Brazing method for controlling TiAl alloy welding cracks

By using the mixing and preheating treatment of β-phase stabilized element powder and brazing in TiAl alloy brazing, the cooling speed is regulated, and the euthanization structure of hard B2 phase and γ phase is formed in network-like distribution, the TiAl alloy brazing joint is solved. The problem of microcracks is prone to occur, which significantly improves the strength and mechanical properties of the joints.

CN118926642AActive Publication Date: 2024-11-12HARBIN INST OF TECH

Patent Information

Application Number
CN202411316311.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-20
Publication Date
2024-11-12
Estimated Expiration
2044-09-20

AI Technical Summary

Technical Problem

TiAl alloys are prone to microcracks during brazing, resulting in a decrease in joint strength. The prior art cannot effectively suppress cracks, and the increase in brazing time will lead to a thick layer of the base material structure, affecting the quality of the joint.

Method used

By mixing the brazing powder with the β-phase stabilized element powder, preheating and cooling speed are performed, the generation of microcracks during the welding of TiAl alloy is controlled, and the β-phase stabilized element is used to expand the β-phase zone during the cooling process and reduce α+ The γ region forms a network-like euthanized structure of hard B2 phase and γ phase, which is distributed, to improve the joint strength.

Benefits of technology

It effectively suppresses the occurrence of microcracks in TiAl alloy welding, improves the strength of the joint, and the average shear strength reaches ≥350MPa, forming an ideal euthanized structure of layered sheet γ-phase structure and hard B2 phase, enhancing the mechanical properties of the joint .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118926642A_ABST
    Figure CN118926642A_ABST
Patent Text Reader

Abstract

The invention discloses a brazing method for controlling TiAl alloy welding cracks, and belongs to the field of brazing. The method aims at solving the problem that an existing TiAl brazed joint is prone to generating microcracks, and consequently the strength of the joint is reduced. The preparation method comprises the following steps: 1, mixing brazing filler metal powder with beta-phase stable element powder; 2, pressurizing to obtain a brazing filler metal foil; and 3, brazing. The method is used for controlling the TiAl alloy welding cracks.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of brazing. Background Art

[0002] The density of TiAl intermetallic compounds is only half of that of nickel-based high-temperature alloys, and they have excellent mechanical properties, which have considerable application prospects in the aerospace field. However, they are brittle at room temperature, difficult to process and form, and difficult to process into integral components. Processing composite components will inevitably involve the connection problem of TiAl alloys.

[0003] At present, the connection methods of TiAl alloy include fusion welding, brazing and friction welding. Among them, fusion welding is very easy to produce microcracks due to the brittleness of TiAl alloy itself and the thermal stress caused by rapid cooling after welding, which affects the performance; friction welding has great restrictions on the connection form and specimen size of the parent material, and is not suitable for joints with complex structures; with brazing connection, as the brazing time increases, the parent material structure on both sides of the joint will become coarse, which is easy to cause microcracks. Therefore, it is urgent to develop a welding method that can effectively suppress microcracks in TiAl brazed joints and thereby improve the strength of the joint. Summary of the invention

[0004] The present invention aims to solve the problem that micro cracks are easily generated in existing TiAl brazed joints, resulting in reduced joint strength, and further provide a brazing method for controlling TiAl alloy welding cracks.

[0005] A brazing method for controlling welding cracks of TiAl alloy is carried out according to the following steps:

[0006] 1. Evenly mix the solder powder and the β-phase stabilizing element powder to obtain a mixed solder;

[0007] The mass percentage of the β-phase stabilizing element powder in the mixed solder is 10% to 20%;

[0008] 2. Pressurizing the mixed solder to obtain solder foil;

[0009] 3. Stack the TiAl base material, brazing foil and TiAl base material in order to obtain a component to be welded, put the component to be welded into a vacuum brazing furnace and evacuate it, then preheat it at 300℃~500℃ for 0.5h~1.5h, and then keep it at the brazing temperature. After keeping it, first cool it to 800℃~900℃ at a rate of 5℃ / min~10℃ / min, then cool it to 200℃~400℃ at a rate of 3℃ / min~5℃ / min, and finally cool it to room temperature with the furnace, take out the sample, and complete the brazing method for controlling TiAl alloy welding cracks.

[0010] The beneficial effects of the present invention are:

[0011] 1. The present invention uses three methods, namely, preheating treatment before welding, design of solder composition and control of cooling rate, to couple and control the generation of microcracks in the welding process of TiAl intermetallic compounds. Preheating before welding can effectively release the residual stress in the forming process of TiAl alloy, and can also help reduce the cooling rate after welding.

[0012] Second, during the brazing process, the present invention utilizes β-phase stabilizing elements to expand the β-phase region and shrink the α+γ region during the cooling process, and then cools down to the eutectoid reaction temperature at a faster cooling rate, so that the β-phase cannot be completely transformed. Since the high-temperature β-phase is orderly transformed into the B2 phase during the cooling process, the remaining β-phase will eventually lead to the presence of part of the B in the brazing seam. 2 Mutually;

[0013] 3. After the brazing insulation process is completed, at the eutectoid reaction temperature, the present invention forms an ideal lamellar γ phase structure by reducing the cooling rate; finally, a network-like distribution of an appropriate amount of hard B2 phase and γ phase eutectoid structure is formed at the joint, and the pinning effect of the B2 phase is used to improve the strength of the joint. The TiAl alloy parts connected by this method have an average shear strength of ≥350MPa.

[0014] Instruction Manual

[0015] Figure 1 This is the brazing process curve of step 3 of embodiment 1;

[0016] Figure 2 This is a scanning electron microscope image of the joint interface structure of the TiAl alloy welded piece prepared in Example 1. DETAILED DESCRIPTION

[0017] Specific implementation method 1: This implementation method is a brazing method for controlling TiAl alloy welding cracks, which is carried out according to the following steps:

[0018] 1. Evenly mix the solder powder and the β-phase stabilizing element powder to obtain a mixed solder;

[0019] The mass percentage of the β-phase stabilizing element powder in the mixed solder is 10% to 20%;

[0020] 2. Pressurizing the mixed solder to obtain solder foil;

[0021] 3. Stack the TiAl base material, brazing foil and TiAl base material in order to obtain a component to be welded, put the component to be welded into a vacuum brazing furnace and evacuate it, then preheat it at 300℃~500℃ for 0.5h~1.5h, and then keep it at the brazing temperature. After keeping it, first cool it to 800℃~900℃ at a rate of 5℃ / min~10℃ / min, then cool it to 200℃~400℃ at a rate of 3℃ / min~5℃ / min, and finally cool it to room temperature with the furnace, take out the sample, and complete the brazing method for controlling TiAl alloy welding cracks.

[0022] The beneficial effects of this embodiment are:

[0023] 1. In this embodiment, three methods, namely, preheating treatment before welding, design of solder composition and control of cooling rate, are used to couple and control the generation of microcracks in the welding process of TiAl intermetallic compounds. Preheating before welding can effectively release the residual stress in the forming process of TiAl alloy, and can also help reduce the cooling rate after welding.

[0024] 2. During the brazing process, this embodiment utilizes β-phase stabilizing elements to expand the β-phase region and shrink the α+γ region during the cooling process, and then cools down to the eutectoid reaction temperature at a faster cooling rate, so that the β-phase cannot be completely transformed. Since the high-temperature β-phase is orderly transformed into the B2 phase during the cooling process, the remaining β-phase will eventually lead to the presence of some B in the brazing seam. 2 Mutually;

[0025] 3. After the brazing insulation process is completed, at the eutectoid reaction temperature, the present embodiment forms an ideal lamellar γ phase structure by reducing the cooling rate; ultimately, a network-like distribution of an appropriate amount of hard B2 phase and γ phase eutectoid structure is formed at the joint, and the pinning effect of the B2 phase is used to improve the strength of the joint. The TiAl alloy parts connected by this method have an average shear strength of ≥350MPa.

[0026] Specific embodiment 2: This embodiment is different from specific embodiment 1 in that the solder powder in step 1 is AgCuTi powder, AgCuInTi powder, TiZrNiCu powder, TiNi powder, BNi2 powder or BNi5 powder. The rest is the same as specific embodiment 1.

[0027] Specific implementation method 3: This implementation method is different from specific implementation method 1 or 2 in that the β-phase stabilizing element powder in step 1 is Mo powder, Nb powder, W powder, V powder or Cr powder. The rest is the same as specific implementation method 1 or 2.

[0028] Specific embodiment 4: This embodiment differs from specific embodiments 1 to 3 in that: in step 2, the mixed solder is pressurized under a pressure of 0.5t to 2t. The rest is the same as specific embodiments 1 to 3.

[0029] Specific embodiment 5: This embodiment is different from specific embodiments 1 to 4 in that the thickness of the solder foil in step 2 is 0.5 mm to 2 mm. The rest is the same as specific embodiments 1 to 4.

[0030] Specific embodiment 6: This embodiment is different from specific embodiments 1 to 5 in that the TiAl base material in step 3 is Ti-48Al, Ti-42Al-5V, Ti-45Al-8.5Nb-0.2W-0.03Y or Ti-48Al-2Cr-2Nb. The rest is the same as specific embodiments 1 to 5.

[0031] Specific embodiment 7: This embodiment differs from the specific embodiments 1 to 6 in that: in step 3, the component to be welded is placed in a vacuum brazing furnace and evacuated to 5×10 -3 Pa or less. The rest is the same as the first to sixth embodiments.

[0032] Specific embodiment 8: This embodiment differs from specific embodiments 1 to 7 in that: in step 3, the temperature is heated to 300°C to 500°C at a rate of 2°C / min to 10°C / min, and preheated for 0.5h to 1.5h at a temperature of 300°C to 500°C. Other aspects are the same as specific embodiments 1 to 7.

[0033] Specific embodiment 9: This embodiment differs from specific embodiments 1 to 8 in that: in step 3, heating is performed at a rate of 5°C / min to 10°C / min to the brazing temperature, and the temperature is kept at the brazing temperature for 10 to 20 minutes. The rest is the same as specific embodiments 1 to 8.

[0034] Specific embodiment 10: This embodiment differs from specific embodiments 1 to 9 in that: in step 3, the temperature is first heated to 400°C to 500°C at a rate of 5°C / min to 10°C / min, and preheated at 400°C to 500°C for 1h to 1.5h; in step 3, the temperature is first cooled to 850°C to 900°C at a rate of 8°C / min to 10°C / min, and then cooled to 200°C to 300°C at a rate of 4°C / min to 5°C / min. The rest is the same as specific embodiments 1 to 9.

[0035] The following examples are used to verify the beneficial effects of the present invention:

[0036] Embodiment 1, combined with Figure 1 Specific instructions:

[0037] A brazing method for controlling welding cracks of TiAl alloy is carried out according to the following steps:

[0038] 1. Evenly mix the solder powder and the β-phase stabilizing element powder to obtain a mixed solder;

[0039] The mass percentage of the β-phase stabilizing element powder in the mixed solder is 20%;

[0040] 2. Pressurize the mixed solder under a pressure of 1t to obtain solder foil;

[0041] The thickness of the solder foil is 1 mm;

[0042] 3. Stack the TiAl base material, brazing material foil and TiAl base material in order to obtain the component to be welded. Put the component to be welded into a vacuum brazing furnace and evacuate to 5×10 -3 Pa, then heated to 400°C at a rate of 10°C / min, and preheated at 400°C for 1h, then heated to 1200°C at a rate of 10°C / min, and kept warm for 10min under the condition of brazing temperature of 1200°C, after keeping warm, first cooled to 900°C at a rate of 10°C / min, and then cooled to 200°C at a rate of 5°C / min, finally cooled to room temperature with the furnace, took out the sample, and obtained the TiAl alloy weldment.

[0043] The solder powder described in step 1 is Ti-28Ni powder.

[0044] The β-phase stabilizing element powder described in step 1 is Nb powder.

[0045] The TiAl base material described in step 3 is Ti-42Al-5V.

[0046] Figure 2 This is a scanning electron microscope image of the joint interface structure of the TiAl alloy welded piece prepared in Example 1. As can be seen from the figure, the joint of the TiAl alloy welded piece is good, without obvious microcracks and other defects, the grains are fine, the grain size is about 5μm, and it can be seen that the joint structure is a lamellar γ phase and a lamellar B phase. 2 The dual-phase structure of the phase is cross-distributed with each other to form a network-like distribution of an appropriate amount of hard B2 phase and γ phase eutectic structure, which improves the strength of the joint through grain boundary strengthening and second phase strengthening, and utilizes the pinning effect of the B2 phase.

[0047] The room temperature shear strength of TiAl alloy welded parts was tested according to the national standard GB / T 11363-2008, and the room temperature shear strength was measured to be 350 MPa.

Claims

1. A brazing method for controlling welding cracks of TiAl alloy, characterized in that It is carried out in the following steps:

1. Evenly mix the solder powder and the β-phase stabilizing element powder to obtain a mixed solder; The mass percentage of the β-phase stabilizing element powder in the mixed solder is 10% to 20%; 2. Pressurizing the mixed solder to obtain solder foil; 3. Stack the TiAl base material, brazing foil and TiAl base material in order to obtain a component to be welded, put the component to be welded into a vacuum brazing furnace and evacuate it, then preheat it at 300℃~500℃ for 0.5h~1.5h, and then keep it at the brazing temperature. After keeping it, first cool it to 800℃~900℃ at a rate of 5℃ / min~10℃ / min, then cool it to 200℃~400℃ at a rate of 3℃ / min~5℃ / min, and finally cool it to room temperature with the furnace, take out the sample, and complete the brazing method for controlling TiAl alloy welding cracks.

2. A brazing method for controlling welding cracks of TiAl alloy according to claim 1, characterized in that The solder powder described in step 1 is AgCuTi powder, AgCuInTi powder, TiZrNiCu powder, TiNi powder, BNi2 powder or BNi5 powder.

3. A brazing method for controlling welding cracks of TiAl alloy according to claim 1, characterized in that The β-phase stabilizing element powder described in step 1 is Mo powder, Nb powder, W powder, V powder or Cr powder.

4. A brazing method for controlling welding cracks of TiAl alloy according to claim 1, characterized in that In step 2, the mixed solder is pressurized at a pressure of 0.5t to 2t.

5. A brazing method for controlling welding cracks of TiAl alloy according to claim 1, characterized in that The thickness of the solder foil described in step 2 is 0.5 mm to 2 mm.

6. A brazing method for controlling welding cracks of TiAl alloy according to claim 1, characterized in that The TiAl base material described in step 3 is Ti-48Al, Ti-42Al-5V, Ti-45Al-8.5Nb-0.2W-0.03Y or Ti-48Al-2Cr-2Nb.

7. A brazing method for controlling welding cracks of TiAl alloy according to claim 1, characterized in that In step 3, the components to be welded are placed in a vacuum brazing furnace and vacuumed to 5×10 -3 Below Pa.

8. A brazing method for controlling welding cracks of TiAl alloy according to claim 1, characterized in that In step 3, the temperature is heated to 300°C to 500°C at a rate of 2°C / min to 10°C / min, and preheated at 300°C to 500°C for 0.5h to 1.5h.

9. A brazing method for controlling welding cracks of TiAl alloy according to claim 1, characterized in that In step 3, the process is heated to the brazing temperature at a rate of 5°C / min to 10°C / min, and kept at the brazing temperature for 10 to 20 minutes.

10. A brazing method for controlling welding cracks of TiAl alloy according to claim 1, characterized in that In step three, first heat to 400°C ~ 500°C at a rate of 5°C / min ~ 10°C / min, and preheat at 400°C ~ 500°C for 1h ~ 1.5h; in step three, first cool to 850°C ~ 900°C at a rate of 8°C / min ~ 10°C / min, and then cool to 200°C ~ 300°C at a rate of 4°C / min ~ 5°C / min.

Citation Information

Patent Citations

  • TiNiNbZr high-temperature filler for TiAl alloy and preparing method and brazing method thereof

    CN110605498A

  • Medium-temperature Ti-based brazing filler metal for same or different material brazing of Ti2AlNb-based alloy and preparation method and brazing process thereof

    CN111702278A

  • Solder for K418B high-temperature alloy guider casting defects and repair welding method

    CN112453754A

  • Brazing filler metal for repairing Ni3Al-based single crystal alloy turbine guide blade and preparation method of brazing filler metal

    CN115647651A

  • Low-temperature brazing method for NiTi shape memory alloy and 316L stainless steel

    CN115846788A

Cited By

  • High-strength and high-toughness brazing method for Ti65 high-temperature titanium alloy