustion engines under high temperature and high humidity conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118925791A_ABST
    Figure CN118925791A_ABST
Patent Text Reader

Abstract

The invention provides an ammonia purification composite molecular sieve catalyst and a preparation method and application thereof.The preparation method comprises the following steps that an ammonia type molecular sieve and a copper salt solution are mixed for the first time, then first solid-liquid separation, first drying and first roasting are conducted in sequence, and a loaded copper molecular sieve is obtained; mixing the ammonia-type molecular sieve and a platinum salt solution for the second time, and then sequentially carrying out second solid-liquid separation, second drying and second roasting to obtain a platinum-loaded molecular sieve; mixing the supported copper molecular sieve and the supported platinum molecular sieve, and then sequentially carrying out first ball milling and second ball milling to obtain the ammonia purification composite molecular sieve catalyst, the platinum-loaded molecular sieve and the copper-loaded molecular sieve are mixed through multi-stage ball milling, the active components platinum and copper are introduced respectively, it is ensured that the two active components do not interfere with each other and have a synergistic effect, and on the basis that platinum form distribution is basically unchanged and the catalyst has high ammoxidation low-temperature activity and nitrogen selectivity, the catalyst has high ammoxidation activity and nitrogen selectivity. And the dosage of precious metal platinum is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of ammonia internal combustion engine tail gas purification, and relates to an ammonia purification composite molecular sieve catalyst and a preparation method and application thereof. Background Art

[0002] At present, due to the shortage of fossil fuels, ammonia is an ideal energy storage material. Its molecules do not contain carbon elements, and the complete combustion products only include water and nitrogen. Compared with most gaseous fuels, it can be easily compressed into liquid, making it convenient for storage and transportation. As the second largest chemical product in the world, ammonia's related storage and transportation facilities are relatively complete. Therefore, ammonia has the potential to become an alternative fuel for internal combustion engines.

[0003] CN114575996A discloses an ammonia internal combustion engine and a control method thereof, provides an internal combustion engine device with zero carbon emissions, and takes into account the difficulty in storing and transporting hydrogen, and adopts ammonia as the main strategy for fuel. By introducing the exhaust gas generated by the internal combustion engine into the ammonia cracking device, partial cracking of ammonia is achieved, and the hydrogen generated by the cracking of ammonia increases the reactivity of the gas in the cylinder, which can achieve stable operation of the entire internal combustion engine. The hydrogen used is only used for starting the internal combustion engine, and the amount used is small, which can avoid the problem of difficulty in carrying hydrogen. The scheme selects a fuel supply strategy according to the working conditions, thereby achieving efficient operation of the ammonia internal combustion engine. The designed ammonia internal combustion engine starts with pure hydrogen, and after starting, pure ammonia is used as the only fuel to supply the internal combustion engine.

[0004] However, during the combustion process of an ammonia internal combustion engine, some of the fuel ammonia will not be fully burned, and will enter the atmosphere with the exhaust gas and cause pollution. Therefore, an ammonia purification catalyst is needed to catalytically purify the ammonia in the exhaust gas. Currently, ammonia purification catalysts mainly use precious metal catalysts, but in order to fully catalyze the oxidation of ammonia, existing catalysts need to use a large amount of precious metals. On the one hand, this leads to high catalyst costs; on the other hand, it will cause deep oxidation of ammonia to produce nitrogen oxides, causing secondary pollution. However, if the amount of precious metal platinum is directly reduced, the performance of the catalyst will be significantly reduced. The above problems make the existing catalysts expensive and cause secondary pollution problems, resulting in the inability to effectively purify the ammonia emitted from the exhaust of ammonia internal combustion engines.

[0005] In summary, providing a low-cost, high-activity, high-selectivity ammonia purification catalyst and a preparation method thereof is an urgent problem to be solved by those skilled in the art. Summary of the invention

[0006] The purpose of the present invention is to provide an ammonia purification composite molecular sieve catalyst and its preparation method and application. The ammonia purification composite molecular sieve catalyst couples the dual functional sites of ammonia oxidation and nitrogen oxide reduction, and still has high ammonia purification low-temperature activity and nitrogen selectivity in the case of extremely low precious metal platinum content. This solves the problem of excessive use of precious metals in ammonia purification catalysts in the prior art, resulting in high costs and secondary pollution, and the problem of directly reducing the amount of precious metal platinum causing catalyst performance degradation.

[0007] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:

[0008] In a first aspect, the present invention provides a method for preparing a composite molecular sieve catalyst for ammonia purification, the preparation method comprising the following steps:

[0009] (1) first mixing an ammonia molecular sieve and a copper salt solution, and then sequentially performing a first solid-liquid separation, a first drying and a first calcination to obtain a loaded copper molecular sieve;

[0010] (2) secondly mixing the ammonia molecular sieve and the platinum salt solution, and then sequentially performing a second solid-liquid separation, a second drying, and a second calcination to obtain a loaded platinum molecular sieve;

[0011] (3) mixing the copper molecular sieve loaded in step (1) and the platinum molecular sieve loaded in step (2), and then sequentially performing a first ball milling and a second ball milling to obtain the ammonia purification composite molecular sieve catalyst;

[0012] There is no particular order in which steps (1) and (2) are performed.

[0013] The preparation method provided by the present invention exchanges copper ions into the pores of a molecular sieve carrier, and after high-temperature roasting, copper is evenly distributed in the cationic sites in the molecular sieve mainly in the form of copper ions; platinum is evenly loaded on the molecular sieve carrier by an impregnation method, and after high-temperature roasting, the platinum mainly exists in a metallic state, and the metallic platinum has high activity and can effectively catalyze and oxidize ammonia in the exhaust gas of an internal combustion engine; finally, the loaded platinum molecular sieve and the loaded copper molecular sieve are mixed by multi-stage ball milling, so that the two groups of molecular sieves are mixed evenly and the two active components do not interfere with each other and have a synergistic effect. In addition, the multi-stage ball milling mixing can also reduce the amount of precious metal platinum in the composite molecular sieve catalyst.

[0014] It is worth mentioning that the use of precious metal platinum is reduced by mixing the loaded platinum molecular sieve and the loaded copper molecular sieve through multi-stage ball milling, which ensures that the morphological distribution of platinum remains basically unchanged while the atomic utilization rate is higher and the activity is stronger, so that the composite molecular sieve catalyst can couple the dual functional sites of ammonia oxidation and nitrogen oxide reduction, and even in the case of low precious metal platinum content, it still has high low-temperature activity for ammonia oxidation and nitrogen selectivity.

[0015] As a preferred technical solution of the present invention, the ammonia type molecular sieve includes any one of ZSM-5 molecular sieve, SSZ-13 molecular sieve, SSZ-39 molecular sieve, SAPO-34 molecular sieve or Y molecular sieve, or a combination of at least two thereof.

[0016] Preferably, the copper salt in the copper salt solution of step (1) includes any one of copper chloride, copper sulfate, copper nitrate or copper acetate, or a combination of at least two of them.

[0017] In the present invention, the solvent in the copper salt solution includes water, for example, deionized water or industrial recycled water that meets the requirements.

[0018] Preferably, the molar concentration of the copper element in the copper salt solution in step (1) is 0.01-0.1 mol / L, for example, it can be 0.02 mol / L, 0.03 mol / L, 0.04 mol / L, 0.05 mol / L, 0.06 mol / L, 0.07 mol / L, 0.08 mol / L, 0.09 mol / L or 0.1 mol / L, but is not limited to the listed values, and other values ​​not listed within this range are also applicable.

[0019] Preferably, the solid-to-liquid ratio of the ammoniacal molecular sieve and the copper salt solution in step (1) is 1:(20-70) g / mL, for example, it can be 1:20 g / mL, 1:25 g / mL, 1:30 g / mL, 1:35 g / mL, 1:40 g / mL, 1:45 g / mL, 1:50 g / mL, 1:55 g / mL, 1:60 g / mL, 1:65 g / mL or 1:70 g / mL, but is not limited to the listed values, and other values ​​not listed within the range are also applicable.

[0020] As a preferred technical solution of the present invention, in step (1), the first mixing is carried out under stirring.

[0021] Preferably, the temperature of the first mixing in step (1) is 40-60°C, for example, it can be 40°C, 41°C, 42°C, 43°C, 44°C, 45°C, 46°C, 47°C, 48°C, 49°C, 50°C, 51°C, 52°C, 53°C, 54°C, 55°C, 56°C, 57°C, 58°C, 59°C or 60°C, but is not limited to the listed values, and other values ​​not listed within the range are also applicable.

[0022] Preferably, the time for the first mixing in step (1) is 4-8h, for example, it can be 4h, 4.1h, 4.2h, 4.3h, 4.4h, 4.5h, 4.6h, 4.7h, 4.8h, 4.9h, 5h, 5.1h, 5.2h, 5.3h, 5.4h, 5.5h, 5.6h, 5.7h, 5.8h, 5.9h, 6h, 6.1h, 6.2h, 6.3h, 6.4h, 6.5h, 6.6h, 6.7h, 6.8h, 6.9h, 7h, 7.1h, 7.2h, 7.3h, 7.4h, 7.5h, 7.6h, 7.7h, 7.8h, 7.9h or 8h, but is not limited to the listed values, and other values ​​not listed in this range are also applicable.

[0023] Preferably, the first solid-liquid separation in step (1) comprises any one of suction filtration, filter pressing or centrifugation, or a combination of at least two of them.

[0024] Preferably, the temperature of the first drying in step (1) is 30-90°C, for example, it can be 30°C, 32°C, 34°C, 36°C, 38°C, 40°C, 42°C, 44°C, 46°C, 48°C, 50°C, 52°C, 53°C, 54°C, 56°C, 58°C, 60°C, 62°C, 64°C, 66°C, 68°C, 69°C, 70°C, 72°C, 74°C, 76°C, 78°C, 80°C, 82°C, 84°C, 86°C, 88°C or 90°C, etc., but is not limited to the listed values, and other values ​​not listed within the range are equally applicable.

[0025] As a preferred technical solution of the present invention, after the first drying in step (1), before the first calcination, it also includes: replacing the ammonia type molecular sieve in step (1) with the loaded copper molecular sieve precursor after the first drying, and then repeating step (1) until the first drying.

[0026] In the present invention, in order to ensure the loading of the active component copper, the copper element can be loaded multiple times.

[0027] Preferably, the number of repetitions is at least 1, for example, 1, 2 or 3 times, etc., but is not limited to the listed values, and other unlisted values ​​within the range are also applicable.

[0028] Preferably, when the step (1) is repeated, the molar concentration of the copper element in the copper salt solution is different each time.

[0029] Preferably, the temperature of the first calcination in step (1) is 450-550°C, for example, it can be 450°C, 460°C, 470°C, 480°C, 490°C, 500°C, 510°C, 520°C, 530°C, 540°C or 550°C, but is not limited to the listed values, and other unlisted values ​​within the range are also applicable.

[0030] Preferably, the time for the first calcination in step (1) is 4-8h, for example, it can be 4h, 4.1h, 4.2h, 4.3h, 4.4h, 4.5h, 4.6h, 4.7h, 4.8h, 4.9h, 5h, 5.1h, 5.2h, 5.3h, 5.4h, 5.5h, 5.6h, 5.7h, 5.8h, 5.9h, 6h, 6.1h, 6.2h, 6.3h, 6.4h, 6.5h, 6.6h, 6.7h, 6.8h, 6.9h, 7h, 7.1h, 7.2h, 7.3h, 7.4h, 7.5h, 7.6h, 7.7h, 7.8h, 7.9h or 8h, but is not limited to the listed values, and other values ​​not listed within the range are equally applicable.

[0031] As a preferred technical solution of the present invention, the platinum salt in the platinum salt solution in step (2) includes any one of tetraammineplatinum nitrate, chloroplatinic acid, platinum chloride or ammonium chloroplatinate, or a combination of at least two thereof.

[0032] In the present invention, the solvent in the platinum salt solution includes water, for example, deionized water or industrial recycled water that meets the requirements.

[0033] Preferably, the mass ratio of the ammonia molecular sieve and the platinum element in the platinum salt solution in step (2) is 1:(0.002-0.02), for example, it can be 1:0.002, 1:0.003, 1:0.004, 1:0.005, 1:0.006, 1:0.007, 1:0.008, 1:0.009, 1:0.01, 1:0.011, 1:0.012, 1:0.013, 1:0.014, 1:0.015, 1:0.016, 1:0.017, 1:0.018, 1:0.019 or 1:0.02, etc., but is not limited to the listed values, and other unlisted values ​​within the range are also applicable, preferably 1:(0.002-0.01).

[0034] As a preferred technical solution of the present invention, in step (2), the second mixing is carried out under stirring.

[0035] Preferably, the temperature of the second mixing in step (2) is 20-40°C, for example, it can be 20°C, 21°C, 22°C, 23°C, 24°C, 25°C, 26°C, 27°C, 28°C, 29°C, 30°C, 31°C, 32°C, 33°C, 34°C, 35°C, 36°C, 37°C, 38°C, 39°C or 40°C, but is not limited to the listed values, and other values ​​not listed within the range are also applicable.

[0036] Preferably, the time for the second mixing in step (2) is 0.5-3 h, for example, it can be 0.5 h, 0.6 h, 0.7 h, 0.8 h, 0.9 h, 1 h, 1.1 h, 1.2 h, 1.3 h, 1.4 h, 1.5 h, 1.6 h, 1.7 h, 1.8 h, 1.9 h, 2 h, 2.1 h, 2.2 h, 2.3 h, 2.4 h, 2.5 h, 2.6 h, 2.7 h, 2.8 h, 2.9 h or 3 h, but is not limited to the listed values, and other values ​​not listed within the range are equally applicable.

[0037] Preferably, the second solid-liquid separation in step (2) comprises any one of suction filtration, filter pressing or centrifugation, or a combination of at least two of them.

[0038] Preferably, the temperature of the second drying in step (2) is 30-90°C, for example, it can be 30°C, 32°C, 34°C, 36°C, 38°C, 40°C, 42°C, 44°C, 46°C, 48°C, 50°C, 52°C, 53°C, 54°C, 56°C, 58°C, 60°C, 62°C, 64°C, 66°C, 68°C, 69°C, 70°C, 72°C, 74°C, 76°C, 78°C, 80°C, 82°C, 84°C, 86°C, 88°C or 90°C, etc., but is not limited to the listed values, and other values ​​not listed within the range are equally applicable.

[0039] Preferably, the temperature of the second calcination in step (2) is 500-600°C, for example, it can be 500°C, 510°C, 520°C, 530°C, 540°C, 550°C, 560°C, 570°C, 580°C, 590°C or 600°C, but is not limited to the listed values, and other unlisted values ​​within this range are also applicable.

[0040] Preferably, the time for the second calcination in step (2) is 3-7h, for example, it can be 3h, 3.1h, 3.2h, 3.3h, 3.4h, 3.5h, 3.6h, 3.7h, 3.8h, 3.9h, 4h, 4.1h, 4.2h, 4.3h, 4.4h, 4.5h, 4.6h, 4.7h, 4.8h, 4.9h, 5h, 5.1h, 5.2h, 5.3h, 5.4h, 5.5h, 5.6h, 5.7h, 5.8h, 5.9h, 6h, 6.1h, 6.2h, 6.3h, 6.4h, 6.5h, 6.6h, 6.7h, 6.8h, 6.9h or 7h, but is not limited to the listed values, and other values ​​not listed within the range are equally applicable.

[0041] As a preferred technical solution of the present invention, the mass ratio of the loaded copper molecular sieve and the loaded platinum molecular sieve in step (3) is (1-10):1, for example, it can be 1:1, 2:1, 3:1, 4:1, 5:1, 6:1, 7:1, 8:1, 9:1 or 10:1, but is not limited to the listed values, and other unlisted values ​​within the range are also applicable.

[0042] Preferably, the rotation speed of the first ball mill in step (3) is 50-100 rpm, for example, it can be 50 rpm, 55 rpm, 60 rpm, 65 rpm, 70 rpm, 75 rpm, 80 rpm, 85 rpm, 90 rpm, 95 rpm or 100 rpm, but is not limited to the listed values, and other values ​​not listed within the range are also applicable.

[0043] Preferably, the ball-to-material ratio of the first ball milling in step (3) is (5-50):1, for example, it can be 5:1, 10:1, 15:1, 20:1, 25:1, 30:1, 35:1, 40:1, 45:1 or 50:1, but is not limited to the listed values, and other unlisted values ​​within this range are also applicable.

[0044] Preferably, the time for the first ball milling in step (3) is 5-30 min, for example, it can be 5 min, 6 min, 7 min, 8 min, 9 min, 10 min, 11 min, 12 min, 13 min, 14 min, 15 min, 16 min, 17 min, 18 min, 19 min, 20 min, 21 min, 22 min, 23 min, 24 min, 25 min, 26 min, 27 min, 28 min, 29 min or 30 min, but is not limited to the listed values, and other values ​​not listed in the range are also applicable.

[0045] Preferably, the rotation speed of the second ball mill in step (3) is 200-400rpm, for example, it can be 200rpm, 210rpm, 220rpm, 230rpm, 240rpm, 250rpm, 260rpm, 270rpm, 280rpm, 290rpm, 300rpm, 310rpm, 320rpm, 330rpm, 340rpm, 350rpm, 360rpm, 370rpm, 380rpm, 390rpm or 400rpm, but is not limited to the listed values, and other values ​​not listed within the range are also applicable.

[0046] Preferably, the ball-to-material ratio of the second ball milling in step (3) is (5-50):1, for example, it can be 5:1, 10:1, 15:1, 20:1, 25:1, 30:1, 35:1, 40:1, 45:1 or 50:1, but is not limited to the listed values, and other unlisted values ​​within the range are also applicable.

[0047] Preferably, the time for the second ball milling in step (3) is 5-20 min, for example, it can be 5 min, 6 min, 7 min, 8 min, 9 min, 10 min, 11 min, 12 min, 13 min, 14 min, 15 min, 16 min, 17 min, 18 min, 19 min or 20 min, but is not limited to the listed values, and other values ​​not listed within the range are also applicable.

[0048] It is worth noting that the present invention controls the process parameters of the first ball mill and the second ball mill to ensure that the two groups of molecular sieves are fully and evenly mixed, and can also significantly improve the utilization rate of the molecular sieve powder.

[0049] As a preferred technical solution of the present invention, the preparation method comprises the following steps:

[0050] (1) mixing the ammonia molecular sieve and the copper salt solution at a solid-liquid ratio of 1:(20-70) g / mL at a temperature of 40-60° C. for a first time for 4-8 hours, performing a first solid-liquid separation, performing a first drying at a temperature of 30-90° C., and then performing a first roasting at a temperature of 450-550° C. for 4-8 hours to obtain a loaded copper molecular sieve;

[0051] The copper salt in the copper salt solution includes any one of copper chloride, copper sulfate, copper nitrate or copper acetate or a combination of at least two thereof; the molar concentration of the copper element in the copper salt solution is 0.01-0.1 mol / L;

[0052] After the first drying and before the first calcination, the method further comprises: replacing the ammonia molecular sieve in step (1) with the loaded copper molecular sieve precursor after the first drying, and then repeating step (1) until the first drying; the number of repetitions is at least 1; when the step (1) is repeated, the molar concentration of copper element in the copper salt solution is different each time;

[0053] (2) mixing the ammonia molecular sieve and the platinum salt solution for a second time at a temperature of 20-40° C. for 0.5-3 h, performing a second solid-liquid separation, performing a second drying at a temperature of 30-90° C., and then performing a second calcination at a temperature of 500-600° C. for 3-7 h to obtain a loaded platinum molecular sieve;

[0054] The platinum salt in the platinum salt solution includes any one of tetraammine platinum nitrate, chloroplatinic acid, platinum chloride or ammonium chloroplatinate, or a combination of at least two thereof; the mass ratio of the ammonia molecular sieve to the platinum element in the platinum salt solution is 1:(0.002-0.02);

[0055] (3) mixing the copper molecular sieve loaded in step (1) and the platinum molecular sieve loaded in step (2) in a mass ratio of (1-10):1, and then performing a first ball milling for 5-30 min at a rotation speed of 50-100 rpm and a ball-to-material ratio of (5-50):1, and then performing a second ball milling for 5-20 min at a rotation speed of 200-400 rpm and a ball-to-material ratio of (5-50):1 to obtain the ammonia purification composite molecular sieve catalyst;

[0056] There is no particular order in which steps (1) and (2) are performed.

[0057] In a second aspect, the present invention provides an ammonia purification composite molecular sieve catalyst, wherein the ammonia purification composite molecular sieve catalyst is prepared by the preparation method described in the first aspect;

[0058] Taking the mass percentage as 100%, the ammonia purification composite molecular sieve catalyst comprises: 0.01-0.095% of platinum, 1-4% of copper, and the remainder is ammonia type molecular sieve.

[0059] In the present invention, the mass percentage of platinum in the ammonia purification composite molecular sieve catalyst is 0.01-0.095%, for example, it can be 0.01%, 0.02%, 0.03%, 0.04%, 0.05%, 0.06%, 0.07%, 0.08%, 0.09% or 0.095%, etc., and the mass percentage of copper in the ammonia purification composite molecular sieve catalyst is 1-4%, for example, it can be 1%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2%, 2.1%, 2.2%, 2.3%, 2.4%, 2.5%, 2.6%, 2.7%, 2.8%, 2.9%, 3%, 3.1%, 3.2%, 3.3%, 3.4%, 3.5%, 3.6%, 3.7%, 3.8%, 3.9% or 4%, etc., but not limited to the listed values, other values ​​not listed in the range are also applicable.

[0060] In the present invention, the ammonia purification composite molecular sieve catalyst has dual functional sites for coupling ammonia oxidation and nitrogen oxide reduction, and still has high ammonia purification low-temperature activity and nitrogen selectivity under the condition of low precious metal platinum content, which can ensure the efficient progress of the ammonia purification reaction in a high humidity and low oxygen environment, and can meet the purification requirements of ammonia internal combustion engines for unburned ammonia; in addition, the precious metal platinum in the ammonia purification composite molecular sieve catalyst is the reason for the high activity in the entire temperature range. The precious metal platinum has excellent oxidation ability and is distributed on the molecular sieve carrier in the form of small nanoparticles, which can effectively catalyze and oxidize ammonia in the exhaust gas of ammonia internal combustion engines, so that the ammonia can be completely oxidized. The active metal copper in the ammonia purification composite molecular sieve catalyst is present in the molecular sieve carrier in the form of highly dispersed ions, which can selectively reduce the by-product nitrogen oxides to nitrogen, thereby improving the nitrogen selectivity.

[0061] In a third aspect, the present invention provides an application of an ammonia purification composite molecular sieve catalyst, the application comprising using the ammonia purification composite molecular sieve catalyst of the second aspect to catalytically purify the tail gas generated during the operation of an ammonia internal combustion engine;

[0062] The temperature of the catalytic purification is 150-350°C;

[0063] Taking the volume percentage as 100%, the water content in the tail gas of the ammonia internal combustion engine is 5-15%, and the oxygen content in the tail gas of the ammonia internal combustion engine is 2-10%;

[0064] The volume concentration of ammonia in the tail gas generated during the operation of the ammonia internal combustion engine is 300-1500 ppm.

[0065] In the present invention, the total flow rate of the gas in the catalytic purification can be 300-1000 mL / min, and the space velocity is 100000-300000 h -1 .

[0066] Compared with the prior art, the present invention has the following beneficial effects:

[0067] (1) The preparation method provided by the present invention ensures that the two groups of molecular sieves are mixed evenly by multi-stage ball milling, and the two active components do not interfere with each other and have a synergistic effect. In addition, the multi-stage ball milling mixing ensures that the ammonia purification composite molecular sieve catalyst has dual functional sites for coupling ammonia oxidation and nitrogen oxide reduction, and can also reduce the amount of precious metal platinum. While ensuring that the morphological distribution of platinum remains basically unchanged, the atomic utilization rate is higher and the activity is stronger, so that the composite molecular sieve catalyst has higher low-temperature activity for ammonia oxidation and nitrogen selectivity;

[0068] (2) The ammonia purification composite molecular sieve catalyst provided by the present invention has high activity in the range of 200-350°C in the presence of 10% water vapor and 5% oxygen, and can meet the requirements of catalyst purification of ammonia under high temperature and high humidity conditions of ammonia internal combustion engines; at the same time, it also has high nitrogen selectivity in the range of 200-350°C, meeting the requirements for gas purification in ammonia internal combustion engines. BRIEF DESCRIPTION OF THE DRAWINGS

[0069] Figure 1 The graph shows the ammonia conversion rate and nitrogen selectivity of the ammonia purification composite molecular sieve catalyst obtained in Example 1 for the catalytic purification reaction of ammonia in the exhaust gas of an ammonia internal combustion engine. DETAILED DESCRIPTION

[0070] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0071] Example 1

[0072] This embodiment provides an ammonia purification composite molecular sieve catalyst and a preparation method thereof. The ammonia purification composite molecular sieve catalyst comprises, based on a mass percentage of 100%, 0.05% platinum, 2.5% copper, and the balance SSZ-39 molecular sieve;

[0073] The preparation method comprises the following steps:

[0074] (1) mixing SSZ-39 molecular sieve and copper nitrate aqueous solution at a solid-liquid ratio of 1:50 g / mL at a temperature of 60° C. for a first time and stirring for 6 hours, filtering, drying at a temperature of 60° C., and then calcining at a temperature of 500° C. for a first time for 6 hours to obtain a loaded copper molecular sieve;

[0075] After the first drying and before the first calcination, the method further comprises: replacing the SSZ-39 molecular sieve in step (1) with the loaded copper molecular sieve precursor after the first drying, and then repeating step (1) until the first drying; the number of repetitions is 1; when the step (1) is repeated, the molar concentration of the copper element in the copper nitrate aqueous solution is different each time, which is 0.1 mol / L and 0.05 mol / L respectively;

[0076] (2) mixing the SSZ-39 molecular sieve and the tetraammine platinum nitrate aqueous solution for a second time at a temperature of 25° C. and stirring for 0.5 h, centrifuging, and then drying for a second time at a temperature of 60° C., and then calcining for a second time at a temperature of 550° C. for 6 h to obtain a loaded platinum molecular sieve;

[0077] The mass ratio of the ammonia molecular sieve to the platinum element in the platinum salt solution is 1:0.004;

[0078] (3) mixing the copper molecular sieve loaded in step (1) and the platinum molecular sieve loaded in step (2) in a mass ratio of 4:1, and then performing a first ball milling for 10 min at a rotation speed of 80 rpm and a ball-to-material ratio of 8:1, and then performing a second ball milling for 10 min at a rotation speed of 300 rpm and a ball-to-material ratio of 10:1 to obtain the ammonia purification composite molecular sieve catalyst;

[0079] There is no particular order in which steps (1) and (2) are performed.

[0080] Example 2

[0081] This embodiment provides an ammonia purification composite molecular sieve catalyst and a preparation method thereof. The ammonia purification composite molecular sieve catalyst comprises, based on a mass percentage of 100%, 0.09% platinum, 2% copper, and the balance SSZ-39 molecular sieve;

[0082] The preparation method comprises the following steps:

[0083] (1) mixing SSZ-39 molecular sieve and copper nitrate aqueous solution at a solid-liquid ratio of 1:60 g / mL at a temperature of 60° C. for a first time and stirring for 6 hours, filtering, drying at a temperature of 60° C., and then calcining at a temperature of 550° C. for a first time for 6 hours to obtain a loaded copper molecular sieve;

[0084] After the first drying and before the first calcination, the method further comprises: replacing the SSZ-39 molecular sieve in step (1) with the loaded copper molecular sieve precursor after the first drying, and then repeating step (1) until the first drying; the number of repetitions is 1; when the step (1) is repeated, the molar concentration of the copper element in the copper nitrate aqueous solution is different each time, which is 0.08 mol / L and 0.09 mol / L respectively;

[0085] (2) mixing the SSZ-39 molecular sieve and the tetraammine platinum nitrate aqueous solution for a second time at a temperature of 25° C. and stirring for 0.5 h, centrifuging, and then drying for a second time at a temperature of 60° C., and then calcining for a second time at a temperature of 600° C. for 5 h to obtain a loaded platinum molecular sieve;

[0086] The mass ratio of the ammonia molecular sieve to the platinum element in the platinum salt solution is 1:0.008;

[0087] (3) mixing the copper molecular sieve loaded in step (1) and the platinum molecular sieve loaded in step (2) in a mass ratio of 3:1, and then performing a first ball milling for 6 min at a rotation speed of 100 rpm and a ball-to-material ratio of 10:1, and then performing a second ball milling for 9 min at a rotation speed of 280 rpm and a ball-to-material ratio of 15:1 to obtain the ammonia purification composite molecular sieve catalyst;

[0088] There is no particular order in which steps (1) and (2) are performed.

[0089] Example 3

[0090] This embodiment provides an ammonia purification composite molecular sieve catalyst and a preparation method thereof. Except that the temperature of the second calcination in step (2) is 520°C, the speed of the first ball milling in step (3) is 50 rpm and the time is 5 min, and the speed of the second ball milling is 200 rpm and the time is 10 min, other conditions are the same as those in Example 1.

[0091] Example 4

[0092] This embodiment provides an ammonia purification composite molecular sieve catalyst and a preparation method thereof. Except that the mass ratio of the loaded copper molecular sieve to the loaded platinum molecular sieve in step (3) is 15:1, other conditions are the same as those in Example 1.

[0093] Example 5

[0094] This embodiment provides an ammonia purification composite molecular sieve catalyst and a preparation method thereof. Except that the rotation speed of the second ball mill in step (3) is the same as that of the first ball mill, both are 80 rpm, other conditions are the same as those in Example 1.

[0095] Example 6

[0096] This embodiment provides an ammonia purification composite molecular sieve catalyst and a preparation method thereof. Except that the rotation speed of the second ball mill in step (3) is 500 rpm, other conditions are the same as those in Example 1.

[0097] Example 7

[0098] This embodiment provides an ammonia purification composite molecular sieve catalyst and a preparation method thereof. Except that the time for the first ball milling and the second ball milling in step (3) are both 1 min, other conditions are the same as those in Example 1.

[0099] Comparative Example 1

[0100] This comparative example provides an ammonia purification composite molecular sieve catalyst and a preparation method thereof. Except that only the first ball milling is performed in step (3), other conditions are the same as those in Example 1.

[0101] Application Examples 1-7 and Comparative Application Example 1

[0102] The ammonia purification composite molecular sieve catalyst prepared in Examples 1-7 and Comparative Example 1 was used to catalytically purify ammonia in a simulated ammonia internal combustion engine, and the catalytic purification temperature was 225°C; based on the volume percentage of 100%, the water content in the exhaust gas of the ammonia internal combustion engine was 10%, and the oxygen content in the exhaust gas of the ammonia internal combustion engine was 5%; the total gas flow rate in the exhaust gas of the ammonia internal combustion engine was 500 mL / min, and the air velocity was 200000 h -1 ; The volume concentration of ammonia in the exhaust gas formed during the operation of the ammonia internal combustion engine is 1000ppm.

[0103] The purified gas was measured by infrared spectrometer. The indicators of the purified gas are shown in Table 1.

[0104] Table 1

[0105] Ammonia conversion rate / % Nitrogen selectivity / % Application Example 1 99.9 80.7 Application Example 2 98.2 85.2 Application Example 3 93.3 88.5 Application Example 4 80.2 98.0 Application Example 5 95.7 78.8 Application Example 6 83.4 80.2 Application Example 7 100.0 73.9 Comparative application example 1 98.6 76.4

[0106] From Table 1, we can see that:

[0107] (1) The ammonia purification composite molecular sieve catalyst and the preparation method thereof provided in Examples 1-3 of the present invention, by multi-stage ball milling, the loaded platinum molecular sieve and the loaded copper molecular sieve are mixed, and the active components of platinum and copper are introduced respectively, so as to ensure that the two active components do not interfere with each other and have a synergistic effect, thereby reducing the amount of precious metal platinum, while ensuring that the composite molecular sieve catalyst still has high low-temperature activity and nitrogen selectivity for ammonia oxidation, and can also avoid the deep oxidation of ammonia to produce nitrogen oxides;

[0108] (2) By comparing Application Example 1 and Application Example 4, it can be seen that when the proportion of copper molecular sieve in the composite molecular sieve catalyst is too high, the low-temperature activity of ammonia oxidation is greatly reduced due to the low amount of precious metal platinum introduced;

[0109] (3) By comparing Application Example 1 with Application Examples 5-7, it can be seen that when the rotation speed of the second ball mill is too low or the ball milling time is too short, it is not conducive to uniform mixing of the loaded copper molecular sieve and the loaded platinum molecular sieve, and the spatial distribution of the two active components is poor, and they cannot effectively cooperate, resulting in a significant decrease in nitrogen selectivity; when the rotation speed of the second ball mill is too high, the structure of the obtained composite molecular sieve catalyst is destroyed, resulting in a significant decrease in low-temperature activity of ammonia oxidation and a slight decrease in nitrogen selectivity;

[0110] (4) From the comparison between Application Example 1 and Comparative Application Example 1, it can be seen that when only the first ball milling is performed, it is not conducive to uniform mixing of the loaded copper molecular sieve and the loaded platinum molecular sieve. The spatial distribution of the two active components is poor and they cannot effectively cooperate, resulting in a significant decrease in nitrogen selectivity.

[0111] The ammonia purification composite molecular sieve catalyst prepared in Example 1 was used to catalytically purify ammonia in a simulated ammonia internal combustion engine, and a gradient temperature test was conducted on the catalytic purification temperature, and the temperatures were 150°C, 175°C, 200°C, 225°C, 250°C, 275°C, 300°C, 325°C, and 350°C respectively;

[0112] Taking the volume percentage as 100%, the water content in the tail gas of the ammonia internal combustion engine is 10%, and the oxygen content in the tail gas of the ammonia internal combustion engine is 5%; the total gas flow rate in the tail gas of the ammonia internal combustion engine is 500mL / min, and the air velocity is 200000h -1 ; The volume concentration of ammonia in the exhaust gas of the ammonia internal combustion engine is 1000ppm.

[0113] The results of the purified gas are shown in Figure 1 and Table 2.

[0114] Table 2

[0115]

[0116]

[0117] Depend on Figure 1 As can be seen from Table 2, the present invention provides an ammonia purification composite molecular sieve catalyst and a preparation method thereof. The active components platinum and copper are introduced respectively by mixing a loaded platinum molecular sieve and a loaded copper molecular sieve through multi-stage ball milling, thereby ensuring that the two active components do not interfere with each other and have a synergistic effect. The amount of precious metal platinum is reduced while ensuring that the distribution of platinum morphology remains basically unchanged and the catalyst has high ammonia oxidation low-temperature activity and nitrogen selectivity. The deep oxidation of ammonia to produce nitrogen oxides is avoided, thereby solving the problem of high cost caused by excessive platinum use in current ammonia purification catalysts and the problem of catalyst performance degradation caused by directly reducing the amount of precious metal platinum.

[0118] The applicant declares that the present invention illustrates the detailed structural features of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned detailed structural features, that is, it does not mean that the present invention must rely on the above-mentioned detailed structural features to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the components selected by the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. A method for preparing a composite molecular sieve catalyst for ammonia purification, characterized in that: The preparation method comprises the following steps: (1) first mixing an ammonia molecular sieve and a copper salt solution, and then sequentially performing a first solid-liquid separation, a first drying and a first calcination to obtain a loaded copper molecular sieve; (2) secondly mixing the ammonia molecular sieve and the platinum salt solution, and then sequentially performing a second solid-liquid separation, a second drying, and a second calcination to obtain a loaded platinum molecular sieve; (3) mixing the copper molecular sieve loaded in step (1) and the platinum molecular sieve loaded in step (2), and then sequentially performing a first ball milling and a second ball milling to obtain the ammonia purification composite molecular sieve catalyst; There is no particular order in which steps (1) and (2) are performed.

2. The preparation method according to claim 1, characterized in that: The ammonia molecular sieve includes any one of ZSM-5 molecular sieve, SSZ-13 molecular sieve, SSZ-39 molecular sieve, SAPO-34 molecular sieve or Y molecular sieve, or a combination of at least two thereof; Preferably, the copper salt in the copper salt solution of step (1) includes any one of copper chloride, copper sulfate, copper nitrate or copper acetate, or a combination of at least two thereof; Preferably, the molar concentration of copper in the copper salt solution in step (1) is 0.01-0.1 mol / L; Preferably, the solid-to-liquid ratio of the ammonia molecular sieve and the copper salt solution in step (1) is 1:(20-70) g / mL.

3. The preparation method according to claim 1 or 2, characterized in that: Step (1) the first mixing is carried out under stirring; Preferably, the temperature of the first mixing in step (1) is 40-60°C; Preferably, the first mixing time in step (1) is 4-8 hours; Preferably, the first solid-liquid separation in step (1) comprises any one of suction filtration, filter pressing or centrifugation, or a combination of at least two thereof; Preferably, the temperature of the first drying in step (1) is 30-90°C.

4. The preparation method according to any one of claims 1 to 3, characterized in that After the first drying in step (1), before the first calcination, the method further comprises: replacing the ammonia molecular sieve in step (1) with the loaded copper molecular sieve precursor after the first drying, and then repeating step (1) until the first drying; Preferably, the number of repetitions is at least 1; Preferably, when the step (1) is repeated, the molar concentration of the copper element in the copper salt solution is different each time; Preferably, the temperature of the first calcination in step (1) is 450-550°C; Preferably, the first calcination time in step (1) is 4-8 hours.

5. The preparation method according to any one of claims 1 to 4, characterized in that: The platinum salt in the platinum salt solution of step (2) includes any one of tetraammine platinum nitrate, chloroplatinic acid, platinum chloride or ammonium chloroplatinate, or a combination of at least two thereof; Preferably, the mass ratio of the ammonia molecular sieve and the platinum element in the platinum salt solution in step (2) is 1:(0.002-0.02), preferably 1:(0.002-0.01).

6. The preparation method according to any one of claims 1 to 5, characterized in that: Step (2) the second mixing is carried out under stirring; Preferably, the temperature of the second mixing in step (2) is 20-40°C; Preferably, the second mixing time in step (2) is 0.5-3h; Preferably, the second solid-liquid separation in step (2) comprises any one of suction filtration, filter pressing or centrifugation, or a combination of at least two thereof; Preferably, the temperature of the second drying in step (2) is 30-90°C; Preferably, the temperature of the second calcination in step (2) is 500-600°C; Preferably, the second calcination time in step (2) is 3-7 hours.

7. The preparation method according to any one of claims 1 to 6, characterized in that: The mass ratio of the loaded copper molecular sieve to the loaded platinum molecular sieve in step (3) is (1-10):1; Preferably, the rotation speed of the first ball mill in step (3) is 50-100 rpm; Preferably, the ratio of balls to materials in the first ball milling in step (3) is (5-50):1; Preferably, the first ball milling time in step (3) is 5-30 min; Preferably, the rotation speed of the second ball mill in step (3) is 200-400 rpm; Preferably, the ratio of balls to materials in the second ball milling in step (3) is (5-50):1; Preferably, the time of the second ball milling in step (3) is 5-20 min.

8. The preparation method according to any one of claims 1 to 7, characterized in that: The preparation method comprises the following steps: (1) mixing the ammonia molecular sieve and the copper salt solution at a solid-liquid ratio of 1:(20-70) g / mL at a temperature of 40-60° C. for a first time for 4-8 hours, performing a first solid-liquid separation, performing a first drying at a temperature of 30-90° C., and then performing a first roasting at a temperature of 450-550° C. for 4-8 hours to obtain a loaded copper molecular sieve; The copper salt in the copper salt solution includes any one of copper chloride, copper sulfate, copper nitrate or copper acetate or a combination of at least two thereof; the molar concentration of the copper element in the copper salt solution is 0.01-0.1 mol / L; After the first drying and before the first calcination, the method further comprises: replacing the ammonia molecular sieve in step (1) with the loaded copper molecular sieve precursor after the first drying, and then repeating step (1) until the first drying; the number of repetitions is at least 1; when the step (1) is repeated, the molar concentration of copper element in the copper salt solution is different each time; (2) mixing the ammonia molecular sieve and the platinum salt solution for a second time at a temperature of 20-40° C. for 0.5-3 h, performing a second solid-liquid separation, performing a second drying at a temperature of 30-90° C., and then performing a second calcination at a temperature of 500-600° C. for 3-7 h to obtain a loaded platinum molecular sieve; The platinum salt in the platinum salt solution includes any one of tetraammine platinum nitrate, chloroplatinic acid, platinum chloride or ammonium chloroplatinate, or a combination of at least two thereof; the mass ratio of the ammonia molecular sieve to the platinum element in the platinum salt solution is 1:(0.002-0.02); (3) mixing the copper molecular sieve loaded in step (1) and the platinum molecular sieve loaded in step (2) in a mass ratio of (1-10):1, and then performing a first ball milling for 5-30 min at a rotation speed of 50-100 rpm and a ball-to-material ratio of (5-50):1, and then performing a second ball milling for 5-20 min at a rotation speed of 200-400 rpm and a ball-to-material ratio of (5-50):1 to obtain the ammonia purification composite molecular sieve catalyst; There is no particular order in which steps (1) and (2) are performed.

9. A composite molecular sieve catalyst for ammonia purification, characterized in that: The ammonia purification composite molecular sieve catalyst is prepared by the preparation method described in any one of claims 1 to 8; Taking the mass percentage as 100%, the ammonia purification composite molecular sieve catalyst comprises: 0.01-0.095% of platinum, 1-4% of copper, and the remainder is ammonia type molecular sieve.

10. An application of a composite molecular sieve catalyst for ammonia purification, characterized in that: The application includes using the ammonia purification composite molecular sieve catalyst according to claim 9 to catalytically purify the tail gas generated during the operation of an ammonia internal combustion engine; The temperature of the catalytic purification is 150-350°C; Taking the volume percentage as 100%, the water content in the tail gas of the ammonia internal combustion engine is 5-15%, and the oxygen content in the tail gas of the ammonia internal combustion engine is 2-10%; The volume concentration of ammonia in the tail gas generated during the operation of the ammonia internal combustion engine is 300-1500 ppm.

Citation Information

Patent Citations

  • Ammonia gas purification catalyst, and preparation method and use thereof

    CN109289906A

  • Ammoxidation catalyst and preparation method and application thereof

    CN112076803A

  • Preparation method of molecular sieve catalyst, catalyst and application thereof

    CN113617386A

  • Diesel vehicle tail gas ammonia purification molecular sieve catalyst and preparation method and application thereof

    CN115445654A

  • Molecular sieve catalyst for ammonia purification of ammonia internal combustion engine as well as preparation method and application of molecular sieve catalyst

    CN115532304A