Manufacturing method of high-strength concrete for concrete pole manufacturing
By detecting environmental parameters, building a strength model and optimizing the group distribution ratio, the problem of insufficient strength and durability of traditional concrete poles in high load and harsh environments is solved, and efficient hardness improvement and cost control are achieved, which is suitable for infrastructure construction.
Patent Information
- Application Number
- CN202411216138.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-02
- Publication Date
- 2024-11-12
AI Technical Summary
Traditional concrete poles have problems such as low strength, poor crack resistance and insufficient durability in high load and harsh environments. The existing technology cannot accurately quantify the required hardness and blindly increasing the hardness will lead to cost waste.
By installing sensors to detect the external environmental parameters of the cement pole arrangement site, a concrete strength index model is constructed, the assembly distribution ratio of the foundation material is optimized, and vibration forming and specific curing processes are adopted to improve the strength and durability of concrete.
It has achieved accurate improvement in the strength and durability of concrete, better adaptability and better cost control, and is suitable for infrastructure construction such as power transmission and communications.
Smart Images

Figure CN118927376A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of concrete manufacturing, and in particular to a method for manufacturing high-strength concrete for manufacturing cement poles. Background Art
[0002] As an indispensable component of infrastructure such as electricity and communications, the demand for cement poles is increasing year by year.
[0003] However, traditional concrete poles have problems such as low strength, poor crack resistance, and insufficient durability, which limit their application in high-load and harsh environments. Specifically:
[0004] 1. Low strength: The strength of traditional concrete poles usually depends on the mix ratio of concrete and the curing conditions after pouring. If the concrete mix ratio is unreasonable or the curing is improper, the strength of the pole may not meet the design requirements, which will cause the pole to deform or be damaged when subjected to external loads.
[0005] 2. Poor crack resistance: Concrete poles may shrink during the hardening process. If the shrinkage is restrained, stress will be generated, which will lead to cracks. In addition, the drying shrinkage and temperature changes of concrete will also cause cracks. These cracks not only affect the appearance of the poles, but also may become channels for corrosive substances, reducing the durability of the poles.
[0006] 3. Insufficient durability: Traditional concrete poles are easily damaged in harsh environments (such as acidic or alkaline soils, or extreme temperature changes). The presence of cracks accelerates the corrosion process, resulting in a shortened life of the poles. In addition, the concrete itself may also be corroded due to chemical reactions or microbial activity.
[0007] Therefore, among the many existing technologies, hardness is mostly achieved by improving the raw material ratio, production process and construction process. However, the existing hardness realization methods are all broadly considered and have not been adaptively improved for specific environmental conditions. On the one hand, the required hardness cannot be accurately quantified and the accuracy is insufficient. On the other hand, blindly increasing the hardness will lead to a waste of cost. Summary of the invention
[0008] The purpose of this section is to summarize some aspects of embodiments of the present invention and briefly introduce some preferred embodiments. Some simplifications or omissions may be made in this section and the specification abstract and the invention title of this application to avoid blurring the purpose of this section, the specification abstract and the invention title, and such simplifications or omissions cannot be used to limit the scope of the present invention.
[0009] In view of the problems existing in the above-mentioned existing pole concrete preparation process, the present invention is proposed.
[0010] Therefore, the technical problem solved by the present invention is to solve the problem that the existing preparation process of electric pole concrete has no adaptability improvement according to specific environmental conditions.
[0011] To solve the above technical problems, the present invention provides the following technical solutions: A method for making high-strength concrete for cement pole manufacturing, comprising the following steps: S1: installing a group of sensors at the cement pole arrangement site to detect the external environmental parameters of the current cement site; S2: constructing a concrete strength index model based on the detected external environmental parameters, and outputting the strength index value corresponding to the current site; S3: preparing various base materials for concrete, and performing component proportioning of each base material based on the strength index value; S4: stirring and mixing the various base materials with good proportions and pouring them into a mold, and vibrating and forming them for 2 minutes; S5: the formed concrete pole is left to stand for curing at room temperature for 24 hours, and then watered for curing, and the curing time is at least 7 days; S6: after the curing is completed, the concrete pole is demolded for subsequent finished product processing.
[0012] As a preferred scheme of the method for making high-strength concrete for cement pole manufacturing described in the present invention, the detected external environmental parameters specifically include: ambient humidity, ambient temperature, water content of the soil under the current collection environment, porosity of the soil under the current collection environment and soil pH value; wherein the collected ambient humidity specifically includes: annual average humidity, %RH, annual maximum humidity, %RH and annual minimum humidity, %RH; wherein the collected ambient temperature specifically includes: annual average temperature, ℃, annual maximum temperature, ℃ and annual minimum temperature, ℃; wherein the collected soil pH value specifically includes: annual average pH value, annual maximum pH value and annual minimum pH value.
[0013] As a preferred solution of the method for producing high-strength concrete for cement pole manufacturing according to the present invention, the concrete strength index model constructed is specifically:
[0014]
[0015] Among them, δ is the strength index value; S 均 is the annual average humidity, %RH; S 小 is the annual minimum humidity, %RH; S 大 is the annual maximum humidity, %RH; T 均 is the annual average temperature, °C; T 小 is the annual minimum temperature, °C; T 大 is the annual maximum temperature, ℃; α is the soil moisture content under the current collection environment, %; β is the soil porosity under the current collection environment, %; H 均 is the annual average pH value; H 小 is the annual minimum pH value; H 大is the annual maximum pH value; 1.654, 2.003, 0.87, 0.9103 and 0.39 are adjustment constants; dx is the integral operation and the integral constant is 0.
[0016] As a preferred embodiment of the method for producing high-strength concrete for cement pole manufacturing described in the present invention, the basic materials of the concrete specifically include cement, fine aggregate, coarse aggregate, mineral admixture, high-efficiency water reducing agent and water; the cement is ordinary Portland cement; the fine aggregate is river sand or mountain sand, and the fineness modulus is between 2.6 and 3.0; the coarse aggregate is crushed stone or pebbles, and the particle size is between 5 and 25 mm; the mineral admixture is fly ash or slag powder; the high-efficiency water reducing agent is polyethylene glycol methacrylate; and the water is tap water.
[0017] As a preferred embodiment of the method for making high-strength concrete for cement pole manufacturing according to the present invention, the composition ratio of each base material based on the strength index value specifically includes: by mass fraction, cement accounts for 60.45δ parts; by mass fraction, fine aggregate accounts for 37.16δ parts. -1 / 2.19 By mass, the proportion of coarse aggregate is: 25.90δ -1.05 Parts; by mass, mineral admixture accounts for: 33.61δ -2 %; by mass, high efficiency water reducer accounts for: 7.82δ -1.3 parts; by mass, water accounts for 9.70δ parts.
[0018] As a preferred embodiment of the method for producing high-strength concrete for cement pole manufacturing described in the present invention, the mixing of the base materials with good proportions specifically includes the following steps: Q1: putting cement, mineral admixtures and coarse aggregate into a concrete mixer for dry mixing for 30 seconds; Q2: adding fine aggregate and continuing to stir for 40 seconds; Q3: adding high-efficiency water reducing agent and half of the water, stirring until uniform, for 40 seconds; Q4: finally adding the remaining water, continuing to stir for 30 seconds, and stirring to form.
[0019] As a preferred solution of the method for producing high-strength concrete for cement pole manufacturing described in the present invention, wherein: adding a high-efficiency water reducing agent and half of the water, stirring until uniform, and further comprising maintaining the temperature at 33°C for 5 minutes, and maintaining stirring during the temperature maintenance process.
[0020] As a preferred solution of the method for making high-strength concrete for cement pole manufacturing of the present invention, wherein: adding high-efficiency water reducing agent and half of the water, stirring until uniform, and then maintaining the temperature at N℃ for 5min, and stirring is maintained during the temperature maintenance process; wherein N=33×δ 1 / 2 .
[0021] The present invention provides a method for producing high-strength concrete for cement pole manufacturing, which has the following characteristics:
[0022] Beneficial effects:
[0023] 1. The optimized mix ratio and new admixtures are used to improve the strength and durability of concrete;
[0024] 2. The production process of the present invention collects parameters of the external environment in advance, establishes a concrete strength index model based on the corresponding parameters, outputs the strength index value corresponding to the current site, and performs the component proportioning of each basic material based on the index value. Compared with the prior art, the hardness expression obtained by the present invention is more accurate, has better adaptability, and can also better control the cost;
[0025] 3. The cement poles produced by the present invention can be widely used in infrastructure construction fields such as power transmission and communication, and have high economic and social benefits. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the following briefly introduces the drawings required for describing the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative labor. Among them:
[0027] Figure 1 The present invention is a flowchart of the overall method for producing high-strength concrete for cement pole manufacturing.
[0028] Figure 2 The present invention is a flow chart of a method for stirring and mixing various basic materials with good proportions. DETAILED DESCRIPTION
[0029] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are described in detail below in conjunction with the accompanying drawings.
[0030] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein, and those skilled in the art may make similar generalizations without violating the connotation of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.
[0031] Therefore, please refer to Figure 1 The present invention provides a method for producing high-strength concrete for cement pole manufacturing, comprising the following steps:
[0032] S1: Install a set of sensors at the cement pole layout site to detect the external environmental parameters of the current cement site;
[0033] It should be noted that, considering that the electric poles are inserted into pre-selected pits, in actual situations, the environmental factors that each pit is exposed to are actually inconsistent. Therefore, the situation of each electric pole needs to be discussed separately.
[0034] The present invention creatively proposes this concept. Compared with the direct high-strength hardening of electric poles in the prior art, the present invention specifically considers the environmental conditions of each electric pole and makes corresponding raw material ratios according to the corresponding environmental conditions. On the one hand, the hardness of the selected raw materials is more accurately adapted to the current environment. On the other hand, it is more optimized than the unquantified blind increase in hardness cost.
[0035] Specifically, the detected external environmental parameters include: ambient humidity, ambient temperature, water content of the soil under the current collection environment, porosity of the soil under the current collection environment, and soil pH value;
[0036] Among them, the collected environmental humidity specifically includes: annual average humidity, %RH, annual maximum humidity, %RH and annual minimum humidity, %RH; the reason why the environmental humidity parameters collect three basic factors is that the annual average humidity can most accurately reflect the average humidity conditions of the pole at the current location. This factor is the most balanced, while the annual maximum humidity and annual minimum humidity take more into account the extreme humidity environment of the pole, which is also the core factor affecting the life of the pole.
[0037] Among them, the collected ambient temperatures specifically include: annual average temperature, ℃, annual maximum temperature, ℃ and annual minimum temperature, ℃; the reason why the ambient temperature parameters collect three basic factors is that the annual average temperature can most accurately reflect the average temperature conditions of the pole at the current location, and this factor is the most balanced, while the annual maximum temperature and annual minimum temperature take more into account the extreme temperature environment of the pole, which is also the core factor affecting the life of the pole.
[0038] The soil pH values collected specifically include: annual average pH value, annual maximum pH value and annual minimum pH value. The reason why the soil pH value parameters collect three basic factors is that the annual average pH value can most accurately reflect the average pH value conditions of the pole at the current location. This factor is the most balanced, while the annual maximum pH value and annual minimum pH value take into account the extreme pH value environment of the pole more, which is also the core factor affecting the life of the pole.
[0039] Among them, the humidity detector for detecting ambient humidity, the temperature detector for detecting ambient temperature, the soil moisture sensor for detecting the water content of the soil under the current collection environment, the soil porosity sensor for detecting the porosity of the soil under the current collection environment, and the soil pH sensor for detecting the soil pH value are all applications of existing sensor electronic components, and no unnecessary details will be given here.
[0040] In addition, soil moisture sensors are used to detect the moisture content of the soil under the current collection environment. The following methods are usually used:
[0041] 1. Frequency Domain Reflection (FDR): This sensor infers the moisture content of the soil by measuring the reflectivity of the soil to electromagnetic waves. The sensor sends electromagnetic waves to the soil and calculates the dielectric constant of the soil based on the reflected frequency of the waves, which is directly related to the moisture content of the soil.
[0042] 2. Tension Needle Method: This method indirectly calculates the moisture content of the soil by measuring the tension exerted on a thin needle inserted into the soil. The drier the needle, the greater the tension exerted; the wetter the needle, the smaller the tension exerted.
[0043] 3. Time Domain Reflectometry (TDR): Similar to FDR, TDR technology determines the moisture content of soil by sending a short electromagnetic pulse that interacts with water molecules and then reflects back, and measuring the travel time of the pulse.
[0044] 4. HotWire Method: This method uses a heating wire inserted into the soil and calculates the moisture content of the soil by measuring the temperature change caused by the heating wire absorbing heat due to moisture.
[0045] 5. Nuclear Magnetic Resonance (NMR) Technology: Nuclear magnetic resonance technology can non-invasively measure the water content in soil pores. This technology can infer the water content of the soil by analyzing the nuclear magnetic resonance signals of soil water molecules.
[0046] 6. Electrical conductivity method: This method infers the water content of the soil by measuring the electrical conductivity of the soil. The presence of water increases the electrical conductivity of the soil.
[0047] 7. Gravimetric method: The moisture content of the soil is calculated by measuring the change in weight of the soil sample, combining the initial and final weights, and the known moisture content with the adsorption capacity of the soil desiccant.
[0048] In addition, soil porosity sensors are used to detect the porosity of the soil under the current collection environment. The following methods are usually used:
[0049] 1. Calculation method: By measuring the bulk density and specific gravity of the soil, the soil porosity is calculated according to the formula. Soil porosity (%) = (1-soil bulk density / soil specific gravity) × 100%. This method does not require special sensors, but obtains data through laboratory tests.
[0050] 2. Optical method: Use optical instruments, such as a microporosimeter, to infer porosity by measuring the optical properties of soil samples under different moisture conditions.
[0051] 3. Nuclear Magnetic Resonance (NMR) Technology: Nuclear magnetic resonance technology can measure soil porosity non-invasively. This technology can infer the porosity of the soil by analyzing the nuclear magnetic resonance signals of soil water molecules.
[0052] 4. Gas permeability method: The porosity is estimated by measuring the gas permeability of a soil sample at a specific pressure. This method is usually performed using a gas permeability tester (such as a gas permeameter).
[0053] 5. Electrical resistance method: This method infers porosity by measuring the resistivity of the soil. The resistivity of the soil is related to the porosity and moisture content of the soil.
[0054] 6. Vibrating Wire Sensor: Vibrating Wire Pore Water Pressure Meter can indirectly measure soil porosity. By measuring the changes in the vibration frequency and amplitude of the vibrating wire, the pore water pressure in the soil can be calculated, and thus the porosity can be inferred.
[0055] In addition, soil pH sensors are usually used to detect soil pH using the following methods:
[0056] 1. Electrochemical sensor: This sensor is based on the principle of electrochemistry and usually includes a sensitive electrode and a reference electrode. The sensitive electrode is in contact with the soil solution and produces a potential change according to the change in the hydrogen ion concentration in the solution, thereby obtaining the pH value of the soil.
[0057] 2. Glass electrode sensor: This is a common electrochemical sensor that uses a wetted glass electrode to measure the pH value of the soil solution. The principle of the glass electrode is based on the chemical reaction of hydrogen ions with the glass membrane on the electrode, resulting in a potential change.
[0058] 3. Ion selective electrode: This sensor is specially designed to measure the concentration of certain ions (such as hydrogen ions) in the soil, thereby inferring the pH value of the soil. Ion selective electrodes are highly selective and can accurately measure the concentration of target ions.
[0059] 4. Optical Sensors: Optical sensors use light sensors to measure the pH of soil solutions. For example, colorimetry can be used to infer the pH by measuring changes in the color of the solution.
[0060] S2: construct a concrete strength index model based on the detected external environmental parameters, and output the strength index value corresponding to the current site;
[0061] Furthermore, the concrete strength index model constructed is as follows:
[0062]
[0063] Among them, δ is the strength index value; S 均 is the annual average humidity, %RH; S 小 is the annual minimum humidity, %RH; S 大 is the annual maximum humidity, %RH; T 均 is the annual average temperature, °C; T 小 is the annual minimum temperature, °C; T 大 is the annual maximum temperature, ℃; α is the soil moisture content under the current collection environment, %; β is the soil porosity under the current collection environment, %; H 均 is the annual average pH value; H 小 is the annual minimum pH value; H 大 is the annual maximum pH value; 1.654, 2.003, 0.87, 0.9103 and 0.39 are adjustment constants; dx is the integral operation and the integral constant is 0.
[0064] It should be noted that when generating the above model, several basic factors need to be identified first, and each basic factor has been obtained in S1 above. Then, the corresponding basic influence formula is obtained based on the five basic conditions.
[0065] In the first basic impact formula: the numerator expresses the maximum extreme impact under the comprehensive influence of the annual average humidity, among which the maximum extreme impact uses the annual maximum humidity as the upper limit of the integral and the annual minimum humidity as the lower limit of the integral, maximizing the "aging degree" of the pole under humidity conditions; the denominator expresses the difference between the annual maximum humidity, the annual minimum humidity and the annual average humidity; the overall formula expresses the public impact of the maximum extreme impact of humidity, which is similar to the "common denominator" in mathematical expressions, and can most accurately reflect the degree of influence on aging under comprehensive consideration of various conditions.
[0066] In the second basic impact formula: the numerator expresses the maximum extreme impact under the comprehensive influence of the annual average temperature, among which the maximum extreme impact uses the annual maximum temperature as the upper limit of the integral and the annual minimum temperature as the lower limit of the integral, maximizing the "aging degree" of the pole under temperature conditions; the denominator expresses the difference between the annual maximum temperature, the annual minimum temperature and the annual average temperature; the overall formula expresses the public impact of the maximum extreme impact of temperature, which is similar to the "common denominator" in mathematical expressions, and can most accurately reflect the degree of influence on aging under comprehensive consideration of various conditions.
[0067] The third basic influence formula and the fourth basic influence formula correspond to the influence of the soil water content and the porosity under the current collection environment on the overall situation respectively. On the one hand, the soil water content and porosity will not affect the aging degree of the poles too much in the actual process. On the other hand, the fifth basic formula of soil pH value in the model has considered the influence of these two factors from the side. Therefore, the third basic formula and the fourth basic formula only need to use simple basic formulas.
[0068] The fifth basic impact formula: In: The numerator expresses the maximum extreme impact under the comprehensive influence of the annual average pH value, among which the maximum extreme impact uses the annual maximum pH value as the upper limit of the integral and the annual minimum pH value as the lower limit of the integral, maximizing the display of the "aging degree" of the pole under the pH value conditions; the denominator expresses the concentrated influence of the annual maximum pH value and the annual minimum pH value. The overall formula expresses the secondary public impact of the maximum extreme impact of the pH value. The secondary public impact is similar to the "greatest common divisor" in mathematical expression, which can most accurately reflect the degree of influence on aging under comprehensive consideration of various conditions.
[0069] S3: preparing various base materials for concrete, and performing component proportioning of various base materials based on strength index values;
[0070] Specifically, the basic materials of concrete include cement, fine aggregate, coarse aggregate, mineral admixtures, high-efficiency water reducing agent and water;
[0071] Among them, cement is ordinary Portland cement, which is the conventional cement on the market; fine aggregate is river sand or mountain sand with a fineness modulus between 2.6 and 3.0; coarse aggregate is crushed stone or pebbles with a particle size between 5 and 25 mm; mineral admixture is fly ash or slag powder; high-efficiency water reducer is polyethylene glycol methacrylate; and water is tap water.
[0072] Furthermore, the composition ratio of each base material based on the strength index value specifically includes:
[0073] By mass, cement accounts for 60.45δ parts;
[0074] By mass percentage, the fine aggregate accounts for: 37.16δ -1 / 2.19 share;
[0075] By mass percentage, coarse aggregate accounts for: 25.90δ -1.05 share;
[0076] By mass percentage, mineral admixture accounts for: 33.61δ -2 share;
[0077] By mass, high efficiency water reducer accounts for: 7.82δ -1.3 share;
[0078] By mass percentage, water accounts for 9.70δ parts.
[0079] S4: After mixing the base materials in a certain proportion, pour them into a mold and perform vibration molding for 2 minutes;
[0080] For details, please refer to Figure 2 , stirring and mixing the base materials in a certain proportion specifically comprises the following steps:
[0081] Q1: Put cement, mineral admixtures and coarse aggregate into a concrete mixer and dry mix for 30 seconds;
[0082] Q2: Add fine aggregate and continue mixing for 40 seconds;
[0083] Q3: Add high-efficiency water reducer and half of the water, stir until uniform, time 40 seconds;
[0084] Q4: Finally add the remaining water and continue stirring for 30 seconds until it is formed.
[0085] Furthermore, a high-efficiency water reducing agent and half of the water are added, and the mixture is stirred until uniform and then maintained at 33°C for 5 minutes, with stirring being maintained during the temperature maintenance process.
[0086] In addition, in addition to the above specific temperature maintenance conditions, the present invention also provides the following temperature maintenance conditions:
[0087] Add high-efficiency water reducer and half of the water, stir until uniform, and then maintain the temperature at N℃ for 5 minutes. Keep stirring during the temperature maintenance process;
[0088] Where N = 33 × δ 1 / 2 .
[0089] Compared with the temperature maintenance conditions, the temperature maintenance under the variable temperature maintenance conditions is more precise, which can optimize the dispersion, wetting, retarding and strengthening effects of the high-efficiency water reducer, and ultimately obtain concrete with higher strength and better durability.
[0090] S5: The formed concrete pole is left to stand at room temperature for 24 hours and then watered for curing. The curing time is at least 7 days.
[0091] S6: After the curing is completed, the concrete poles are demoulded and the finished products are processed later.
[0092] In order to verify the technical effect of the present invention, the following test process is now given:
[0093] 1. Raw material preparation:
[0094] Cement: Choose ordinary Portland cement that meets national standards.
[0095] Coarse and fine aggregate: coarse aggregate and fine aggregate that meet standard requirements.
[0096] Admixtures: New admixtures such as fly ash or industrial slag.
[0097] High-efficiency water reducing agent: Choose the high-efficiency water reducing agent commonly used in the market.
[0098] 2. Mix ratio design:
[0099] A concrete strength index model is established based on the pre-collected external environmental parameters (such as temperature, humidity, soil composition, etc.) and design requirements.
[0100] Output the strength index value corresponding to the current site.
[0101] The component proportions of each base material are made according to the index values.
[0102] 3. Mixing and pouring:
[0103] Mix cement, coarse and fine aggregates, admixtures and high-efficiency water reducer thoroughly according to the designed mix ratio.
[0104] Ensure that the concrete is mixed evenly and there is no obvious visible segregation.
[0105] Pour concrete into the mold and use a vibrating table to demould the mold to ensure that the concrete is dense and free of bubbles.
[0106] 4. Maintenance and testing:
[0107] After standing and curing for 24 hours, take out the mold and place the concrete pole under standard curing conditions (temperature 20℃±5℃, humidity 60%±10%, curing time 7 days) for curing.
[0108] After curing, concrete specimens were prepared and tested.
[0109] 5. Performance testing:
[0110] Test the compressive strength, flexural strength, impermeability and other indicators of concrete.
[0111] Compare the degree of conformity between the test data and the expected strength index values.
[0112] The data proof table is shown in Table 1 below:
[0113] Table 1: Partial table of performance data
[0114]
[0115] Experimental data analysis:
[0116] The compressive strength of sample A is 60 MPa, which is much higher than the standard value of 40 MPa, indicating that the concrete of the present invention has higher compressive resistance.
[0117] The flexural strength of sample B is 35 MPa, which is also higher than the standard value of 30 MPa, indicating that the concrete of the present invention also performs well in bending performance.
[0118] The impermeability of sample C is 8 mm, which is less than the standard value of 10 mm, indicating that the concrete has good sealing performance.
[0119] The present invention provides a method for producing high-strength concrete for cement pole manufacturing, which has the following characteristics:
[0120] Beneficial effects:
[0121] 1. The optimized mix ratio and new admixtures are used to improve the strength and durability of concrete;
[0122] 2. The production process of the present invention collects parameters of the external environment in advance, establishes a concrete strength index model based on the corresponding parameters, outputs the strength index value corresponding to the current site, and performs the component proportioning of each basic material based on the index value. Compared with the prior art, the hardness expression obtained by the present invention is more accurate, has better adaptability, and can also better control the cost;
[0123] 3. The cement poles produced by the present invention can be widely used in infrastructure construction fields such as power transmission and communication, and have high economic and social benefits.
[0124] Importantly. Although only a few embodiments are described in detail in this disclosure, it should be readily understood by those who refer to this disclosure that many modifications are possible (e.g., the size, scale, structure, shape and proportion of various elements, and parameter values (e.g., temperature, pressure, etc.), mounting arrangements, use of materials, color, changes in orientation, etc.) without substantially departing from the novel teachings and advantages of the subject matter described in this application. For example, an element shown as integrally formed may be composed of multiple parts or elements, the position of the element may be inverted or otherwise changed, and the nature or number or position of the discrete element may be altered or changed. Therefore, all such modifications are intended to be included within the scope of the present invention. The order or sequence of any process or method steps may be changed or reordered according to an alternative embodiment. In the claims, any "device plus function" clause is intended to cover the structure described herein that performs the function, and is not only structurally equivalent but also equivalent structure. Other substitutions, modifications, changes and omissions may be made in the design, operating conditions and arrangement of the exemplary embodiments without departing from the scope of the present invention. Therefore, the invention is not limited to a specific embodiment, but extends to numerous modifications still falling within the scope of the appended claims.
[0125] Additionally, in order to provide a concise description of exemplary embodiments, all features of an actual embodiment (ie, those features that are not relevant to the best mode presently contemplated for carrying out the invention or those that are not relevant to implementing the invention) may not be described.
[0126] It will be appreciated that in the development of any actual implementation, as in any engineering or design project, numerous implementation-specific decisions may be made. Such a development effort may be complex and time-consuming, but will be a routine task of design, fabrication, and production for those of ordinary skill having the benefit of this disclosure without undue experimentation.
[0127] It should be noted that the above technical description is only used to illustrate the technical solution of the present invention rather than to limit it. Those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the spirit and scope of the technical solution of the present invention, which should be included in the scope of the claims of the invention.
Claims
1. A method for producing high-strength concrete for cement pole manufacturing, characterized in that: The steps include: S1: Install a set of sensors at the cement pole layout site to detect the external environmental parameters of the current cement site; S2: construct a concrete strength index model based on the detected external environmental parameters, and output the strength index value corresponding to the current site; S3: preparing various base materials of concrete, and performing component proportioning of various base materials based on the strength index value; S4: After mixing the base materials in a certain proportion, pour them into a mold and perform vibration molding for 2 minutes; S5: The formed concrete pole is left to stand at room temperature for 24 hours and then watered for curing. The curing time is at least 7 days. S6: After the curing is completed, the concrete poles are demoulded and the finished products are processed later.
2. The method for producing high-strength concrete for cement pole manufacturing according to claim 1, characterized in that: The external environmental parameters detected specifically include: ambient humidity, ambient temperature, soil moisture content under the current collection environment, soil porosity under the current collection environment, and soil pH value; The collected environmental humidity specifically includes: annual average humidity, %RH, annual maximum humidity, %RH and annual minimum humidity, %RH; The collected ambient temperatures specifically include: annual average temperature, °C, annual maximum temperature, °C and annual minimum temperature, °C; Among them, the collected soil pH values specifically include: annual average pH value, annual maximum pH value and annual minimum pH value.
3. The method for producing high-strength concrete for cement pole manufacturing according to claim 2, characterized in that: The concrete strength index model constructed is specifically: Among them, δ is the strength index value; S 均 is the annual average humidity, %RH; S 小 is the annual minimum humidity, %RH; S 大 is the annual maximum humidity, %RH; T 均 is the annual average temperature, °C; T 小 is the annual minimum temperature, °C; T 大 is the annual maximum temperature, ℃; α is the soil moisture content under the current collection environment, %; β is the soil porosity under the current collection environment, %; H 均 is the annual average pH value; H 小 is the annual minimum pH value; H 大 is the annual maximum pH value; 1.654, 2.003, 0.87, 0.9103 and 0.39 are adjustment constants; dx is the integral operation and the integral constant is 0.
4. The method for producing high-strength concrete for cement pole manufacturing according to claim 1, characterized in that: The basic materials of concrete specifically include cement, fine aggregate, coarse aggregate, mineral admixtures, high-efficiency water reducing agent and water; Among them, cement is ordinary Portland cement; fine aggregate is river sand or mountain sand, and the fineness modulus is between 2.6 and 3.0; coarse aggregate is crushed stone or pebbles, and the particle size is between 5 and 25 mm; mineral admixture is fly ash or slag powder; high-efficiency water reducing agent is polyethylene glycol methacrylate; water is tap water.
5. The method for producing high-strength concrete for cement pole manufacturing according to claim 4, characterized in that: The component proportioning of each base material based on the strength index value specifically includes: By mass, cement accounts for 60.45δ parts; By mass percentage, the fine aggregate accounts for: 37.16δ -1 / 2.19 share; By mass percentage, coarse aggregate accounts for: 25.90δ -1.05 share; By mass percentage, mineral admixture accounts for: 33.61δ -2 share; By mass, high efficiency water reducer accounts for: 7.82δ -1.3 share; By mass percentage, water accounts for 9.70δ parts.
6. The method for producing high-strength concrete for cement pole manufacturing according to claim 5, characterized in that: The mixing of the base materials in a certain proportion specifically comprises the following steps: Q1: Put cement, mineral admixtures and coarse aggregate into a concrete mixer and dry mix for 30 seconds; Q2: Add fine aggregate and continue mixing for 40 seconds; Q3: Add high-efficiency water reducer and half of the water, stir until uniform, time 40 seconds; Q4: Finally add the remaining water and continue stirring for 30 seconds until it is formed.
7. The method for producing high-strength concrete for cement pole manufacturing according to claim 6, characterized in that: Add high-efficiency water reducer and half of the water, stir until uniform, and maintain the temperature at 33℃ for 5 minutes. Keep stirring during the temperature maintenance process.
8. The method for producing high-strength concrete for cement pole manufacturing according to claim 7, characterized in that: Add high-efficiency water reducer and half of the water, stir until uniform, and then maintain the temperature at N℃ for 5 minutes. Keep stirring during the temperature maintenance process; Where N = 33 × δ 1 / 2 .