Mn-UiO-66 material as well as preparation method and application thereof
By combining soluble manganese salts on the UiO-66 support, the problem of deactivation of nano manganese oxide catalysts is solved, and the efficient removal of phenolic pollutants under acidic conditions is achieved, and the Mn-based catalysts is broadened. Application scope.
Patent Information
- Application Number
- CN202410808004.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-21
- Publication Date
- 2024-11-12
AI Technical Summary
The nano-manganese oxide catalyst is prone to aggregate into blocks due to its small fineness, which limits its practical application in water treatment.
UiO-66 is used as a support, and the soluble manganese salt is combined with UiO-66 by hydrothermal method to prepare Mn-UiO-66 material. By adjusting the content of manganese element, the specific surface area of Mn3O4 is increased and more exposed. Mn active site.
Mn50-UiO catalyst exhibits high catalytic activity under acidic conditions, can effectively remove phenolic pollutants, and can significantly degrade bisphenol A in the presence or absence of PMS, broadening the Mn-based catalysts in the field of water treatment. application.
Smart Images

Figure CN118925808A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of water treatment, and in particular relates to a Mn-UiO-66 material and a preparation method and application thereof. Background Art
[0002] Advanced oxidation processes (AOPs) based on peroxymonosulfate (PMS) oxidation have attracted more and more attention from researchers in the degradation of organic pollutants in water. Due to the asymmetric molecular structure of PMS, which has peroxy bonds (OO), PMS can be activated by free radicals and non-free radical pathways to produce different active oxidative species, such as sulfate radicals (SO4· - ), hydroxyl radical (HO·), singlet oxygen ( 1 O2), high-valent metal species and metal-PMS complexes. Generally speaking, due to SO4· - (2.5-3.1ev) and HO·(1.8-2.7ev) have higher redox potentials and show higher reactivity, while non-radical active species are relatively mild, so they show higher selectivity for electron-rich organic compounds (phenols, organic dyes). Compared with H2O2, PMS has more advantages in storage and transportation due to its high stability, easy transportation and non-decomposition. These advantages have attracted more scientists to turn their attention to PMS-based AOPs to treat various organic pollutants in wastewater.
[0003] In recent years, many catalysts for activating PMS have been developed. For example, transition metal-based catalysts, noble metal-based catalysts and carbon-based catalysts. Since transition metal-based catalysts have the advantages of high activity, low price and good stability, they have attracted the research attention of many scientific researchers. Among them, manganese-based catalysts have been more widely studied due to their low toxicity, high natural abundance and environmental friendliness. Although the synthesized nano manganese oxide has high catalytic activity, it is easy to aggregate into blocks due to their small particle fineness, resulting in deactivation, which in turn limits their practical application. Summary of the invention
[0004] In order to solve the above technical problems, the present invention proposes a Mn-UiO-66 material and a preparation method and application thereof.
[0005] To achieve the above object, the present invention provides the following technical solutions:
[0006] A method for preparing a Mn-UiO-66 material comprises taking UiO-66 as a carrier and a soluble manganese salt as a manganese precursor, and adopting a hydrothermal method to prepare the Mn-UiO-66 material.
[0007] Furthermore, the preparation method of the Mn-UiO-66 material comprises the following steps:
[0008] UiO-66 is dispersed in water, ultrasonically obtained to obtain a suspension, a soluble manganese salt is added, ultrasonically and magnetically stirred to obtain a mixture, the mixture is subjected to a hydrothermal reaction, cooled to room temperature, centrifuged to obtain a precipitate, washed, and dried to obtain the Mn-UiO-66 material, denoted as MnX-UiO, where X is the mass percentage of manganese element in the soluble manganese salt to UiO-66, and the value range of X is 20-95.
[0009] Further, the mass ratio of UiO-66 to manganese in soluble manganese salt is 1:(0.20-0.95). For example, when the mass ratio of UiO-66 to manganese in soluble manganese salt is 1:0.20, X is 20, and the prepared Mn-UiO-66 material is recorded as Mn20-UiO. The mass ratio of UiO-66 to manganese in soluble manganese salt is preferably 1:0.50.
[0010] Furthermore, the manganese salt is a soluble divalent manganese salt, including one of manganese acetate, manganese nitrate, manganese chloride, and manganese oxalate, preferably manganese acetate.
[0011] Further, the temperature of the hydrothermal reaction is 95-120°C and the time is 15-24h;
[0012] More preferably, the temperature of the hydrothermal reaction is 100° C. and the time is 16 h.
[0013] Furthermore, the washing is: washing with deionized water and ethanol three times respectively.
[0014] Furthermore, the preparation method of UiO-66 comprises the following steps:
[0015] ZrCl4 and terephthalic acid (H2BDC) were added to dimethylformamide (DMF), stirred until completely dissolved, and then hydrochloric acid was added and stirred continuously until all solids were completely dissolved to obtain a mixture. The obtained mixture was hydrothermally reacted at 120°C for 24 hours, cooled to room temperature, and solid MOFs were collected by centrifugation, thoroughly washed three times with DMF, and washed three times with anhydrous ethanol to obtain UiO-66.
[0016] Furthermore, in the preparation method of UiO-66, the mass ratio of ZrCl4 to terephthalic acid is 1.64:1.16.
[0017] Furthermore, the preparation method of the Mn-UiO-66 material is:
[0018] Preparation of UiO-66:
[0019] First, add 1.64g ZrCl4 and 1.16g H2BDC to 80mL DMF and stir until completely dissolved. Then, add 3.5mL hydrochloric acid and stir continuously until all solids are completely dissolved to obtain a mixture. The obtained mixture is transferred to a 100mL stainless steel autoclave with a polytetrafluoroethylene liner and reacted at 120℃ for 24h. After cooling to room temperature, the solid MOFs are collected by centrifugation, thoroughly washed three times with DMF and three times with anhydrous ethanol. Finally, vacuum dry overnight to obtain UiO-66.
[0020] Preparation of MnX-UiO
[0021] 0.10g of the UiO-66 prepared above was dispersed in 10mL of deionized water and ultrasonicated for 0.5h to obtain a suspension, and then manganese salt (the amount of manganese salt added was calculated as manganese element, specifically, the mass of manganese element was 20-95% of the mass of UiO-66) was added to the suspension, and after ultrasonication for 10min, magnetic stirring was performed for 1h to ensure that the manganese salt was completely dissolved. Next, the mixture was transferred to a 100mL stainless steel autoclave with a polytetrafluoroethylene liner, and after isothermal reaction in a 100°C oven for 20h, it was naturally cooled to room temperature, and the obtained precipitate was separated by centrifugation, washed three times with deionized water and ethanol, respectively, and finally dried overnight in an oven at 80°C to obtain MnX-UiO, where X is the mass percentage of manganese element to UiO-66, and the value range of X is 20-95, preferably 30-95, and more preferably X is 50. For example, when the added amount of UiO-66 is 0.10 g and the added amount of manganese element is 0.050 g, X is 50, which is recorded as Mn50-UiO.
[0022] The present invention uses UiO-66 as a carrier and a soluble manganese salt as a precursor to synthesize a series of Mn-UiO-66 catalysts by a hydrothermal method. Characterization results show that the present invention successfully synthesizes a composite catalyst of UiO-66 loaded with Mn3O4. Mn3O4 is tightly combined with UiO-66 by forming a CO-Mn bond, which greatly increases the specific surface area of Mn3O4, exposes more Mn active sites, and can reduce the cost of practical application. Experimental research results show that Mn50-UiO has excellent catalytic activity. There are three oxidation mechanisms in the removal process of bisphenol A (BPA): (1) direct oxidation mechanism; (2) singlet oxygen oxidation mechanism; (3) electron transfer mechanism. The direct oxidation mechanism is extremely dependent on the pH of the reaction solution. Under acidic conditions (pH<3), even without adding PMS (peroxymonosulfate), BPA can be effectively removed within 30 minutes. Under the condition of pH>4.1, the two oxidation mechanisms mainly involved are singlet oxygen oxidation and electron transfer. Since Mn50-UiO has a small impedance and a large specific surface area, it promotes the transfer of electrons on the catalyst surface and the adsorption and degradation of pollutants on the catalyst. In the singlet oxygen oxidation mechanism, UiO-66 as a carrier plays the role of electron donor, which greatly accelerates the oxidation process of BPA. The present invention conducts in-depth research on the mechanism of Mn50-UiO catalytic oxidation to remove phenolic pollutants, and broadens the application of Mn-based catalysts in the field of water treatment.
[0023] The present invention also provides a Mn-UiO-66 material prepared by the above method.
[0024] The present invention also provides application of the Mn-UiO-66 material in treating organic matter in wastewater.
[0025] Further preferably, the Mn-UiO-66 material of the present invention can treat phenolic organic matter, antibiotics or rhodamine B in water.
[0026] More preferably, when the organic matter is phenolic organic matter, the pH of the wastewater is less than 3 or the wastewater contains PMS.
[0027] More preferably, the phenolic organic compound includes but is not limited to BPA, m-cresol, 4-chlorophenol or 2,4,6-trichlorophenol. The antibiotic includes but is not limited to ciprofloxacin or tetracycline hydrochloride.
[0028] Compared with the prior art, the present invention has the following advantages and technical effects:
[0029] The present invention utilizes the characteristics of strong interaction between the abundant μ3-OH or μ3-O on the surface of UiO-66 and metal ions, modifies the surface of UiO-66 with Mn oxide, forms a composite Mn-UiO-66 material, and obtains a Mn50-UiO catalyst with an optimal composition by systematically adjusting the manganese content of the Mn precursor. BPA is used as a model pollutant, and the synthesized Mn50-UiO metal composite material is applied to the degradation of organic pollutants in the water phase. Studies have found that the composite material exhibits a high removal effect on phenolic pollutants under PMS or acidic conditions (pH<3), and its high catalytic activity originates from the Mn active sites enriched on the surface of UiO-66. In short, the Mn-based catalyst of the present invention is reasonably designed and can effectively remove a variety of pollutants in water. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] The drawings constituting a part of the present application are used to provide a further understanding of the present application. The illustrative embodiments and descriptions of the present application are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:
[0031] Figure 1 This is a scanning electron microscope (SEM) image of the Mn50-UiO catalyst prepared in Example 1 at 500 nm;
[0032] Figure 2 XRD pattern of the Mn50-UiO catalyst prepared in Example 1-6;
[0033] Figure 3 N2 adsorption-desorption isotherms of the Mn50-UiO catalyst prepared in Example 1, the original UiO-66 and the Mn3O4 prepared in Comparative Example 1;
[0034] Figure 4 Fourier transform infrared images of the Mn50-UiO catalyst and UiO-66 prepared in Example 1;
[0035] Figure 5 This is the full XPS spectrum of the Mn50-UiO catalyst prepared in Example 1;
[0036] Figure 6 The Mn 2p fine spectrum in the Mn50-UiO catalyst prepared in Example 1;
[0037] Figure 7 is the removal rate of different organic matter by Mn50-UIO catalyst (the concentration of catalyst in the system is 0.2g / L);
[0038] Figure 8(a) shows the removal effect of BPA by Mn50-UiO / PMS system under different pH conditions, and (b) shows the removal efficiency of BPA and 4-CP by Mn50-UiO under pH=1 condition.
[0039] Fig. 9 This is a diagram showing the removal rate of BPA in sewage after different times of use of Mn50-UiO catalyst. DETAILED DESCRIPTION
[0040] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0041] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.
[0042] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.
[0043] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present invention description and examples are exemplary only.
[0044] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.
[0045] Unless otherwise specified, the room temperature in the present invention is 25±2°C.
[0046] All raw materials used in the examples of the present invention are commercially available.
[0047] Metal-organic frameworks (MOFs) have attracted much attention due to their high specific surface area, adjustable structure and potential application value. UiO-66(Zr) is a kind of Zr-based MOFs. It has the advantages of controllable pore size structure, chemical stability, functionalization and versatility. It is suitable for various application fields and shows broad application prospects in adsorption, catalysis, separation and other aspects. Compared with materials such as ZrO2, Fe3O4, TiO2, SBA-15 and graphene, the preparation process of UiO-66 is simple and the production cost is low. UiO-66 is connected by Zr6 octahedral clusters and terephthalic acid through coordination bonds. In its hydroxylated state, the surface of each octahedral metal cluster is bridged by μ3-OH or μ3-O groups, which makes the surface of UiO-66 with regular octahedral morphology rich in terminal μ3-OH or μ3-O groups, which can not only provide active sites but also increase the hydrophilicity of the UiO-66 surface, thereby forming interactions with other substances. The present invention utilizes the μ3-OH or μ3-O groups on the surface of UiO-66 to interact strongly with metal ions, thereby achieving the purpose of anchoring other materials. Based on this, the present invention utilizes the characteristics of strong interaction between the abundant μ3-OH or μ3-O on the surface of UiO-66 and metal ions, modifies the surface of UiO-66 with Mn oxide, forms a composite Mn-UiO-66 material, and systematically adjusts the manganese content in the Mn precursor to obtain a Mn50-UiO catalyst with an optimal composition. BPA, m-methylphenol, 4-chlorophenol or 2,4,6-trichlorophenol are used as model pollutants, respectively, and the synthesized Mn50-UiO metal composite material is applied to the degradation of organic pollutants in the aqueous phase. Studies have found that the composite material exhibits a high removal effect on phenolic pollutants under PMS or acidic conditions (pH<3), and its high catalytic activity originates from the Mn active sites enriched on the surface of UiO-66. The effects of several reaction parameters on the catalytic activation of PMS by Mn50-UiO catalyst for the degradation of BPA were investigated, and the different oxidation mechanisms of BPA removal under different conditions were explored, and the activation and regeneration of Mn50-UiO metal composite materials were studied. The results show that the Mn-based catalyst of the present invention is reasonably designed and can effectively remove phenolic water pollutants.
[0048] The technical solution of the present invention is further illustrated by the following embodiments.
[0049] Example 1
[0050] (1) Preparation of UiO-66:
[0051] First, add 1.64g ZrCl4 and 1.16g H2BDC to 80mL DMF and stir until completely dissolved. Then, add 3.5mL hydrochloric acid and stir continuously until all solids are completely dissolved to obtain a mixture. The obtained mixture is transferred to a 100mL stainless steel autoclave with a polytetrafluoroethylene liner and reacted at 110℃ for 24h. After cooling to room temperature, the solid MOFs are collected by centrifugation, and the chalk is washed three times with N,N-dimethylformamide and anhydrous ethanol. Finally, vacuum dry for 8h to obtain UiO-66.
[0052] (2) Preparation of Mn50-UiO
[0053] 0.10 g of the UiO-66 prepared above was dispersed in 10 mL of deionized water and ultrasonicated for 30 minutes to obtain a suspension, and then 0.156 g of manganese acetate was added to the suspension, ultrasonicated for 10 minutes, and magnetically stirred for 1 hour to ensure that the manganese acetate was completely dissolved. Next, the mixture was transferred to a 100 mL stainless steel autoclave with a polytetrafluoroethylene liner, and after a constant temperature reaction at 100 ° C for 20 hours, it was cooled to room temperature, and the obtained precipitate was separated by centrifugation, washed three times with deionized water and ethanol, and finally dried in vacuum for 8 hours, which was recorded as Mn50-UiO (50 represents that the mass of Mn is 50% of the mass of UiO-66, the same below).
[0054] Example 2
[0055] The same as Example 1, except that when preparing MnX-UiO, the amount of manganese acetate added was 0.063 g, and the prepared sample was marked as Mn20-UiO.
[0056] Example 3
[0057] The same as Example 1, except that when preparing MnX-UiO, the amount of manganese acetate added was 0.125 g, and the prepared sample was marked as Mn40-UiO.
[0058] Example 4
[0059] The same as Example 1, except that when preparing MnX-UiO, the amount of manganese acetate added was 0.188 g, and the prepared sample was marked as Mn60-UiO.
[0060] Example 5
[0061] The same as Example 1, except that when preparing MnX-UiO, the amount of manganese acetate added was 0.250 g, and the prepared sample was marked as Mn80-UiO.
[0062] Example 6
[0063] The same as Example 1, except that when preparing MnX-UiO, the amount of manganese acetate added was 0.296 g, and the prepared sample was marked as Mn95-UiO.
[0064] Example 7
[0065] The same as Example 1, except that when preparing MnX-UiO, the manganese source is manganese nitrate, the addition amount is 0.161 g, and the prepared sample is marked as Mn50-UiO-N.
[0066] Example 8
[0067] The same as Example 1, except that when preparing MnX-UiO, the manganese source is manganese chloride, the addition amount is 0.113 g, and the prepared sample is marked as Mn50-UiO-Cl.
[0068] Example 9
[0069] The same as Example 1, except that when preparing MnX-UiO, the manganese source is manganese oxalate, the addition amount is 0.129 g, and the prepared sample is marked as Mn50-UiO-OA.
[0070] Example 10
[0071] Same as Example 1, except that the reaction was carried out at a constant temperature of 95° C. for 24 hours.
[0072] Embodiment 11
[0073] Same as Example 1, except that the reaction was carried out at a constant temperature of 110° C. for 18 h.
[0074] Example 12
[0075] Same as Example 1, except that the reaction was carried out at a constant temperature of 120° C. for 15 h.
[0076] Comparative Example 1 Preparation of Mn3O4
[0077] 60 mL of 0.4 mol / L manganese acetate aqueous solution was placed in a 100 mL stainless steel reactor with a polytetrafluoroethylene liner, and hydrothermally reacted at 100 ° C for 16 h. After cooling to room temperature, it was washed three times with deionized water and ethanol respectively, and then dried in an oven at 80 ° C overnight. After grinding, powdered Mn3O4 particles were obtained.
[0078] The scanning electron microscope (SEM) image of the Mn50-UiO catalyst prepared in Example 1 at 500 nm is as follows: Figure 1 As shown, it can be seen that Mn50-UiO all show an irregular octahedral morphology with staggered growth and a size range of 20-100 nm.
[0079] The XRD pattern of the Mn50-UiO catalyst prepared in Example 1 is as follows: Figure 2 As shown in the figure, the characteristic peaks of the synthesized UiO-66 match the fitted UiO-66 very well, indicating that the original UiO-66 is composed of a single UiO-66 phase. As the amount of manganese acetate added during the synthesis process gradually increases, the diffraction peak corresponding to the 111 crystal plane of UiO-66 disappears, and the peak corresponding to the 211 crystal plane of Mn3O4 becomes more and more obvious, indicating that the manganese compound combined with UiO-66 mainly exists in the form of Mn3O4, and as the Mn3O4 loading increases, the peak type of the composite material becomes less and less obvious, indicating that the amorphous Mn3O4 is successfully dispersed on the surface of UiO-66 and mainly combined with the 111 crystal plane of UiO-66.
[0080] In order to further study the structural parameters of the samples before and after Mn3O4 loading, the specific surface area of the samples before and after loading was tested using N2 adsorption-isotherm curves. The N2 adsorption-isotherm curves of the Mn50-UiO catalyst prepared in Example 1, the original UiO-66 and the Mn3O4 prepared in Comparative Example 1 are shown in Figure 3 The specific surface areas of original UiO-66 and Mn3O4 are 1070.8 and 35.5 m 2 / g, and the specific surface area of the Mn50-UiO sample synthesized by hydrothermal method is 767.3m 2 / g, which is between the two. This shows that the large specific surface area of UiO-66 is conducive to the uniform distribution of Mn3O4. Compared with the original Mn3O4, the Mn50-UiO sample has a larger specific surface area, which is conducive to the adsorption and transfer of PMS and organic pollutants on the catalyst surface, thereby enhancing the degradation activity of organic pollutants.
[0081] Figure 4 This is the Fourier transform infrared image of the Mn50-UiO catalyst prepared in Example 1, where 656 cm -1 and 476cm -1 The vibration peaks appearing at correspond to the stretching of μ3-O and μ3-OH, respectively. Compared with UiO-66, the absorption peak of μ3-O in the sample Mn50-UiO shifts toward the low wavenumber direction, which is attributed to the bonding between μ3-O and Mn on UiO-66.
[0082] In order to understand the composition and chemical bond information of the Mn50-UiO composite material, the present invention conducted an XPS test. The XPS full spectrum of the Mn50-UiO catalyst prepared in Example 1 is shown in Figure 5, the four main elements Mn, Zr, C and O exist on Mn50-UiO, indicating that Mn3O4 is successfully compounded with UiO-66, and the mass percentage of Mn3O4 on Mn50-UiO can be calculated to be 25% through the atomic content of Mn50-UiO. The XPS of C 1s further proves that Mn3O4 is compounded with UiO-66 through CO-Mn bonds. The 3dXPS spectrum of Zr shows that its binding energy does not change significantly after Mn modification, indicating that the introduction of Mn3O4 cannot significantly change the chemical structure and electronic state of Zr. The Mn 2p fine spectrum in the Mn50-UiO catalyst prepared in Example 1 is as follows Figure 6 As shown, in Mn2p 1 / 2 and Mn 2p 3 / 2 The spin-orbit splitting energy separation of 11.9 eV was observed in the orbit, which is between Mn2O3 (11.6 eV) and MnO (12.1 eV), indicating that manganese in Mn50-UiO is mainly in the form of Mn 2+ and Mn 3+ The valence state exists and the main component is Mn3O4, which is consistent with the results of XRD.
[0083] Performance Testing:
[0084] At room temperature, 0.2 g / L of catalyst was added to a reaction bottle containing 10 mg / L of organic pollutants ((bisphenol A (BPA), p-chlorophenol (4-CP), m-cresol (3-MP), rhodamine (RhB), ciprofloxacin (BCIP), tetracycline hydrochloride (TCH), 2,4,6-trichlorophenol (2,4,6-TCP)) (i.e., the concentrations of catalyst and organic pollutants in simulated sewage were 0.2 g / L and 10 mg / L, respectively), and ultrasonicated for 30 s to fully disperse the catalyst, and then 0.4 mM PMS was added. The reaction temperature was 25 ° C and the stirring rate was 600 rpm. Samples were taken every 3 min and quenched with an equal volume of ethanol to prevent further reaction. The reaction time was 30 min. The concentrations of 4-CP, 3-MP, BPA, BCIP, 2,4,6-TCP, RhB, and TCH were determined by ultra-high performance liquid chromatography (Thermo Scientific UltiMate 3000) detection.
[0085] The results (removal rates) of the catalytic degradation of BPA by the catalysts prepared in Examples 1 to 12 after 30 minutes are shown in Table 1.
[0086] Table 1
[0087] serial number catalyst Removal rate (%) 1 UiO-66 5.6 2 <![CDATA[Mn3O4]]> 21.2 3 <![CDATA[Mn3O4+UiO-66]]> 32.5 4 Example 1 100 5 Example 2 98.2 6 Example 3 99.1 7 Example 4 98.7 8 Example 5 98.2 9 Example 6 97.3 10 Example 7 99.2 11 Example 8 99.6 12 Example 9 97.6 13 Example 10 99.3 14 Embodiment 11 96.6 15 Example 12 97.5
[0088] Note: Mn3O4+UiO-66 in No. 3 in Table 1 is a simple physical mixed system, and the content ratio of manganese element to UiO-66 is the same as that in Example 5.
[0089] It can be seen from Table 1 that the Mn50-UiO catalyst prepared in each embodiment of the present invention shows a good effect on the removal of BPA, and is higher than UIO-66, Mn3O4, and also higher than the mixed system of Mn3O4 and UiO-66. It can be seen that the catalyst designed by the present invention is reasonable.
[0090] Figure 7 The removal rate of different organic matter by Mn50-UIO catalyst (the concentration of catalyst in the system is 0.2 g / L) is shown. It can be seen that Mn50-UIO catalyst has a good removal effect on different types of organic matter.
[0091] Figure 8 (a) is the degradation effect diagram of the Mn50-UiO / PMS system under different pH conditions. It can be seen that with the decrease of pH, the degradation effect of the catalyst gradually improves; (b) is the removal efficiency of different types of pollutants by Mn50-UiO under pH = 1. It can be seen that the removal effect of BPA is better, and the removal effect of 4-CP is slightly worse.
[0092] Fig. 9 The figure is a diagram showing the removal rate of BPA in sewage by the Mn50-UiO catalyst after different times of use. It can be seen that the removal rate of BPA is still as high as about 93% after 10 cycles of use. It can be seen that the catalyst prepared by the present invention has good stability and can be used multiple times.
[0093] In summary, the present invention utilizes the characteristics of strong interaction between the abundant μ3-OH or μ3-O on the surface of UiO-66 and metal ions, modifies the surface of UiO-66 with Mn oxide, forms a composite Mn-UiO-66 material, and obtains a Mn50-UiO catalyst with an optimal composition by systematically adjusting the manganese acetate content of the Mn precursor. Bisphenol A (BPA) is used as a model pollutant, and the synthesized Mn50-UiO metal composite material is applied to the degradation of organic pollutants in the aqueous phase. Studies have found that the composite material exhibits a high removal effect on phenolic pollutants under PMS or acidic conditions (pH<3), and its high catalytic activity originates from the Mn active sites enriched on the surface of UiO-66. Studies have shown that the Mn-based catalyst of the present invention is reasonably designed and can effectively remove phenolic water pollutants.
[0094] The above are only preferred specific implementations of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed in the present application should be included in the protection scope of the present application. Therefore, the protection scope of the present application should be based on the protection scope of the claims.
Claims
1. A method for preparing a Mn-UiO-66 material, characterized in that: Mn-UiO-66 material was prepared by a hydrothermal method using UiO-66 as a carrier and soluble manganese salt as a manganese precursor.
2. The method for preparing the Mn-UiO-66 material according to claim 1, characterized in that: The following steps are involved: UiO-66 is dispersed in water, ultrasonically obtained to obtain a suspension, a soluble manganese salt is added, ultrasonically and magnetically stirred to obtain a mixture, the mixture is subjected to a hydrothermal reaction, cooled to room temperature, centrifuged to obtain a precipitate, washed, and dried to obtain the Mn-UiO-66 material.
3. The method for preparing the Mn-UiO-66 material according to claim 2, characterized in that: The mass ratio of the UiO-66 to the manganese element in the soluble manganese salt is 1:(0.20-0.95).
4. The method for preparing the Mn-UiO-66 material according to claim 3, characterized in that: The mass ratio of the UiO-66 to the manganese element in the soluble manganese salt is 1:(0.30-0.95).
5. The method for preparing the Mn-UiO-66 material according to claim 2, characterized in that: The soluble manganese salt is one of manganese acetate, manganese nitrate, manganese oxalate and manganese chloride.
6. The method for preparing the Mn-UiO-66 material according to claim 2, characterized in that: The temperature of the hydrothermal reaction is 95-120° C. and the time is 15-24 hours.
7. A Mn-UiO-66 material, characterized in that: Prepared according to the preparation method according to any one of claims 1 to 6.
8. Use of the Mn-UiO-66 material as claimed in claim 7 in treating organic matter in wastewater.
9. The use according to claim 8, characterized in that: The organic matter is phenolic organic matter, antibiotics or rhodamine B.
10. The use according to claim 8, characterized in that: When the organic matter is phenolic organic matter, the pH of the wastewater is less than 3 or the wastewater contains PMS.
Citation Information
Cited By
Mn-doped UiO-66 catalyst and application thereof in activating periodate to degrade organic pollutants