Bare board door ring and production method thereof

By using a bare-plate door ring production method, the problems of toughness and hydrogen embrittlement risk of coated plates in high-strength door rings have been solved, achieving the requirements of strength and lightweight while reducing production costs.

CN118926694APending Publication Date: 2024-11-12CHONGQING ZHIXIN IND CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411192567.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In the production of high-strength door rings, coated plates in the existing technology suffer from problems such as reduced toughness, increased risk of hydrogen embrittlement, and high production costs, making it difficult to meet the requirements of strength and lightweight.

Method used

Bare plates are used instead of coated plates. By setting a thickness of ≥1.2mm in key locations and controlling the oxygen content to ≤2% during heating, liquid nitrogen protective gas is used to reduce the oxide layer. Combined with shot blasting to remove the oxide layer, bare plate door rings are produced.

Benefits of technology

The strength and toughness of the door ring have been improved, the risk of hydrogen embrittlement has been reduced, and lightweighting and cost reduction have been achieved, resulting in an increase in production efficiency of approximately 20-50%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118926694A_ABST
    Figure CN118926694A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of door ring production, and discloses a bare board door ring and a production method thereof.The high-strength door ring is produced by replacing a coating plate with a bare board, and the production method comprises the following steps that 1, according to the performance requirement of the door ring, the strength position of the door ring is determined, and the strength position serves as the key position of a bare board material piece; 2, the material thickness of the key position of the bare board material sheet is set to be larger than or equal to 1.2 mm; the bare board material pieces are tailored and welded into an annular structure corresponding to the door ring through laser; 3, putting the annular bare board into a heating furnace for heating treatment, and controlling the oxygen content in the furnace to be less than or equal to 2%; and 4, after hot stamping of the bare board, shot blasting removal is carried out on the oxide layer on the surface of the bare board, and the bare board door ring is manufactured. The bare plate is adopted to directly replace a coating plate to produce the door ring, the overall weight is reduced, the hydrogen embrittlement risk is reduced, the deformation amount is reduced, the door ring strength is improved, and meanwhile the production cost is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of vehicle door knocker production, and in particular to a bare plate door knocker and a production method thereof. Background Art

[0002] In the current door knocker production technology, coated plates are widely used in the field of door knocker manufacturing due to their excellent corrosion resistance, wear resistance and decorative properties, which significantly improves the overall performance of the product. However, despite the excellent performance of coated plates, their production costs are relatively high, which is mainly due to the complexity of the coating process and the procurement cost of the required high-quality raw materials.

[0003] In addition, as the market's requirements for door knocker strength and lightness continue to increase, especially when it is necessary to produce high-strength door knockers with a strength of 1500 MPa or above, the risk of hydrogen embrittlement of coated plates will increase significantly under high-strength hot forming. And as the strength of the material increases, its toughness tends to decrease accordingly. This phenomenon is particularly obvious in high-strength coated plates, resulting in poor toughness under high-strength hot forming, and more prone to cracking and other problems, affecting the overall performance of the door knocker.

[0004] In order to deal with the problems of reduced toughness and increased risk of hydrogen embrittlement in high-strength coated plates, the only way is to increase the thickness of the coated plates on the basis of low-strength coated plates. However, although this approach can improve the strength and crack resistance of the door knocker to a certain extent, it also brings about the problem of increased weight, making it difficult to meet the lightweight requirements. In addition, the increase in thickness not only makes the door knocker more complicated in design and installation, but also increases the consumption of raw materials and the difficulty of processing, further pushing up production costs. Summary of the invention

[0005] The present invention aims to provide a bare plate door knocker and a production method thereof, wherein bare plates are used directly to replace coated plates for the production of door knockers, thereby improving the toughness of door knocker plates under high strength, reducing the risk of cracking and hydrogen embrittlement, while improving the strength of the door knocker and effectively reducing the weight of the door knocker, thereby achieving the requirements of both strength and lightness, and effectively reducing the production difficulty, shortening the production cycle, and reducing production costs.

[0006] To achieve the above object, the present invention adopts the following technical scheme: a method for producing a bare plate door knocker, using a bare plate instead of a coated plate to produce a high-strength door knocker, comprising the following steps:

[0007] Step 1: determine the door knocker strength position according to the door knocker strength performance requirements, and use the strength position as the key position of the bare plate sheet;

[0008] Step 2, setting the material thickness of the key position of the bare sheet to be ≥1.2 mm; laser welding the bare sheet into a ring structure corresponding to the door ring;

[0009] Step 3, placing the annular bare plate into a heating furnace for heating treatment, and controlling the oxygen content in the furnace to be ≤2%;

[0010] Step 4: After the bare plate is hot stamped, the oxide layer on the surface of the bare plate is removed by shot blasting to form a bare plate door ring.

[0011] Furthermore, the bare plate sheet includes key positions and other positions, and the thickness of the other positions of the bare plate sheet is ≥0.8 mm.

[0012] Furthermore, the key positions are divided according to the door knocker performance requirements, which include strength requirements, size requirements and stability requirements.

[0013] Furthermore, in step 2, the bare sheet material is laser welded by autogenous welding.

[0014] Furthermore, in step 3, the heating temperature of the annular bare plate is 800° C.-970° C., and dry liquid nitrogen protective gas is filled into the furnace during heating to control the oxygen content.

[0015] Furthermore, during the heating process, liquid nitrogen protective gas is dynamically inflated according to the oxygen content detected in the furnace until the heating is completed.

[0016] Furthermore, the nitrogen content in the liquid nitrogen protective gas is greater than 99%, so as to ensure that the nitrogen content meets the demand and reaches the requirement of controlling the oxygen content.

[0017] Furthermore, in step 4, it also includes laser cutting the bare plate door ring after hot forming.

[0018] At the same time, the present invention also provides a bare plate door knocker, which is a bare plate door knocker produced by applying the above-mentioned bare plate door knocker production method.

[0019] The principles and advantages of this solution are:

[0020] Traditional door knocker production generally uses coated plates instead of bare plates. The reason is that technicians in this field believe that coated plates have higher corrosion resistance and wear resistance, and their performance will be better. However, bare plates are more easily oxidized on the surface, so the oxide layer of the bare plates needs to be shot blasted to remove the oxide layer. During the shot blasting process, it is easy to cause the bare plates to deform. Since the position of the oxide layer is not controllable, the deformation during the shot blasting process is also difficult to control, thus affecting the overall performance of the door knocker. Since coated plates have a layer of coating protection on the surface, they do not need to be shot blasted, and there is no risk of deformation. Therefore, there is a technical prejudice that coated plates must be used.

[0021] Even in the prior art, there is a method of using bare plates for door knocker production, which is used in combination with coated plates in a local or small size range, and the coated plates are mainly used as the main material for production. This can avoid the deformation caused by the shot blasting process, and the performance requirements of the door knocker are ensured by the performance of the coated plates. Therefore, it is still believed that bare plate materials cannot be directly used in the production of door knockers.

[0022] In the prior art, since bare plates are prone to deformation during shot blasting, bare plates are generally used for the production of small-sized parts, and the material thickness is 1.2mm to reduce the deformation of bare plates during shot blasting, but it is difficult to use in the manufacture of large-sized parts such as door knockers. However, this solution sets the strength position corresponding to the door knocker as the key position of the bare plate, and sets its thickness to more than 1.2mm to improve the strength of the key position of the bare plate. At the same time, during the heating process, dry liquid nitrogen protective gas is filled to control the oxygen content in the furnace to ≤2%. When the size increases, the oxygen content in the furnace is effectively reduced, thereby reducing the range of the oxide layer on the surface of the bare plate, thereby reducing the shot blasting process and shot blasting intensity, further reducing the risk of deformation, and enabling the bare plate to replace the coated plate and be directly used in the production of door knockers.

[0023] In addition, since there is no coating on the surface of the bare plate, its hydrogen embrittlement risk is lower than that of the coated plate, and its toughness is higher, which can better meet the production needs of high-strength door rings, thereby improving the strength of the door ring and achieving the requirements of strength and lightweight. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 The present invention is a schematic flow chart of a method for producing a bare plate door knocker. DETAILED DESCRIPTION

[0025] The following is further described in detail through specific implementation methods:

[0026] Embodiment 1

[0027] A bare plate door ring production method in the present embodiment controls the oxygen content in the heating furnace, reduces the area of ​​the bare plate oxide layer, reduces the shot blasting intensity, and at the same time increases the material thickness at key positions of the bare plate to reduce the risk of deformation, so that the bare plate door ring production can achieve the required size and performance. It can directly replace the coated plate to produce door rings, effectively improve the door ring strength, meet the high-strength door ring production requirements, and at the same time ensure the lightweight requirements of the door ring and reduce the overall production cost.

[0028] Details are as attached Figure 1 As shown, the production method comprises the following steps:

[0029] S1, according to the door ring performance requirements, determine the door ring strength position, take the strength position as the key position of the bare plate sheet, and make the bare plate sheet include the key position and other positions.

[0030] In this embodiment, the key positions are divided according to the door knocker performance requirements, where the performance requirements include strength (mechanical properties) requirements, which need to meet design requirements, size requirements and stability requirements, and which need to meet production design requirements. The key positions are determined in this way, and other positions except the key positions are the remaining positions.

[0031] S2, set the material thickness of the key position of the bare sheet material to ≥1.2mm to reduce the risk of deformation of the bare sheet material during the shot blasting process and reduce the weight of the sheet; the material thickness of the remaining positions of the bare sheet material is ≥0.8mm. By adopting the method of local thickening, the weight of the bare sheet is reduced as much as possible, the lightweight requirements are improved, and the strength of the door ring is guaranteed.

[0032] After the bare sheet material is made according to the set material thickness, the bare sheet material is laser welded into an annular structure corresponding to the door ring to form an annular bare sheet. In this embodiment, the bare sheet material is laser welded by self-melting welding to reduce the loss of material splicing, reduce the use of consumables, avoid material waste, and ensure the strength of the welded joint. Among them, welding can be done in two ways: with or without wire filling, and performance verification is performed after welding to ensure that the parts meet the technical requirements after welding.

[0033] S3, placing the annular bare board into a heating furnace for heating treatment, and controlling the oxygen content in the furnace to be ≤2%. In this embodiment, the heating temperature of the annular bare board is set to 800°C-970°C. Specifically, if a box-type heating furnace is used, the heating temperature is controlled to be 900°C-970°C; if a roller bottom heating furnace is used, the heating temperature is controlled to be 800°C-970°C.

[0034] During heating, dry liquid nitrogen protective gas is continuously charged into the furnace to control the oxygen content in the heating furnace. In this embodiment, the liquid nitrogen protective gas is a gas with a nitrogen content greater than 99%. During the heating process, the liquid nitrogen protective gas is dynamically inflated according to the oxygen content detected in the furnace. In this embodiment, the gas is inflated according to the oxygen content detected in the heating furnace. The maximum gas filling volume is dynamically defined according to the size of the furnace door and the production rhythm until the heating is completed to ensure that the oxygen content in the heating furnace is ≤2%, reduce the formation of the oxide layer on the surface of the bare board, and then effectively reduce the shot blasting intensity and shot blasting time, reduce the deformation of the bare board during the shot blasting process, control the deformation of the bare board, and effectively reduce the dew point below -10°C to avoid the risk of hydrogen embrittlement and ensure that the bare board meets the door ring strength production requirements.

[0035] S4, after the bare plate is hot stamped, the oxide layer on the surface of the bare plate is shot blasted to remove it, so as to form a bare plate door ring.

[0036] In this embodiment, after heating is completed, the bare plate door ring is hot stamped, and the material of the stamping die insert and the corresponding surface treatment are strengthened. Specifically, the surface strengthening treatment can be performed by surface hardening methods such as plasma nitriding and laser cladding. After hot forming, the bare plate door ring is laser cut according to the door ring size to improve production efficiency while ensuring the stability of part size. Then, the bare plate door ring is subjected to oxide scale removal processes such as shot blasting, which effectively reduces the oxygen content to reduce the oxide layer while increasing the thickness of the bare plate material, thereby ensuring that the deformation of the part is minimized during the shot blasting process, and at the same time effectively removes the oxide layer to ensure that the bare plate can be directly used in the production of the door ring.

[0037] At the same time, in this embodiment, a bare plate door knocker is also provided. The bare plate door knocker produced by the above-mentioned bare plate door knocker production method effectively improves the door knocker strength while greatly reducing the production cost.

[0038] Since the coated plate has the properties of corrosion resistance and wear resistance, in order to ensure the strength and performance of the door knocker, the prior art generally uses the coated plate as the production material of the door knocker, and does not consider directly using the bare plate for production. This is because, in the prior art, since the coated plate has a layer of coating on the surface, it does not need to undergo processes such as shot blasting to remove the surface oxide layer, thereby not causing deformation and other problems, in order to ensure the strength and performance of the coated plate door knocker. And because the shot blasting process is uncontrollable, the deformation produced during the shot blasting process is also uncontrollable, and further processing is required after deformation, which increases the process and affects the overall performance of the sheet. Therefore, even if bare plate production is used, it is only used in the production of small-sized or local parts to reduce the impact of deformation. As a result, there is a technical prejudice that bare plates cannot be directly used in large-sized production such as door knockers.

[0039] However, the demand for door knockers' strength and lightness is increasing. When faced with the production demand for high-strength door knockers (above 1500 MPa), the coated plate has poor toughness under high-strength hot forming and is more prone to cracking. In addition, there is a layer of coating on the surface of the coated plate, which makes it difficult for the hydrogen atoms inside to be discharged, increasing the risk of hydrogen embrittlement. As a result, it is difficult to meet the strength requirements when high-strength door knockers are made of coated plates. Therefore, only low-strength coated plates can be used for production. However, in order to ensure the improvement of strength, the only way is to increase the thickness of the coated plate, which in turn brings about the problem of increased weight and is difficult to meet the demand for lightweight.

[0040] In this embodiment, by overcoming technical prejudice, bare plates are used instead of coated plates to directly produce door knockers. According to the strength position of the door knocker, the key position of the bare plate is delineated, and the material thickness of the key position is set to be greater than or equal to 1.2 mm to ensure the strength requirements of the key positions of the bare plate and effectively reduce the weight. At the same time, during heating, by filling with liquid nitrogen protective gas, the oxygen content is controlled to be less than 2%, and the formation of the oxide layer on the surface of the bare plate is reduced, thereby reducing the shot blasting intensity and shot blasting time, ensuring the minimum deformation of the parts, and removing the oxide layer at the same time. Since the bare plate has no coating on the surface, the hydrogen atoms inside it are easier to be discharged, thereby reducing the risk of hydrogen embrittlement of the bare plate, and the toughness of the bare plate at high strength is higher than that of the coated plate, thereby effectively improving the strength of the door knocker and meeting the production requirements of high-strength door knockers.

[0041] By directly using bare plates to replace coated plates to produce door knockers, the strength of the door knockers is improved, and while production needs and performance requirements are met, the production cost is effectively reduced by about 20% to 50%.

[0042] The above is only an embodiment of the present invention, and the common knowledge such as the known specific technical solutions and / or characteristics in the solution is not described in detail here. It should be pointed out that for those skilled in the art, without departing from the technical solution of the present invention, several modifications and improvements can be made, which should also be regarded as the protection scope of the present invention, and these will not affect the effect of the implementation of the present invention and the practicality of the patent. The scope of protection required by this application shall be based on the content of its claims, and the specific implementation methods and other records in the specification can be used to interpret the content of the claims.

Claims

1. A method for producing a bare plate door knocker, characterized in that: The production of high-strength door knockers using bare plates instead of coated plates includes the following steps: Step 1: determine the door ring strength position according to the door ring performance requirements, and use the strength position as the key position of the bare plate sheet; Step 2, setting the material thickness of the key position of the bare sheet to be ≥1.2 mm; laser welding the bare sheet into a ring structure corresponding to the door ring; Step 3, placing the annular bare plate into a heating furnace for heating treatment, and controlling the oxygen content in the furnace to be ≤2%; Step 4: After the bare plate is hot stamped, the oxide layer on the surface of the bare plate is removed by shot blasting to form a bare plate door ring.

2. A method for producing a bare plate door knocker according to claim 1, characterized in that: The bare plate sheet includes key positions and other positions, and the thickness of the other positions of the bare plate sheet is ≥0.8 mm.

3. The method for producing a bare plate door knocker according to claim 1, characterized in that: The key positions are divided according to the door knocker performance requirements, which include strength requirements, size requirements and stability requirements.

4. The method for producing a bare plate door knocker according to claim 1, characterized in that: In step 2, the bare sheet material is laser welded by autogenous welding.

5. The method for producing a bare plate door knocker according to claim 1, characterized in that: In step 3, the heating temperature of the annular bare plate is 800° C.-970° C., and dry liquid nitrogen protective gas is filled into the furnace during heating to control the oxygen content.

6. A method for producing a bare plate door knocker according to claim 5, characterized in that: During the heating process, liquid nitrogen protective gas is dynamically inflated according to the oxygen content detected in the furnace until the heating is completed.

7. The method for producing a bare plate door knocker according to claim 5, characterized in that: The nitrogen content in the liquid nitrogen protective gas is greater than 99%.

8. The method for producing a bare plate door knocker according to claim 1, characterized in that: In step 4, laser cutting of the bare plate door ring is also included after the thermoforming.

9. A bare plate door knocker, characterized in that: A bare plate door knocker produced by a bare plate door knocker production method as described in any one of claims 1 to 8.