Activation method of structural catalyst for silane production
Through the combination of nitrogen bubble pre-activated and low-temperature leaching activation, the problem of large temperature rise during the activation of structural catalysts is solved, the gentle control and safety improvement of temperature rise are achieved, and the service life of the catalyst is extended.
Patent Information
- Application Number
- CN202411002227.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-11-12
AI Technical Summary
The existing structural catalyst activation methods have problems such as large temperature rise and difficulty in controlling, which leads to the risk of safety accidents and fails to effectively extend the service life of the catalyst.
The combined method of nitrogen bubble pre-activation and low-temperature leaching activation was adopted. The nitrogen entrains chlorosilane to contact the catalyst, and the reaction heat is controlled below 40°C, and the chlorosilane flow rate is adjusted to calm the temperature rise during the leaching process.
It reduces the exothermic temperature and risk during catalyst activation, shortens the activation time, and improves safety and catalyst service life.
Smart Images

Figure CN118925811A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of silane preparation, and in particular relates to an activation method for a structured catalyst used in silane production. Background Art
[0002] Silane is a key material required for existing semiconductors. It is the basic raw material for a series of silicon compounds such as single crystal silicon, polycrystalline silicon, amorphous silicon, metal silicide, silicon nitride, silicon carbide, and silicon oxide. It has been widely used and mass-produced.
[0003] In large-scale process production, structural catalysts are increasingly valued and widely used in the preparation of silanes because of their advantages of high conversion rate, stable performance and long service life. However, as the generation process proceeds, the activity of the structural catalyst will decrease, thereby affecting the stability and conversion rate of the silane. Existing patent CN106865553A discloses a method for activating a resin catalyst for preparing trichlorosilane. The patent obtains trichlorosilane and an activator intermediate by passing chlorosilane into a reactor with a catalyst and an activator, thereby completing the activation of the catalyst and extending the service life of the catalyst. However, the patent does not take into account the safety issues of temperature rise during the catalyst activation process. In addition, the conventional activation method of spraying chlorosilane on the surface of the structural catalyst also has the problem of large temperature rise, difficulty in control, and prone to safety accidents.
[0004] Therefore, there is an urgent need for an activation method with a gentle temperature rise and the ability to reduce the risk of catalyst activation to solve the above problems. Summary of the invention
[0005] In order to solve the above technical problems, the present invention provides a method for activating a structured catalyst for silane production.
[0006] To achieve the above object, the present invention provides the following technical solutions:
[0007] The invention provides a method for activating a structured catalyst for silane production, comprising the following steps: introducing chlorosilane as an activator into a tower kettle, firstly using a bubbling method to make the chlorosilane contact with the structured catalyst under the entrainment of nitrogen for pre-activation, and the pre-activation is completed when the chlorosilane concentration data monitored at the top of the tower kettle is stable; then, the structured catalyst is subjected to low-temperature elution activation using chlorosilane as an eluent, thereby completing the activation of the structured catalyst.
[0008] Preferably, the flow rate of the nitrogen is 1 to 2 m 3 / h.
[0009] Preferably, the reaction heat T during the pre-activation process is controlled to be ≤40°C.
[0010] Preferably, the step of cooling the activator chlorosilane to 10-20° C. is further included before the activator chlorosilane is introduced into the tower kettle.
[0011] Preferably, the flow rate of chlorosilane during the low-temperature elution activation process is 50% of the designed flow rate, and when the temperature rise of the structured catalyst bed exceeds 10° C., the flow rate increases by 10-20%.
[0012] Preferably, the process parameters of nitrogen bubbling pre-activation include: the flow rate of nitrogen is 1 to 2 m 3 / h.
[0013] Preferably, the structured catalyst is in the shape of a block.
[0014] Preferably, the pre-activation process specifically includes the following steps: feeding the activating agent chlorosilane into the tower kettle, and then introducing nitrogen for bubbling, the nitrogen entraining chlorosilane passes through the packing layer and contacts the structural catalyst layer to pre-activate the structural catalyst; when the temperature of the structural catalyst layer rises to above 40°C, reducing the feed, and when the temperature of the structural catalyst layer drops to below 40°C, increasing the feed, thereby controlling the temperature in the tower kettle to remain below 40°C; during the activation process, regularly detecting the tail gas at the top of the tower, and when a stable concentration of chlorosilane is detected in the tail gas, stopping the feed and passing nitrogen to complete the pre-activation.
[0015] Preferably, during the pre-activation process, the remote liquid level of chlorosilane in the tower kettle is controlled to be 20-30%.
[0016] Preferably, the temperature of the structured catalyst layer includes three temperature sections, T1, T2 and T3; when any temperature of the three temperature sections rises to above 40°C, the feed needs to be reduced.
[0017] Compared with the prior art, the present invention has the following advantages and technical effects:
[0018] The present invention pre-activates the structured catalyst by nitrogen bubbling first, and then performs leaching activation. The combination of the two activation methods reduces the exothermic temperature of the structured catalyst in the tower kettle, makes the temperature rise of the activation process gentle and easy to control, and greatly shortens the activation time, further solves the problem of large heat release in the catalyst activation process, reduces the risk of structured catalyst activation, and improves safety, which is of great significance to the technical field of structured catalyst activation. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] The drawings constituting a part of the present application are used to provide a further understanding of the present application. The illustrative embodiments and descriptions of the present application are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:
[0020] Figure 1 It is a schematic diagram of the structure of the device used in the activation process in Example 1;
[0021] Figure 2 is a curve diagram of the change of the temperatures T1, T2, and T3 of the structured catalyst layer in step (1) of Example 1;
[0022] Figure 3 The graph of the change of the temperature T1, T2, and T3 of the structured catalyst layer in step (1) of comparative example 1;
[0023] Figure 4 It is a curve diagram of the change of the temperature T1, T2, and T3 of the structure catalyst layer during the activation process of Comparative Example 2;
[0024] Figure 5 This is a curve chart of the changes in the temperatures T1, T2, and T3 of the structural catalyst layer during the elution process in step (2) of Example 1. DETAILED DESCRIPTION
[0025] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0026] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.
[0027] An embodiment of the present invention provides a method for activating a structured catalyst for silane production, comprising the following steps: introducing an activating agent, chlorosilane, into a tower kettle, first using a bubbling method to allow the chlorosilane to contact with the structured catalyst under the entrainment of nitrogen for pre-activation, and the pre-activation is completed when the chlorosilane concentration data monitored at the top of the tower kettle is stable; then, the structured catalyst is subjected to low-temperature elution activation using chlorosilane as an eluent, thereby completing the activation of the structured catalyst.
[0028] The present invention activates the structured catalyst by nitrogen bubbling, thereby reducing the exothermic temperature of the structured catalyst, making the temperature rise in the activation process gentle and easy to control, and the activation time short, solving the problem of large heat release in the catalyst activation process, reducing the risk of structured catalyst activation, and improving safety.
[0029] The activation method provided by the invention is applicable to various structured catalysts used for silane production.
[0030] In a preferred embodiment, the flow rate of the nitrogen is 1 to 2 m 3 / h. The present invention controls the flow rate of nitrogen within the above range to ensure that the change of reaction heat T during the pre-activation process tends to be gentle, thereby reducing the risk of activation; if the flow rate of nitrogen is too large, the heat release of the catalyst will increase significantly, resulting in a large temperature rise that is difficult to control and prone to safety accidents.
[0031] In a preferred embodiment, the reaction heat T during the pre-activation process is controlled to be ≤40° C. The present invention controls the reaction heat T during the pre-activation process to be below 40° C. to avoid destructive damage to the catalyst caused by excessively high temperature.
[0032] In a preferred embodiment, the step of cooling the activator chlorosilane to 10-20° C. is further included before the activator chlorosilane is introduced into the tower kettle.
[0033] In a preferred embodiment, the flow rate of chlorosilane during the low-temperature elution activation process is 50% of the designed flow rate, and when the temperature rise of the structured catalyst bed exceeds 10° C., the flow rate increases by 10-20%, and the temperature of the chlorosilane is 10-20° C. The present invention uses low-temperature chlorosilane to elute the pre-activated structured catalyst, which helps to reduce the temperature of the structured catalyst layer and improve the safety of the activation process.
[0034] In a preferred embodiment, the structured catalyst is in a block shape. The block-shaped structured catalyst of the present invention is easy to recycle and reuse.
[0035] In a preferred embodiment, the pre-activation process specifically includes the following steps: feeding the activating agent chlorosilane into the tower kettle, and then introducing nitrogen for bubbling, the nitrogen entraining chlorosilane passes through the packing layer and contacts the structural catalyst layer to pre-activate the structural catalyst; when the temperature of the structural catalyst layer rises to above 40°C, reducing the feed, and when the temperature of the structural catalyst layer drops below 40°C, increasing the feed, thereby controlling the temperature in the tower kettle to remain below 40°C; during the activation process, regularly detecting the tail gas at the top of the tower, when a stable concentration of chlorosilane is detected in the tail gas, stopping the feed and passing nitrogen to complete the pre-activation.
[0036] In a preferred embodiment, during the pre-activation process, the remote liquid level of chlorosilane in the tower kettle is controlled to be 20-30%.
[0037] In a preferred embodiment, the temperature of the structured catalyst layer includes three temperature sections, T1, T2 and T3; when any temperature of the three temperature sections rises to above 40°C, the feed needs to be reduced. The present invention further ensures the safety of the activation process by monitoring the three temperature sections of the structured catalyst layer during the nitrogen bubbling activation process.
[0038] In a preferred embodiment, the low-temperature elution activation specifically includes the following steps: injecting low-temperature chlorosilane into the reflux tank, turning on the reflux pump to perform low-temperature elution activation on the structured catalyst, and when the temperature change of the structured catalyst layer is within 3°C or the tower bottom liquid level rises by more than 5%, elution is terminated, thereby completing the activation of the structured catalyst. The present invention ensures the full activation of the structured catalyst through low-temperature elution activation.
[0039] In a preferred embodiment, the temperature of the low-temperature chlorosilane is 10-20° C., and the liquid level of the low-temperature chlorosilane is 80%.
[0040] In the embodiments of the present invention, normal temperature refers to "25±2°C".
[0041] Unless otherwise specified, the raw materials in the examples of the present invention were purchased from commercial sources.
[0042] Example 1
[0043] A method for activating a structured catalyst for silane production, comprising the following steps:
[0044] (1) Open the feed valve of the No. 1 pipeline of the cooler shell side to cool the chlorosilane to obtain low-temperature chlorosilane with a temperature of 20°C; send the low-temperature chlorosilane into the tower kettle, and control the remote transmission liquid level at 30%, then open the temporary nitrogen pipeline valve on the top of the tower kettle pump filter to introduce nitrogen for bubbling, and the nitrogen entrains the low-temperature chlorosilane through the packing layer and contacts the structured catalyst layer to activate the structured catalyst, wherein the flow rate of nitrogen is 1 to 2 m 3 / h; observe the temperature change of the structural catalyst layer (T1, T2, T3); when the temperature of the structural catalyst layer rises to above 40°C, slowly close the feed valve to reduce the feed, balance the bed temperature, and wait until the temperature of the structural catalyst layer drops below 40°C, then increase the feed; during the activation process, regularly detect the tail gas at the top of the tower, and when a stable concentration of chlorosilane is detected in the tail gas, close the nitrogen and temporary feed pipeline valves, and the bubbling process ends;
[0045] (2) Low-temperature chlorosilane at 20°C is injected into the upper reflux tank through a temporary feed pipeline, the liquid level is controlled at 80%, and the reflux pump is turned on to perform low-temperature elution of the structured catalyst. When the temperature change of the structured catalyst layer is within 3°C or the liquid level in the tower bottom rises by more than 5%, the elution is terminated and the activation is completed.
[0046] Comparative Example 1
[0047] The difference from Example 1 is that in step (1), the flow rate of nitrogen during the bubbling process is controlled to be 3-5m 3 / h, and the remaining steps are the same as in Example 1.
[0048] Comparative Example 2
[0049] Chlorosilane at room temperature is injected into the upper reflux tank through a temporary feed pipeline, the liquid level is controlled at 80%, and the reflux pump is turned on to elute the structural catalyst. When the temperature change of the structural catalyst layer is within 3°C or the liquid level in the tower bottom rises by more than 5%, activation is completed.
[0050] Figure 1 This is a schematic diagram of the structure of the device used in the activation process in Example 1.
[0051] Figure 2 The curve diagram of the change of the temperature T1, T2, and T3 of the structure catalyst layer in step (1) of Example 1. Figure 2 It can be seen that the highest point T2 temperature is only 20.7°C, which indicates that the heat release of the catalyst structured by the activation method of the present invention is small, the temperature rise is gentle, and the risk of the bubbling activation process can be controlled.
[0052] Figure 3 The curve diagram of the change of the temperature T1, T2, and T3 of the structure catalyst layer in step (1) of comparative example 1 is shown in FIG. Figure 3 It can be seen that by increasing the nitrogen flow rate, T2 rises to 40°C, T3 temperature rises to 42°C, and the heat release of the catalyst increases significantly. At this time, the bubbling nitrogen valve and the raw material manual valve should be closed first, and then the normal temperature nitrogen manual valve of the tower kettle should be opened for cold blowing and cooling. After several hours of blowing, the bed temperature can be lowered, which not only prolongs the activation time but also poses a safety risk in the bubbling activation process.
[0053] Figure 4 The curve diagram of the change of the temperature T1, T2, and T3 of the structure catalyst layer during the activation process of Comparative Example 2 is shown in FIG. Figure 4 It can be seen that in Comparative Example 2, the catalyst is activated by a direct elution method. During the activation process, the heat release is too large, the temperature is uncontrollable, the catalyst surface maintains a high temperature for a long time, and the catalyst is destructively damaged. The cooling time is also long. In addition, due to the closed system, the safety risk is relatively large. In Comparative Example 2, room temperature chlorosilane is directly sprayed on the catalyst surface. The surface area of the catalyst is large. When the sprayed chlorosilane contacts the catalyst, a large amount of heat is released, and the temperature trend rises significantly. In addition, the direct spraying contact area is large. If the temperature rises linearly, even if the reflux is stopped immediately and the room temperature nitrogen hand valve at the bottom is opened to cool the catalyst, the heat release of the bed will continue, which has a great impact on the performance of the catalyst and has the risk of damage.
[0054] Figure 5 The curve diagram of the change of the temperature T1, T2, and T3 of the structure catalyst layer during the elution process of step (2) of Example 1. Figure 5It can be seen that after the catalyst has undergone an exothermic process, the heat release is very slow after contacting chlorosilane again. The large-scale contact of the reflux liquid with the catalyst achieves deep activation of the catalyst, which not only ensures the activation effect but also greatly reduces the risk of large heat release and difficulty in controlling the temperature.
[0055] The above are only preferred specific implementations of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed in the present application should be included in the protection scope of the present application. Therefore, the protection scope of the present application should be based on the protection scope of the claims.
Claims
1. A method for activating a structured catalyst for silane production, characterized in that: The following steps are involved: The activator chlorosilane is introduced into the tower kettle, and the chlorosilane is first brought into contact with the structured catalyst under the entrainment of nitrogen by bubbling to perform pre-activation, and the pre-activation is completed when the chlorosilane concentration data monitored at the top of the tower kettle is stable; then, the structured catalyst is subjected to low-temperature elution activation using chlorosilane as the eluent, thereby completing the activation of the structured catalyst.
2. The method for activating a structured catalyst for silane production according to claim 1, characterized in that: The flow rate of the nitrogen is 1-2 m 3 / h.
3. The method for activating a structured catalyst for silane production according to claim 1, characterized in that: Control the reaction heat T≤40℃ during the pre-activation process.
4. The method for activating a structured catalyst for silane production according to claim 1, characterized in that: The method further comprises cooling the activator chlorosilane to 10-20° C. before the activator chlorosilane is introduced into the tower kettle.
5. The method for activating a structured catalyst for silane production according to claim 1, characterized in that: The flow rate of chlorosilane in the low-temperature elution activation process is 50% of the designed flow rate. When the temperature rise of the structured catalyst bed exceeds 10° C., the flow rate increases by 10-20%.
6. The method for activating a structured catalyst for silane production according to claim 1, characterized in that: The process parameters of nitrogen bubbling pre-activation include: nitrogen flow rate is 1~2m 3 / h.
7. The method for activating a structured catalyst for silane production according to claim 1, characterized in that: The structured catalyst is in the shape of a block.
8. The method for activating a structured catalyst for silane production according to claim 1, characterized in that: The pre-activation process specifically includes the following steps: feeding the activating agent chlorosilane into the tower kettle, and then introducing nitrogen for bubbling, wherein the nitrogen carries the chlorosilane through the packing layer and contacts the structural catalyst layer to pre-activate the structural catalyst; when the temperature of the structural catalyst layer rises to above 40°C, reducing the feed, and when the temperature of the structural catalyst layer drops to below 40°C, increasing the feed, thereby controlling the temperature in the tower kettle to be maintained below 40°C; during the activation process, regularly detecting the tail gas at the top of the tower, and when a stable concentration of chlorosilane is detected in the tail gas, stopping the feed and passing nitrogen to complete the pre-activation.
9. The method for activating a structured catalyst for silane production according to claim 8, characterized in that: During the preactivation process, the remote liquid level of chlorosilane in the tower kettle is controlled to be 20-30%.
10. The method for activating a structured catalyst for silane production according to claim 8, characterized in that: The temperature of the structured catalyst layer includes three temperature sections, T1, T2 and T3; when any temperature of the three temperature sections rises to above 40°C, the feed needs to be reduced.
Citation Information
Patent Citations
Activating method for preparing resin catalyst of trichlorosilane
CN106865553A