Coating preparation method of magnetic metal absorbent
By pre-ball milling and precursor solution processing of carbonyl iron powder, an inorganic or organic layer is generated, which solves the problem of deterioration of wave absorption performance of carbonyl iron powder in corrosive environment, improves magnetic permeability and realizes an industrial-applicable coating method .
Patent Information
- Application Number
- CN202410988045.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-11-12
AI Technical Summary
The prior art cannot effectively solve the problem of deterioration in the absorption performance of carbonyl iron powder in corrosive environments, and the conventional coating method is poor in applicability and cannot meet engineering needs.
By pre-ball milling of carbonyl iron powder, anhydrous ethanol and zirconia balls, and adding a precursor solution for ball milling, an inorganic or organic layer is formed, followed by separation, drying, sieving and high-temperature heating treatment to form efficient coating layer.
It improves the magnetic permeability of carbonyl iron powder, enhances its absorption performance, and realizes the simplicity and controllability of the coating process, which is suitable for industrial promotion.
Smart Images

Figure CN118926522A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of wave absorbing materials, and in particular relates to a coating preparation method for a magnetic metal absorber. Background Art
[0002] The rapid development of the fifth generation of electronic information technology and communication technology has led to the widespread use of more and more electronic and electrical equipment. With the rapid development of information, it also brings the problem of electromagnetic wave pollution. Electromagnetic wave pollution not only interferes with the normal function of electronic equipment, causing interruption, degradation and failure, but also has an adverse impact on conventional production applications and daily life, and will also cause harm to human health and the ecosystem. Therefore, electromagnetic wave absorption technology occupies an increasingly important role, and research on absorbing materials with advantages such as strong absorption capacity, broadband, light weight and thin thickness is also being deepened. At present, the most commonly used absorbent in absorbing materials is carbonyl iron powder. Carbonyl iron powder has high saturation magnetization, high Curie temperature, good permeability dispersion characteristics, can be mass-produced at low cost, and is widely used in electromagnetic shielding and aviation fields.
[0003] However, in recent years, the environmental resistance requirements of absorbing materials have become increasingly higher. Since absorbing materials are often directly exposed to corrosive environments (rich in acids, alkalis, and salts), their absorbing performance is seriously deteriorated. Therefore, coating the carbonyl iron powder absorber can prevent the carbonyl iron powder from being corroded. At present, the coating process of the carbonyl iron powder absorber usually adopts the sol-gel method, emulsion polymerization, graft polymerization, in-situ polymerization, etc. to coat the surface of the absorber with an inorganic layer (silicon dioxide, graphene), an organic layer (polyaniline, polypyrrole, organosilane), and an organic-inorganic hybrid coating, etc. However, the currently disclosed coating methods are only in the laboratory stage (each batch is in grams), which cannot meet the engineering needs. The conventional coating methods have poor applicability and other shortcomings that are still difficult to overcome. Therefore, it is necessary to improve the traditional spherical carbonyl iron powder coating method.
[0004] In view of this, the present inventor provides a coating preparation method for a magnetic metal absorbent to solve the above technical problems. Summary of the invention
[0005] The purpose of the present invention is to overcome the shortcomings of the above-mentioned prior art and propose a coating preparation method for a magnetic metal absorbent, by pre-ball milling carbonyl iron powder, anhydrous ethanol and zirconium oxide balls in a set proportion, and then adding a precursor solution to continue ball milling, in the process of carbonyl iron powder flaking, an inorganic layer or an organic layer is generated in situ on its surface, and then through separation, drying, screening and high-temperature heating treatment, the carbonyl iron powder absorbent is ensured to be coated to prevent the carbonyl iron powder from being corroded, and the magnetic permeability of the carbonyl iron powder is improved.
[0006] In order to achieve the above object, the present invention adopts the following technical solutions:
[0007] The present invention provides a coating preparation method for a magnetic metal absorbent, comprising the following steps:
[0008] Step 1, pouring a set proportion of carbonyl iron powder, anhydrous ethanol and zirconium oxide balls into a ball mill, and stirring to pre-ball mill the carbonyl iron powder;
[0009] Step 2, adding the pre-prepared precursor solution into the ball milling tank after the pre-ball milling, stirring and ball milling the carbonyl iron powder, and performing separation treatment after the ball milling to obtain the first flaky carbonyl iron powder with an inorganic layer or an organic layer on the surface and the zirconium oxide ball with the first flaky carbonyl iron powder attached;
[0010] Step 3, separating the first flaky carbonyl iron powder obtained in step 2 from the zirconium oxide balls attached with the first flaky carbonyl iron powder, and then separating the separated zirconium oxide balls attached with the first flaky carbonyl iron powder again with anhydrous ethanol to obtain zirconium oxide balls and a turbid liquid containing the first flaky carbonyl iron powder and anhydrous ethanol;
[0011] Step 4, filtering the turbid liquid obtained in step 3 to obtain a second flaky carbonyl iron powder with an inorganic layer or an organic layer coated on the surface;
[0012] Step 5, placing the first flaky carbonyl iron powder and the second flaky carbonyl iron powder into an oven, and keeping the oven temperature at 50° C. to 80° C. for 8 h to 15 h to obtain a third flaky carbonyl iron powder coated with an inorganic layer or an organic layer;
[0013] Step 6, sieving the third flaky carbonyl iron powder obtained in step 5, placing the sieved third flaky carbonyl iron powder into a vacuum furnace, heating it to 700°C to 800°C at a set speed, keeping it warm for 2h to 4h, and then annealing it to obtain the target flaky carbonyl iron powder with an inorganic layer or an organic layer coated on the surface.
[0014] Preferably, the surface of the target flaky carbonyl iron powder is coated with an inorganic layer.
[0015] Specifically, the carbonyl iron powder in step 1 is a commercially available common spherical carbonyl iron powder formed by aerosolization, which is not limited here.
[0016] Specifically, in step 3, the first flaky carbonyl iron powder and the zirconium oxide balls are separated by using a sieve of about 10 meshes, as long as the first flaky carbonyl iron powder and the zirconium oxide balls can be separated.
[0017] Furthermore, in step 1, the mass ratio of the carbonyl iron powder, anhydrous ethanol and zirconium oxide balls is 4-5:2-6:15-25.
[0018] Furthermore, the stirring speed in step 1 is 100 r / min to 150 r / min, and the stirring time is 3 h to 5 h.
[0019] Furthermore, in step 2, the stirring speed is 100 r / min to 150 r / min, and the stirring time is 2 h to 5 h.
[0020] Furthermore, in step 2, the precursor solution includes a first mixed solution and a second mixed solution, and the mass ratio of the first mixed solution to the second mixed solution is 6-10:2-5.
[0021] Furthermore, the first mixed solution is obtained by mixing ammonia water and deionized water in a mass ratio of 6-8:10-13, and the concentration of the ammonia water is 24%-28%.
[0022] Furthermore, the second mixed liquid is obtained by mixing a silicon source material and anhydrous ethanol in a mass ratio of 1:1 to 8.
[0023] Furthermore, the silicon source material is any one of tetraethyl orthosilicate, tetramethyl orthosilicate, dimethyldiethoxysilane (DDS), diphenyldiethoxysilane (DPDS), and (3-aminopropyl)triethoxysilane.
[0024] Preferably, the silicon source material is tetraethyl orthosilicate.
[0025] Furthermore, in step 6, a sieve with a mesh size of 80 to 200 is selected for the screening process.
[0026] Furthermore, in step 6, the set speed is 5°C / min to 10°C / min.
[0027] In the present invention, ammonia water is used as a catalyst and the Stober method is adopted to react water and a silicon source to generate silicon dioxide, namely, an inorganic layer.
[0028] Compared with the prior art, the present invention has the following beneficial effects:
[0029] 1) The present invention provides a coating preparation method for a magnetic metal absorbent. The method pre-mills a set proportion of carbonyl iron powder, anhydrous ethanol and zirconium oxide balls, and then adds a precursor solution to continue ball milling, so that the carbonyl iron powder can generate silicon dioxide in situ on its surface during the flaking process. The carbonyl iron powder is separated, dried, sieved and heated at high temperature to achieve a one-step method to change the microstructure of the carbonyl iron powder, increase the flaking degree and aspect ratio of the carbonyl iron powder, and improve the magnetic permeability of the carbonyl iron powder. The coating preparation method of the present invention is simple and controllable, easy to scale up, and can be promoted industrially.
[0030] 2) The present invention provides a coating preparation method for a magnetic metal absorbent. By subjecting the flaky carbonyl iron powder coated with an inorganic layer or an organic layer to high-temperature treatment, the silicon dioxide on the surface of the flaky carbonyl iron powder can be purified, and the internal stress of the flaky carbonyl iron powder after ball milling can be eliminated, thereby achieving the purpose of enhancing the magnetic properties of the absorbent.
[0031] 3) The present invention provides a method for preparing a coated magnetic metal absorbent, which takes advantage of more complete stirring by ball milling, uses aqueous ammonia as a catalyst, and utilizes the reaction of a silicon source with water to generate silicon dioxide, thereby achieving uniform coating of carbonyl iron powder. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] The accompanying drawings are incorporated in and constitute a part of this specification and, together with the description, serve to explain the principles of the present invention.
[0033] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.
[0034] Figure 1 The present invention is a flow chart of the coating preparation method of the magnetic metal absorbent;
[0035] Figure 2 This is a SEM scanning electron microscope image of the spherical carbonyl iron powder selected in step 1 of Example 1 of the present invention;
[0036] Figure 3 This is a SEM scanning electron microscope image of the flaky carbonyl iron powder after ball milling in step 2 of Example 1 of the present invention;
[0037] Figure 4 This is a SEM scanning electron microscope image of the flaked coated carbonyl iron powder prepared in Example 1 of the present invention;
[0038] Figure 5 This is a comparison diagram of the magnetic permeability of the flaked coated carbonyl iron powder prepared in Example 1 of the present invention;
[0039] Figure 6 This is a comparison chart of the coating reflectivity of the flaked and coated carbonyl iron powder prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0040] Here, exemplary embodiments will be described in detail, and the embodiments described in the following exemplary embodiments do not represent all embodiments consistent with the present invention. Instead, they are only examples consistent with some aspects of the present invention described in detail in the appended claims.
[0041] Preparation Example 1
[0042] Preparing a first mixed solution: mixing ammonia water and deionized water in a mass ratio of 1:2 to form a first mixed solution;
[0043] Preparing a second mixed solution: mixing tetraethyl orthosilicate and anhydrous ethanol at a mass ratio of 1:8 to form a second mixed solution, wherein the concentration of tetraethyl orthosilicate in the second mixed solution is 0.6 mol / L;
[0044] Preparing a precursor solution: mixing the prepared first mixed solution and the second mixed solution in a mass ratio of 8:3 to obtain a precursor solution.
[0045] Preparation Example 2
[0046] Preparing a first mixed solution: mixing ammonia water and deionized water in a mass ratio of 7:10 to form a first mixed solution;
[0047] Preparing a second mixed solution: mixing tetraethyl orthosilicate and anhydrous ethanol at a mass ratio of 1:3 to form a second mixed solution, wherein the concentration of tetraethyl orthosilicate in the second mixed solution is 1.2 mol / L;
[0048] Preparing a precursor solution: mixing the prepared first mixed solution and the second mixed solution at a mass ratio of 3:1 to obtain a precursor solution.
[0049] Preparation Example 3
[0050] Preparing a first mixed solution: mixing ammonia water and deionized water in a mass ratio of 8:13 to form a first mixed solution;
[0051] Preparing a second mixed solution: mixing tetraethyl orthosilicate and anhydrous ethanol at a mass ratio of 1:1 to form a second mixed solution, wherein the concentration of tetraethyl orthosilicate in the second mixed solution is 2.4 mol / L;
[0052] Preparing a precursor solution: mixing the prepared first mixed solution and the second mixed solution in a mass ratio of 2:1 to obtain a precursor solution.
[0053] Example 1
[0054] The embodiment of the present invention provides a coating preparation method of a magnetic metal absorbent, comprising the following steps:
[0055] Step 1, pour 1000g of spherical carbonyl iron powder, 400g of anhydrous ethanol and 2000g of zirconium oxide balls into a 5L ball mill, stir at a speed of 100r / min for 3h to obtain carbonyl iron powder with a certain degree of lamellarity;
[0056] Step 2, adding the precursor solution of Preparation Example 1 into the ball mill after pre-ball milling, sealing the ball mill to prevent moisture in the external air from entering the ball mill and affecting the reaction, stirring at a speed of 100 r / min for 3 hours to obtain a first flaky carbonyl iron powder coated with silicon dioxide and a zirconium oxide ball with the first flaky carbonyl iron powder attached thereto;
[0057] In the above process, water and tetraethyl orthosilicate undergo a hydrolysis reaction to produce silanol [Si(OH)4)] and ethanol. The added ammonia provides hydroxide and an alkaline environment for the reaction. Hydroxide accelerates the formation of silanol. The -OH on the silanol forms a hydrogen bond with the -OH on the surface of the flaky carbonyl iron powder, which is dehydrogenated in an alkaline environment to form a Lewis base, and then continues to undergo dehydration polymerization with other silicon atoms. Finally, while the carbonyl iron powder is flaked, a reticular silica is gradually generated on its surface.
[0058] Step 3, using a 10-mesh sieve to separate the first flaky carbonyl iron powder obtained in step 2 from the zirconium oxide balls attached with the first flaky carbonyl iron powder, and then using anhydrous ethanol to separate the separated zirconium oxide balls attached with the first flaky carbonyl iron powder again to obtain zirconium oxide balls and a turbid liquid containing the first flaky carbonyl iron powder and anhydrous ethanol;
[0059] Step 4: Filter the anhydrous ethanol from the turbid liquid obtained in step 3 by vacuum filtration to obtain a second flaky carbonyl iron powder coated with silicon dioxide;
[0060] Step 5, placing the first flaky carbonyl iron powder and the second flaky carbonyl iron powder obtained above into an oven to remove anhydrous ethanol, and keeping the oven temperature at 80° C. for 10 hours to obtain a third flaky carbonyl iron powder coated with silicon dioxide;
[0061] Step 6, filtering the third flaky carbonyl iron powder obtained in step 5 using a 200-mesh sieve, placing the sieved third flaky carbonyl iron powder in a vacuum furnace, heating it to 800°C at a rate of 10°C / min, and maintaining it for 4 hours to complete annealing, thereby obtaining the target flaky carbonyl iron powder with an inorganic layer or an organic layer coated on the surface, i.e., the flaky coated carbonyl iron powder. The silicon dioxide particles in situ generated on the surface of the flaky coated carbonyl iron powder form a highly crystalline and dense silicon dioxide protective layer to protect the carbonyl iron powder.
[0062] Example 2
[0063] The embodiment of the present invention provides a coating preparation method of a magnetic metal absorbent, comprising the following steps:
[0064] Step 1, pour 6000g of spherical carbonyl iron powder, 2400g of anhydrous ethanol and 12000g of zirconium oxide balls into a 20L ball mill, stir at a speed of 140r / min for 5h to obtain carbonyl iron powder with a certain degree of lamellarity;
[0065] Step 2, adding the precursor solution of Preparation Example 2 into the ball mill after pre-ball milling, sealing the ball mill to prevent moisture in the external air from entering the ball mill and affecting the reaction, stirring at a speed of 140 r / min for 2 hours to obtain a first flaky carbonyl iron powder coated with silicon dioxide and a zirconium oxide ball with the first flaky carbonyl iron powder attached thereto;
[0066] In the above process, water and tetraethyl orthosilicate undergo a hydrolysis reaction to produce silanol [Si(OH)4)] and ethanol. The added ammonia provides hydroxide and an alkaline environment for the reaction. Hydroxide accelerates the formation of silanol. The -OH on the silanol forms a hydrogen bond with the -OH on the surface of the flaky carbonyl iron powder, which is dehydrogenated in an alkaline environment to form a Lewis base, and then continues to undergo dehydration polymerization with other silicon atoms. Finally, while the carbonyl iron powder is flaked, a reticular silica is gradually generated on its surface.
[0067] Step 3, using a 10-mesh sieve to separate the first flaky carbonyl iron powder obtained in step 2 from the zirconium oxide balls attached with the first flaky carbonyl iron powder, and then using anhydrous ethanol to separate the separated zirconium oxide balls attached with the first flaky carbonyl iron powder again to obtain zirconium oxide balls and a turbid liquid containing the first flaky carbonyl iron powder and anhydrous ethanol;
[0068] Step 4: filtering the turbid liquid obtained in step 3 with anhydrous ethanol by gravity filtration to obtain a second flaky carbonyl iron powder coated with silicon dioxide;
[0069] Step 5, placing the first flaky carbonyl iron powder and the second flaky carbonyl iron powder obtained above into an oven to remove the anhydrous ethanol, and keeping the oven temperature at 50° C. for 8 hours to obtain a third flaky carbonyl iron powder coated with silicon dioxide;
[0070] Step 6, filtering the third flaky carbonyl iron powder obtained in step 5 through an 80-mesh sieve, placing the sieved third flaky carbonyl iron powder into a vacuum furnace, heating the temperature to 700°C at a rate of 5°C / min, and maintaining the temperature for 3 hours to complete annealing, thereby obtaining a target flaky carbonyl iron powder coated with an inorganic layer or an organic layer on the surface, wherein the silicon dioxide particles in situ generated on the surface of the target flaky carbonyl iron powder form a highly crystalline and dense silicon dioxide protective layer to protect the carbonyl iron powder.
[0071] Example 3
[0072] The embodiment of the present invention provides a coating preparation method of a magnetic metal absorbent, comprising the following steps:
[0073] Step 1, pour 20000g of spherical carbonyl iron powder, 6000g of anhydrous ethanol and 60000g of zirconium oxide balls into a 60L ball mill, stir at a speed of 110r / min for 4h to obtain carbonyl iron powder with a certain degree of lamellarity;
[0074] Step 2, adding the precursor solution of Preparation Example 3 into the ball mill after pre-ball milling, sealing the ball mill to prevent moisture in the external air from entering the ball mill and affecting the reaction, stirring at a speed of 110 r / min for 4 hours to obtain a first flaky carbonyl iron powder coated with silicon dioxide and a zirconium oxide ball with the first flaky carbonyl iron powder attached thereto;
[0075] In the above process, water and tetraethyl orthosilicate undergo a hydrolysis reaction to produce silanol [Si(OH)4)] and ethanol. The added ammonia provides hydroxide and an alkaline environment for the reaction. Hydroxide accelerates the formation of silanol. The -OH on the silanol forms a hydrogen bond with the -OH on the surface of the flaky carbonyl iron powder, which is dehydrogenated in an alkaline environment to form a Lewis base, and then continues to undergo dehydration polymerization with other silicon atoms. Finally, while the carbonyl iron powder is flaked, a reticular silica is gradually generated on its surface.
[0076] Step 3, using a 10-mesh sieve to separate the first flaky carbonyl iron powder obtained in step 2 from the zirconium oxide balls attached with the first flaky carbonyl iron powder, and then using anhydrous ethanol to separate the separated zirconium oxide balls attached with the first flaky carbonyl iron powder again to obtain zirconium oxide balls and a turbid liquid containing the first flaky carbonyl iron powder and anhydrous ethanol;
[0077] Step 4: filtering the turbid liquid obtained in step 3 with anhydrous ethanol by gravity filtration to obtain a second flaky carbonyl iron powder coated with silicon dioxide;
[0078] Step 5, placing the first flaky carbonyl iron powder and the second flaky carbonyl iron powder obtained above into an oven to remove anhydrous ethanol, and keeping the oven temperature at 60° C. for 15 hours to obtain a third flaky carbonyl iron powder coated with silicon dioxide;
[0079] Step 6, filtering the third flaky carbonyl iron powder obtained in step 5 through an 80-mesh sieve, placing the sieved third flaky carbonyl iron powder into a vacuum furnace, heating the temperature to 800°C at a rate of 5°C / min, and maintaining the temperature for 2 hours to complete annealing, thereby obtaining a target flaky carbonyl iron powder coated with an inorganic layer or an organic layer on the surface, wherein the silicon dioxide particles in situ generated on the surface of the target flaky carbonyl iron powder form a highly crystalline and dense silicon dioxide protective layer to protect the carbonyl iron powder.
[0080] The above description is only a specific embodiment of the present invention, so that those skilled in the art can understand or implement the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present invention.
[0081] It should be understood that the present invention is not limited to what has been described above and that various modifications and changes may be made without departing from its scope. The scope of the present invention is limited only by the appended claims.
Claims
1. A coating preparation method for a magnetic metal absorbent, It is characterized in that The steps include: Step 1, pouring a set proportion of carbonyl iron powder, anhydrous ethanol and zirconium oxide balls into a ball mill, and stirring to pre-ball mill the carbonyl iron powder; Step 2, adding the pre-prepared precursor solution into the ball milling tank after the pre-ball milling, stirring and ball milling the carbonyl iron powder, and performing separation treatment after the ball milling to obtain the first flaky carbonyl iron powder with an inorganic layer or an organic layer on the surface and the zirconium oxide ball with the first flaky carbonyl iron powder attached; Step 3, separating the first flaky carbonyl iron powder obtained in step 2 from the zirconium oxide balls attached with the first flaky carbonyl iron powder, and then separating the separated zirconium oxide balls attached with the first flaky carbonyl iron powder again with anhydrous ethanol to obtain zirconium oxide balls and a turbid liquid containing the first flaky carbonyl iron powder and anhydrous ethanol; Step 4, filtering the turbid liquid obtained in step 3 to obtain a second flaky carbonyl iron powder with an inorganic layer or an organic layer coated on the surface; Step 5, placing the first flaky carbonyl iron powder and the second flaky carbonyl iron powder into an oven, and keeping the oven temperature at 50° C. to 80° C. for 8 h to 15 h to obtain a third flaky carbonyl iron powder coated with an inorganic layer or an organic layer; Step 6, sieving the third flaky carbonyl iron powder obtained in step 5, placing the sieved third flaky carbonyl iron powder into a vacuum furnace, heating it to 700°C to 800°C at a set speed, keeping it warm for 2h to 4h, and then annealing it to obtain the target flaky carbonyl iron powder with an inorganic layer or an organic layer coated on the surface.
2. The coating preparation method of the magnetic metal absorber according to claim 1, It is characterized in that In step 1, the mass ratio of the carbonyl iron powder, anhydrous ethanol and zirconium oxide balls is 4-5:2-6:15-25.
3. The coating preparation method of the magnetic metal absorber according to claim 1, It is characterized in that The stirring speed in step 1 is 100 r / min to 150 r / min, and the stirring time is 3 h to 5 h.
4. The coating preparation method of the magnetic metal absorber according to claim 1, It is characterized in that In step 2, the stirring speed is 100 r / min to 150 r / min, and the stirring time is 2 h to 5 h.
5. The coating preparation method of the magnetic metal absorber according to claim 1, It is characterized in that In step 2, the precursor solution includes a first mixed solution and a second mixed solution, and the mass ratio of the first mixed solution to the second mixed solution is 6-10:2-5.
6. The coating preparation method of the magnetic metal absorber according to claim 5, It is characterized in that The first mixed solution is obtained by mixing ammonia water and deionized water in a mass ratio of 6-8:10-13.
7. The coating preparation method of the magnetic metal absorber according to claim 5, It is characterized in that The second mixed liquid is obtained by mixing a silicon source material and anhydrous ethanol in a mass ratio of 1:1 to 8.
8. The coating preparation method of the magnetic metal absorber according to claim 7, It is characterized in that The silicon source material is any one of tetraethyl orthosilicate, tetramethyl orthosilicate, dimethyldiethoxysilane, diphenyldiethoxysilane and (3-aminopropyl)triethoxysilane.
9. The coating preparation method of the magnetic metal absorber according to claim 1, It is characterized in that In step 6, the sieving process uses a sieve with a mesh size of 80 to 200.
10. The coating preparation method of the magnetic metal absorber according to claim 1, It is characterized in that In step 6, the set speed is 5°C / min to 10°C / min.
Citation Information
Cited By
Iron-based magnetic absorbent with corrosion early warning and inhibition functions as well as preparation method and application of iron-based magnetic absorbent